In-situ synthesis method of metal organic complex-based nano heterogeneous composite material

By using ultrasonic dispersion and solvent regulation technology in nanocomposite synthesis, the close combination of metal organic complexes and nanomatrix is ​​solved, and the problems of complex synthesis steps and low efficiency in traditional methods are improved, and the catalytic activity and performance of the material are improved. Suitable for a variety of application areas.

CN119060356APending Publication Date: 2024-12-03YANCHENG INST OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411322289.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-23
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Traditional nanocomposite synthesis methods are complex and difficult to accurately control the morphology and size distribution of materials. The existing in-situ synthesis methods are inefficient and complex in the process.

Method used

Use N,N-dimethylformamide solvent to disperse with metal salts and aromatic carboxylic acid organic ligands ultrasonic, add methanol and deionized water slowly, control the reaction conditions to aging at 90-150°C, and realize metal-organic complexes High efficiency, uniform and close bond with nanomatrix.

Benefits of technology

Simplify the synthesis steps, improve the catalytic activity and overall performance of the material, is suitable for large-scale preparation, reduce production costs, and is suitable for different types of metal organic complexes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119060356A_ABST
    Figure CN119060356A_ABST
Patent Text Reader

Abstract

The invention discloses an in-situ synthesis method of a metal organic complex-based nano heterogeneous composite material, which comprises the following steps: adding an N, N-dimethylformamide solvent into a metal salt and an aromatic carboxylic acid organic ligand, and carrying out ultrasonic dispersion to obtain a solvent A; slowly adding a methanol solution into the solvent A, and stirring to obtain a solvent B; then adding deionized water into the solvent B, and continuously stirring to obtain a solvent C; and finally, aging the solvent C at the temperature of 90-150 DEG C, and then centrifuging, cleaning and activating to obtain the metal organic complex-based nano heterogeneous composite material. The efficient and controllable in-situ synthesis of the heterogeneous composite material is realized only through the synthesis steps of ultrasonic dispersion, solvent regulation and control, aging reaction and the like, the preparation efficiency of the composite material is improved, the polarity of the solvent and the reaction environment can be adjusted and the reaction conditions can be optimized by introducing deionized water and methanol, and further the growth process of the material can be helped to be controlled. The tight combination of the metal organic complex and the nano matrix is promoted.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of nano composite materials, and in particular to an in-situ synthesis method of a metal-organic complex-based nano heterogeneous composite material. Background Art

[0002] Nanocomposites have been widely used in many fields due to their unique physical and chemical properties, especially nanocomposites based on metal organic complexes, which show excellent performance in catalysis, sensing, energy storage and drug delivery. However, traditional nanocomposite synthesis methods often involve complex multi-step processes, and it is difficult to accurately control the morphology and size distribution of the materials. For example, the method disclosed in the document entitled "A Metal / Graphene Nanocomposite Material and Its Preparation Method" with patent publication number CN103286308A includes a one-step photoreduction method and a one-step photocatalytic reduction method. The one-step photoreduction method comprises mixing graphene oxide with a metal complex acid or an inorganic salt and a photoreductant at room temperature or in an ice-water bath, and reducing metal ions and graphene oxide with an organic negative hydrogen donor under light conditions to obtain a product; the one-step photocatalytic reduction method comprises mixing graphene oxide with a metal complex acid or salt in a DMF aqueous solution or aqueous solution containing a reducing agent, a metal ligand and a photocatalyst, and catalyzing the reducing agent under light conditions to simultaneously reduce metal ions and graphene oxide to obtain a product; the other method comprises mixing graphene oxide with a metal organic complex in a DMF aqueous solution or aqueous solution containing a reducing agent and a photocatalyst, and then catalyzing the reducing agent under light conditions to simultaneously reduce the metal organic complex and graphene oxide to obtain a product; the preparation method involves complex reduction and photocatalytic reduction processes.

[0003] As the core component of nanocomposites, metal organic complexes have multiple oxidation states and complex coordination chemical properties, which enable them to form diverse structures at the nanoscale. These structures show unique electronic, optical and catalytic properties in different application scenarios. For example, transition metal organic complexes have excellent electron transfer ability and stability in photocatalytic and electrocatalytic reactions. At present, sol-gel method, electrochemical deposition method and other methods are generally used to prepare nanocomposites containing metal organic complexes. The preparation method disclosed in the document with patent publication number CN116332706A and name as a preparation method of an energetic metal organic complex and its high-energy composite material is to use a spray cooling anti-solvent crystallization method, place an organic ligand in a first anti-solvent and heat it, place an inorganic salt (inorganic salt and nanoparticles) in a solvent, stir and mix the two to form a clear solution, continue stirring for a period of time, and the fine droplets formed by the solution after spray atomization enter the second anti-solvent that is constantly stirred, but the preparation method only improves the morphology, which is conducive to the reaction, but the binding degree of the metal organic complex with the nano matrix is ​​reduced.

[0004] The in-situ synthesis method refers to the process of forming a nanocomposite material directly in the target environment by accurately controlling the reaction conditions during the material generation process. This method can not only simplify the synthesis steps, improve the uniformity and purity of the material, but also effectively avoid impurities that may be introduced during the post-processing process. For example, the preparation method disclosed in the document entitled "In-situ Synthesis of Inorganic Metal-Organic Complex Composite Photofunctional Material Preparation Method" with the patent publication number CN1140745A is to synthesize the required metal-organic complex in the process of inorganic gel formation or in its post-processing process during the organic-inorganic nanocomposite process. The problem is that the optical functional properties of the composite material are adjusted and optimized by controlling the gel process and heat treatment conditions, and the synthesis process is complicated and the synthesis efficiency is low. Summary of the invention

[0005] The purpose of the present invention is to solve the above-mentioned defects in the prior art and provide an in-situ synthesis method of a nano-heterogeneous composite material based on a metal organic complex, by optimizing the reaction conditions, achieving efficient, uniform and close combination of the metal organic complex and the nano-matrix, thereby improving the performance of the material.

[0006] To achieve the above object, the technical solution adopted by the in-situ synthesis method of the metal organic complex-based nano heterogeneous composite material of the present invention comprises the following steps:

[0007] Step 1): adding N,N-dimethylformamide solvent to metal salt and aromatic carboxylic acid organic ligand, and obtaining solvent A after ultrasonic dispersion;

[0008] Step 2): Slowly add methanol solution to solvent A and stir to obtain solvent B;

[0009] Step 3): adding deionized water to solvent B and continuing stirring to obtain solvent C;

[0010] Step 4): The solvent C is aged at a temperature of 90-150° C., and then centrifuged, washed, and activated to obtain a metal-organic complex-based nano-heterogeneous composite material.

[0011] Furthermore, the molar ratio of the metal salt to the aromatic carboxylic acid in the solvent A is 2 to 5:1, and the concentration ratio of the metal salt to N,N-dimethylformamide is 1:5 to 200 mg / mL.

[0012] Furthermore, the metal salt is a chloride, nitrate, bromide, acetate or iodide of iron, aluminum, manganese, titanium, indium, gallium, zinc, nickel or cobalt.

[0013] Furthermore, the aromatic carboxylic acid is one or more of trimesic acid, phthalic acid, mellitic acid, biphenyl dicarboxylic acid, pyromellitic acid, and derivatives of aromatic carboxylic acid ligands.

[0014] Furthermore, the volume of the methanol solution accounts for 1 to 5% of the total solvent volume, and stirring is continued for 1 to 2 hours after the addition of methanol.

[0015] Furthermore, the volume of deionized water accounts for 0.1-5% of the volume of N,N-dimethylformamide.

[0016] The present invention adopts the above technical solution to have the following advantages:

[0017] 1. The synthesis method of the present invention simplifies the synthesis steps, and only uses ultrasonic dispersion, solvent regulation and aging reaction steps, avoiding complicated post-processing steps, and realizing efficient and controllable in-situ synthesis of heterogeneous composite materials. This improves the efficiency of composite material preparation, makes the overall synthesis process more concise, easy to operate, and suitable for large-scale preparation.

[0018] 2. The present invention can adjust the polarity of the solvent and the reaction environment and optimize the reaction conditions by introducing deionized water and methanol, thereby helping to control the growth process of the material and promote the close combination of the metal organic complex and the nano-matrix, which helps to improve the catalytic activity and overall performance of the nano-heterogeneous composite material.

[0019] 3. The metal salts and aromatic carboxylic acid ligands used in the present invention are of wide variety and are applicable to different metal elements (such as iron, aluminum, titanium, nickel, cobalt, etc.) and various aromatic carboxylic acid organic ligands. Therefore, the method can be widely used in the preparation of different types of metal organic complexes, has strong versatility and flexibility, and significantly reduces production costs to meet the needs of catalysis, sensing, energy storage, and drug delivery. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] In order to further understand the present invention and make its objectives, technical solutions and advantages clearer, the present invention is now described in detail with reference to the accompanying drawings.

[0021] Figure 1 are SEM images of the Fe-MOF@FeOx, Ti-MOF@TiOx, and In-MOF@InOx heterogeneous composite materials in Examples 1-3, and an SEM image of In-MOF@InOx-2 in Comparative Example 3;

[0022] Figure 2 is a CO production performance diagram of the In-MOF@InOx heterogeneous composite material in Example 3;

[0023] Figure 3 This is a CO production performance diagram of the In-MOF material in Comparative Example 1;

[0024] Figure 4 This is a graph showing the CO production performance of InOx in Comparative Example 2;

[0025] Figure 5 This is the CO production performance diagram of the In-MOF@InOx-2 composite material in Comparative Example 3. DETAILED DESCRIPTION

[0026] First, a certain volume of N,N-dimethylformamide solvent is added to a certain molar amount of metal salt and aromatic carboxylic acid organic ligand, and the ultrasonic dispersion time is 30 minutes to obtain solvent A. Among them, the molar ratio of metal salt to aromatic carboxylic acid in solvent A is 1:2.0-5.0; the amount of metal salt and N,N-dimethylformamide in solvent A is: the concentration ratio of the two is 1:5-200 mg / mL.

[0027] The metal salt may be a chloride, nitrate, bromide, acetate or iodide of iron, aluminum, manganese, titanium, indium, gallium, zinc, nickel or cobalt.

[0028] The aromatic carboxylic acid can be one or more of trimesic acid, phthalic acid, mellitic acid, biphenyl dicarboxylic acid, pyromellitic acid, and derivatives of the above aromatic carboxylic acid ligands.

[0029] Then, slowly add methanol solution to solvent A so that the volume of methanol solution in the system accounts for 1% to 5% of the total volume of the solvent. After adding methanol, continue stirring for 1 to 2 hours to obtain solvent B.

[0030] Then, deionized water was added to the solvent B, and stirring was continued for 30 minutes to obtain the solvent C. The volume of the deionized water accounted for 0.1% to 5% of the volume of the N,N-dimethylformamide.

[0031] Finally, the solvent C is aged at 90-150° C., and then centrifuged, washed, and activated to obtain a metal-organic complex-based nano-heterogeneous composite material. The aging time is 6-72 hours.

[0032] Three embodiments of the present invention are provided below:

[0033] Example 1: Preparation of Fe-MOF@FeOx heterogeneous composite materials

[0034] 20 mL of N,N-dimethylformamide solvent was added to ferric chloride and phthalic acid organic ligand, the molar ratio of ferric chloride to phthalic acid was 2:1, and the dosage ratio of ferric chloride to N,N-dimethylformamide was 1:100 mg / mL. Ultrasonic dispersion was performed for 30 minutes to obtain solvent A.

[0035] Slowly add methanol solution to solvent A to make the methanol content in the system reach 2% of the total solvent volume. After adding methanol, continue stirring for 1 hour to obtain solvent B.

[0036] Deionized water was added to solvent B and the mixture was stirred for 30 min to obtain solvent C. The volume of deionized water accounted for 0.1% of the volume of N,N-dimethylformamide.

[0037] The above solvent C was aged at 130°C for 24 hours, and then centrifuged, washed, and activated to obtain a nano-heterogeneous composite material of iron-based phthalic acid complex and FeOx, named Fe-MOF@FeOx. Figure 1 SEM image of the Fe-MOF@FeOx heterocomposite shown in (a).

[0038] Example 2: The metal salt is Ti salt, and a Ti-MOF@TiOx heterogeneous composite material is synthesized.

[0039] 50 mL of N,N-dimethylformamide solvent was added to titanium nitrate and 2-nitroterephthalic acid organic ligand, the molar ratio of titanium nitrate to 2-nitroterephthalic acid was 5:1, and the amount ratio of titanium sulfate to N,N-dimethylformamide was 1:5 mg / mL. Ultrasonic dispersion was performed for 30 minutes to obtain solvent A.

[0040] Slowly add methanol solution to solvent A to make the methanol content in the system reach 5% of the total solvent volume. After adding methanol, continue stirring for 2 hours to obtain solvent B.

[0041] Deionized water was added to solvent B and the mixture was stirred for 30 min to obtain solvent C. The volume of deionized water accounted for 3% of the volume of N,N-dimethylformamide.

[0042] The solvent C was aged at 150°C for 6 hours, centrifuged, washed, and activated to obtain a nano-heterogeneous composite material Ti-MOF@TiOx of titanium-based 2-nitroterephthalic acid complex and TiOx, see Figure 1 SEM image of the Ti-MOF@TiOx heterogeneous composite material shown in Figure (b).

[0043] Example 3: The metal salt is In salt, and In-MOF@InOx heterogeneous composite material is synthesized.

[0044] 50 mL of N,N-dimethylformamide solvent was added to indium sulfate and 2-bromoterephthalic acid organic ligand, the molar ratio of indium sulfate to 2-bromoterephthalic acid was 4:1, the concentration ratio of indium sulfate to N,N-dimethylformamide was 1:200 mg / mL, and ultrasonic dispersion was performed for 30 minutes to obtain solvent A.

[0045] Slowly add methanol solution to solvent A to make the methanol content in the system reach 1% of the total solvent volume. After adding methanol, continue stirring for 1.5 hours to obtain solvent B.

[0046] Deionized water was added to solvent B and the mixture was stirred for 30 min to obtain solvent C. The volume of deionized water accounted for 5% of the volume of N,N-dimethylformamide.

[0047] Solvent C was aged at 90°C for 72 hours, and then centrifuged, washed, and activated to obtain a nano-heterogeneous composite material In-MOF@InOx of indium-based 2-bromoterephthalic acid complex and InOx. Figure 1 SEM image of the In-MOF@InOx heterogeneous composite material shown in Figure (c), see Figure 2 Figure 2 shows the CO production performance of the In-MOF@InOx heterocomposite.

[0048] Three comparative examples are provided below:

[0049] Comparative Example 1: Preparation of pure In-MOF material as a comparative material.

[0050] Step 1: Add 20 mL of N,N-dimethylformamide solvent to indium sulfate and 2-bromoterephthalic acid organic ligand, the molar ratio of indium sulfate to 2-bromoterephthalic acid is 1:1, the dosage ratio of indium sulfate to N,N-dimethylformamide is 6 mg / mL, and ultrasonic dispersion is performed for 30 minutes to obtain solvent A.

[0051] Step 2: The solvent A is aged at 130°C for 12 hours, and then centrifuged, washed, and activated to obtain the indium-based 2-bromoterephthalic acid complex In-MOF. Figure 3 The CO production performance diagram of the indium-based 2-bromoterephthalic acid complex In-MOF material is shown.

[0052] Comparative Example 2: Pure InOx material was prepared as a comparative material.

[0053] Step 1: Add 50 mL of N,N-dimethylformamide solvent to indium sulfate, the dosage ratio of indium sulfate to N,N-dimethylformamide is 100 mg / mL, and perform ultrasonic dispersion for 30 minutes to obtain solvent A.

[0054] Step 2: Add deionized water to solvent A and continue stirring for 30 minutes to obtain solvent C. The volume of deionized water accounts for 0.15% of the volume of N,N-dimethylformamide.

[0055] Step 3: The solvent C is aged at 100°C for 48 hours, and then centrifuged, washed, and dried to obtain InOx nanomaterials. Figure 4The CO production performance diagram of InOx nanomaterials is shown.

[0056] Comparative Example 3: The role of methanol and water introduced into the system in adjusting the polarity of the solvent and the reaction environment, and achieving close integration of the metal organic complex and the nanomatrix was investigated.

[0057] Step 1: Add 50 mL of N,N-dimethylformamide solvent to indium sulfate and 2-bromoterephthalic acid organic ligand, the molar ratio of indium sulfate to 2-bromoterephthalic acid is 4:1, the amount ratio of indium sulfate to N,N-dimethylformamide is 200 mg / mL, and ultrasonic dispersion is performed for 30 minutes to obtain solvent A.

[0058] Step 2: The solvent A is aged at 100°C for 48 hours, and then centrifuged, washed, and activated to obtain the nano-heterogeneous composite material In-MOF@InOx-2 of the indium-based 2-bromoterephthalic acid complex and InOx. Figure 1 The SEM image of In-MOF@InOx-2 shown in (d), and Figure 5 The CO production performance diagram of In-MOF@InOx-2 composite material is shown.

[0059] Analysis of morphological and structural characteristics:

[0060] The Fe-MOF@FeOx, Ti-MOF@TiOx, and In-MOF@InOx synthesized in the above three examples were characterized by scanning electron microscopy. Figure 1 As can be seen from Figures (a), (b) and (c) in FIG, the in-situ synthesis of heterogeneous composite materials is achieved through ultrasonic dispersion, solvent regulation and aging reaction, and the metal complex MOF is tightly combined with the nanomatrix MOx. Figure 1 In the middle figure (d), when methanol and water are not introduced into the system, the obtained metal organic complex and nanomatrix are dispersed, which is not conducive to the transfer of photogenerated carriers during the photocatalytic process.

[0061] Performance Test:

[0062] The catalytic performance of the heterogeneous composite material was evaluated by photocatalytic carbon dioxide reduction test. 20 mg of each material prepared in the above three embodiments and three comparative examples was placed in a reactor, 0.4 mL of deionized water was added, and a high-purity Ar / carbon dioxide mixed gas was introduced after vacuum sealing to ensure that the air in the reaction system was completely replaced. All photocatalytic experiments were carried out under 300 W xenon lamp irradiation.

[0063] Taking the three materials synthesized in Examples 3-5 as an example, 20 mg of the prepared composite material was placed in a reactor, and high-purity CO2 (99.995%) gas was introduced to replace the air in the system. Then the xenon lamp was turned on, and the reaction gas was taken once an hour for gas chromatography to test the product CO production. The light reaction was carried out for 4 hours, see Figure 2 The CO production of the In-MOF@InOx heterogeneous composite material prepared in Example 3 is about 40 μmol, while under the same conditions, see Figure 3 The CO production of In-MOF prepared in Comparative Example 1 is about 5 μmol, see Figure 4 The CO production of InOx prepared in Comparative Example 2 is about ~2 μmol, which proves that In-MOF@InOx has the best photocatalytic CO2 reduction activity.

[0064] In-MOF@InOx-2 synthesized in Example 3, the CO production of In-MOF@InOx-2 was about 5 μmol after 4 hours of light irradiation. Figure 5 , which is comparable to the CO production of In-MOF under the same conditions, and is much smaller than the In-MOF@InOx material (~40 μmol) in which the metal organic complex is tightly integrated with the nanomatrix.

Claims

1. An in-situ synthesis method of a metal organic complex-based nano heterogeneous composite material, characterized in that The following steps are involved: Step 1): adding N,N-dimethylformamide solvent to metal salt and aromatic carboxylic acid organic ligand, and obtaining solvent A after ultrasonic dispersion; Step 2): Slowly add methanol solution to solvent A and stir to obtain solvent B; Step 3): adding deionized water to solvent B and continuing stirring to obtain solvent C; Step 4): The solvent C is aged at a temperature of 90-150° C., and then centrifuged, washed, and activated to obtain a metal-organic complex-based nano-heterogeneous composite material.

2. The in-situ synthesis method of the metal-organic complex-based nano-heterogeneous composite material according to claim 1, characterized in that: The molar ratio of the metal salt to the aromatic carboxylic acid in the solvent A is 2-5:1, and the concentration ratio of the metal salt to N,N-dimethylformamide is 1:5-200 mg / mL.

3. The in-situ synthesis method of the metal-organic complex-based nano-heterogeneous composite material according to claim 1, characterized in that: The metal salt is a chloride, nitrate, bromide, acetate or iodide of iron, aluminum, manganese, titanium, indium, gallium, zinc, nickel or cobalt.

4. The in-situ synthesis method of the metal-organic complex-based nano-heterogeneous composite material according to claim 1, characterized in that: The aromatic carboxylic acid is one or more of trimesic acid, phthalic acid, mellitic acid, biphenyl dicarboxylic acid, pyromellitic acid, and derivatives of aromatic carboxylic acid ligands.

5. The in-situ synthesis method of metal-organic complex-based nano-heterogeneous composite material according to claim 1, characterized in that: The volume of the methanol solution accounts for 1 to 5% of the total solvent volume. After adding methanol, stirring is continued for 1 to 2 hours.

6. The in-situ synthesis method of metal-organic complex-based nano-heterogeneous composite material according to claim 1, characterized in that: The volume of deionized water accounts for 0.1 to 5% of the volume of N,N-dimethylformamide.

7. The in-situ synthesis method of metal-organic complex-based nano-heterogeneous composite material according to claim 1, characterized in that: The ultrasonic dispersion time was 30 min.

8. The in-situ synthesis method of metal-organic complex-based nano-heterogeneous composite material according to claim 1, characterized in that: After adding deionized water, stirring was continued for 30 min.

9. The in-situ synthesis method of metal-organic complex-based nano-heterogeneous composite material according to claim 1, characterized in that: The aging time of solvent C is 6 to 72 hours.