Control method of high-strength and high-toughness spring flat steel decarburized layer

Through stage heating and the use of trace alloy elements, the depth of the spring flat steel decarbonization layer is controlled, which solves the problems of complex process and high cost in the existing technology, and achieves product quality improvement with high strength and high fatigue life.

CN119061255APending Publication Date: 2024-12-03HEBEI YONGYANG SPECIAL STEEL GRP CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202310649435.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-06-02
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The prior art has complex processes and high cost when controlling the depth of the spring flat steel decarbonization layer, making it difficult to meet the fatigue life requirements of products such as high-strength suspension arms and steel sheet springs.

Method used

Through the stage heating process, the preheating and homogenizing section temperature and time are controlled, combined with the use of trace alloy elements Ni and Si, a dense oxide layer is formed to limit the diffusion of carbon and thereby control the depth of the decarbonized layer.

Benefits of technology

It realizes effective control of the depth of the spring flat steel decarbonization layer, improves product quality and qualification rate, is simple in process and low in cost, and meets the requirements of high strength and high fatigue life.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a method for controlling the thickness of a decarburized layer of high-strength and high-toughness spring flat steel. The method comprises a smelting process and a heating process. In the smelting procedure, 0.02%-0.20% of nickel element is added into the spring steel, and the content of silicon element is controlled to be 0.10%-0.40%; in the heating process, the temperature in a preheating section furnace is controlled to be 500-700 DEG C, the in-furnace time is not less than 30 min, the furnace temperature of a soaking section is controlled to be 1200-1250 DEG C, and the in-furnace time is not more than 200 min. According to the method, under the condition of an existing spring steel component system and production process, in the range not exceeding the standard requirement, a trace alloy element Ni is added into steel, the content of the Si element in the steel is limited, formation of an oxidation layer is regulated and controlled by controlling the temperature of a preheating section, and then the depth of a spring flat steel decarburized layer is effectively controlled. The method has the advantages of being simple in process, easy to implement and low in cost, and the product quality and the qualification rate can be effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a production method of spring flat steel, in particular to a control method for a decarburized layer of high-strength and toughness spring flat steel. Background Art

[0002] As an important structural material, spring steel is widely used in the automotive, railway vehicle, aerospace, machinery and instrumentation industries. Spring flat steel is widely used to manufacture leaf springs and suspension arms in automobile suspension systems. These parts are generally large in size and often bear tensile, compressive and torsion loads in service environments. In recent years, with the lightweight and high-performance of automobiles, there is an urgent need to improve the strength and design stress of spring steel to meet the demand for high fatigue life of spring steel products.

[0003] The surface quality of spring steel products has a great influence on their fatigue performance. The presence of decarburized structure on the surface will seriously reduce the fatigue strength and service life of the spring. If a decarburized layer appears on the surface of the spring, it will significantly affect the fatigue performance, especially if a full decarburized layer appears on the surface, which will greatly reduce the spring's fatigue life. Therefore, the control of the depth of the decarburized layer of spring flat steel is crucial for the production of high-strength suspension arms, leaf springs and other products.

[0004] For preventing decarburization on the surface of steel, the main focus is on the following two aspects. The first aspect is to control the depth of the decarburization layer by controlling various processes such as the heating process of the heating furnace and the rolling process. For example, Chinese patent CN100560749C provides a heating method that can prevent decarburization of high-carbon steel billets, and a slightly positive pressure and weak oxidizing atmosphere are used in the preheating section, heating section and soaking section of the billet to control the depth of the decarburization layer of the billet; for example, Chinese patent CN201110151239.5 involves a method for controlling the decarburization layer of a continuous casting billet of spring steel wire rod, and the continuous casting billet is heated in sections in a reducing atmosphere, and the rolling temperature is controlled. The second aspect is to prevent decarburization of steel by spraying anti-decarburization coating. For example, application number 201010208713.9 Anti-oxidation decarburization coating and its preparation method during billet rolling, application number 02156903.7 A coating for preventing decarburization of high-carbon steel billets.

[0005] Although the above methods can reduce the depth of the decarburized layer, they also have certain limitations. Involving the control of the heating process of the heating furnace and the rolling process, the process control requirements are relatively cumbersome and the on-site operation is more difficult; the use of anti-decarburization coatings will increase the cost of spraying equipment and operation, occupy the space of the production site, and the spraying effect is difficult to guarantee. Summary of the invention

[0006] The technical problem to be solved by the present invention is to provide a method for controlling the depth of the decarburized layer of high-strength and toughness spring flat steel with simple process and effective effect.

[0007] In order to solve the above technical problems, the technical solution adopted by the present invention is: A method for controlling the decarburized layer of a high-strength and toughness spring flat steel is specifically controlled in the following steps: (1) The chemical composition of spring steel by mass percentage is: C: 0.46~0.56%, Si: 0.10~0.40%, Mn: 0.50~1.10%, Cr: 0.80~1.20%, Mo: 0.10~0.30%, V: 0.05~0.25%, Ni: 0.02~0.20%, Cu: ≤0.35%, the balance is Fe and unavoidable impurities; (2) In order to reduce the depth of the decarburized layer during the heating process of the billet and ensure uniform heating of the billet, stage heating is adopted, the preheating temperature is controlled at 500~700℃, the furnace time is not less than 30min, the furnace temperature in the soaking section is controlled at 1200~1250℃, and the furnace time does not exceed 200min; (3) The air-fuel ratio of the heating furnace preheating section is controlled at 0.9~1.2, and the air-fuel ratio of the heating furnace soaking section is controlled at 0.7~0.9; (4) The initial rolling temperature is controlled at 1120~1170℃, the continuous rolling inlet temperature is controlled at 1000~1040℃, and the final rolling temperature is controlled at 930~980℃. The steel is then transferred to the cooling bed by rollers and air-cooled at a cooling rate of 0.5~0.9℃ / s to a temperature below 650℃ for sawing on the cooling bed.

[0008] As a further solution of the present invention, the mass percentage of the Si is 0.10-0.32%, and the mass percentage of the Ni is 0.05-0.12%.

[0009] As a further solution of the present invention, the temperature of the preheating section is 550-650° C., and the time in the furnace is 30-40 minutes; the temperature of the soaking section is 1200-1220° C., and the time in the furnace is 150-180 minutes.

[0010] The beneficial effect of adopting the above technical solution is that the present invention does not change the existing spring steel component system and production process, and within the range of standard requirements, by adding trace alloy elements Ni, limiting the content of Si elements, and controlling the temperature of the preheating section to control the formation of the oxide layer, thereby effectively controlling the depth of the decarburized layer of the spring flat steel. The present invention has the characteristics of simple process, easy implementation, and low cost, and can effectively improve product quality and qualified rate. DETAILED DESCRIPTION

[0011] The present invention will be further described in detail below in conjunction with specific embodiments.

[0012] The method for controlling the depth of the decarburization layer of high-strength and toughness spring flat steel adopts the following principles and processes: (1) It is found that during decarburization, oxygen diffuses into the steel on the one hand, and carbon in the steel diffuses outward on the other hand. Decarburization can only be formed when the decarburization rate exceeds the oxidation rate. Steel usually undergoes significant oxidation above 525°C, while the temperature range for complete decarburization of steel is 700~900°C. Therefore, during the heating stage, during the preheating stage of 550~650°C, a dense oxide layer composed of Fe2O3 and Fe3O4 is formed on the surface of the steel billet. At the same time, the upper limit of the temperature in the soaking section furnace and the holding time are controlled to control the depth of the decarburization layer. (2) During the preheating stage, while the oxide layer is formed, the element Ni will concentrate at the interface between the oxide layer and the metal, reducing the dissolution of carbon in the surface layer of the steel billet and limiting its outward diffusion, thereby reducing the decarburization layer; the element Si can increase the activity of carbon and increase the diffusion of carbon to the oxide layer-metal interface. Therefore, controlling the silicon content can reduce the decarburization layer. Therefore, based on the composition of a conventional type of spring flat steel, this method considers its Cr: 0.80~1.20% according to its chemical composition characteristics; adds 0.05~0.12% nickel element, and controls the silicon content at 0.10~0.32%, thereby controlling the decarburization layer of the spring flat steel.

[0013] For spring flat steel produced according to the above chemical composition and process, the control range of decarburization layer depth of finished spring flat steel is 0.14~0.29mm, of which 80% of the samples are ≤0.27mm and the average is 0.25mm, which fully meets the requirements of the standard for the decarburization layer depth of spring flat steel.

[0014] Embodiment 1: This method for controlling the depth of decarburization layer of high-strength and toughness spring flat steel adopts the following specific process.

[0015] Nickel is added during the smelting process to make the finished spring steel ingot contain 0.06% nickel, and the silicon content is controlled to 0.25%. The main components of the finished product are shown in Table 1; the furnace temperature in the preheating section is controlled to 580℃, the furnace time is 40min, the furnace temperature in the soaking section is 1250℃, and the furnace time is 150min. After inspection, the decarburization depth of the finished spring flat steel is 0.19mm.

[0016] Table 1: Main ingredients in the finished product of this embodiment (wt%) C To Mn Cr Know V In P S 0.52 0.15 0.86 1.01 0.17 0.13 0.06 0.012 0.006 .

[0017] Embodiment 2: This method for controlling the depth of decarburization layer of high-strength and toughness spring flat steel adopts the following specific process.

[0018] Nickel is added during the smelting process to make the finished spring steel ingot contain 0.10% nickel, and the silicon content is controlled to 0.22%. The main components of the finished product are shown in Table 1. The furnace temperature in the preheating section is controlled to 600℃, the furnace time is 40min, and the furnace temperature in the soaking section is 1220℃, and the furnace time is 160min. After inspection, the decarburization depth of the finished spring flat steel is 0.12mm.

[0019] Table 2: Main ingredients in the finished product of this embodiment (wt%) C To Mn Cr Know V In P S 0.50 0.22 1.02 0.95 0.15 0.16 0.10 0.010 0.008 .

[0020] Embodiment 3: This method for controlling the depth of decarburization layer of high-strength and toughness spring flat steel adopts the following specific process.

[0021] Nickel is added during the smelting process to make the finished spring steel ingot contain 0.12% nickel, and the silicon content is controlled to 0.28%. The main components of the finished product are shown in Table 1; the furnace temperature in the preheating section is controlled to 650℃, the furnace time is 40min, the furnace temperature in the soaking section is 1250℃, and the furnace time is 150min. After inspection, the decarburization depth of the finished spring flat steel is 0.15mm.

[0022] Table 3: Main ingredients in the finished product of this embodiment (wt%) C To Mn Cr Know V In P S 0.48 0.28 0.95 0.98 0.20 0.15 0.12 0.008 0.008 .

Claims

1. A method for controlling the decarburized layer of high-strength and toughness spring flat steel, characterized in that: Specifically, the control is carried out according to the following steps: the mass percentage of the chemical composition of the spring steel is: C: 0.46~0.56%, Si: 0.10~0.32%, Mn: 0.50~1.10%, Cr: 0.80~1.20%, Mo: 0.10~0.30%, V: 0.05~0.25%, Ni: 0.05~0.12%, Cu: ≤0.35%, and the balance is Fe and unavoidable impurities; in order to reduce the depth of the decarburization layer during the heating process of the billet and ensure uniform heating of the billet, stage heating is adopted. The preheating temperature is controlled at 500~700℃, the time in the furnace is not less than 30min, the furnace temperature in the soaking section is controlled at 1200~1250℃, and the time in the furnace is not more than 200min; the air-fuel ratio in the preheating section of the heating furnace is controlled at 0.9~1.2, and the air-fuel ratio in the soaking section of the heating furnace is controlled at 0.7~0.9; the initial rolling temperature is controlled at 1120~1170℃, the continuous rolling inlet temperature is controlled at 1000~1040℃, and the final rolling temperature is controlled at 930~980℃; then it is conveyed to the cooling bed by the roller, air-cooled at a cooling rate of 0.5~0.9℃ / s to below 650℃ for sawing on the cooling bed.

2. The method for controlling the decarburized layer of a high-strength and toughness spring flat steel according to claim 1, characterized in that: The mass percentage of Si is 0.10-0.32%, and the mass percentage of Ni is 0.05-0.12%.

3. The method for controlling the decarburized layer of high-strength and toughness spring flat steel according to claim 1, characterized in that: The temperature of the preheating section is 550-650°C, and the time in the furnace is 30-40 minutes; the temperature of the soaking section is 1200-1220°C, and the time in the furnace is 150-180 minutes.

Citation Information

Cited By

  • Heating process for controlling depth of 55Cr3 decarburized layer of small-specification bar spring steel

    CN120758717A