High-conductivity aluminum-silicon alloy and preparation method thereof

By adding Sr elements to the aluminum-silicon alloy and performing solid solution treatment and graded aging treatment, the problem of insufficient conductivity and deformation ability of the aluminum-silicon alloy is solved, and high conductivity and good deformation ability are achieved, which is suitable for the molding of complex workpieces. .

CN119061273APending Publication Date: 2024-12-03SHENYANG UNIVERSITY OF TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411185130.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Traditional aluminum-silicon alloys have poor conductivity and limited deformation capabilities in power systems, so they cannot mold complex workpieces through a single casting method, resulting in limited application.

Method used

By adding Sr elements to the aluminum-silicon alloy, and performing solid solution treatment and graded aging treatment, the conductivity and plasticity of the alloy are improved, casting defects are reduced, and a high-conductive aluminum-silicon alloy is prepared.

Benefits of technology

It significantly improves the conductivity and deformation capability of aluminum-silicon alloy, achieves conductivity not less than 42%, IACS and elongation at break of no less than 2.5%, which is suitable for the molding of complex workpieces.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides a high-conductivity aluminum-silicon alloy and a preparation method thereof. The method comprises the following steps: smelting a raw material alloy to obtain a smelting solution, adding a Sr element into the smelting solution, casting the newly prepared smelting solution, and carrying out solution treatment and graded aging treatment correction on a casting. The high-conductivity aluminum-silicon alloy obtained through the method has the advantages of being high in conductivity and good in deformability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of materials, and in particular to a high-conductivity aluminum-silicon alloy and a preparation method thereof. Background Art

[0002] With the rapid development of science and technology, especially in the fields of aerospace, automobile manufacturing, new energy and electricity, the requirements for material performance are increasing day by day. In addition to meeting their traditional application scenarios, the research and development of new materials requires new performance in new application environments.

[0003] As a common lightweight metal material, aluminum silicon alloy is widely used in power systems, such as conductive parts and structural parts in power transmission and transformation switches. As a cast aluminum alloy, traditional aluminum silicon alloy has great advantages in the preparation of high-precision parts that can maintain dimensional stability at different temperatures due to its low thermal expansion coefficient and low cost. However, the electrical conductivity of aluminum silicon alloy is poor, and its deformation ability is limited by the number and morphology of different second phases in the alloy structure. When complex-shaped workpieces in the power system cannot be formed by a single casting method, the low deformation ability of aluminum silicon alloy becomes the biggest obstacle to its application.

[0004] Therefore, the current high-conductivity aluminum-silicon alloy and its preparation method still need to be improved. Summary of the invention

[0005] The embodiments of the present disclosure provide a highly conductive aluminum-silicon alloy and a preparation method thereof to solve or alleviate one or more technical problems in the related art.

[0006] As the first aspect of the present application, the present application proposes a method for preparing a high-conductivity aluminum-silicon alloy. The method comprises: smelting a raw material alloy to obtain a smelting liquid; adding Sr elements to the smelting liquid to obtain a newly prepared smelting liquid; casting the newly prepared smelting liquid to obtain a casting; performing a solid solution treatment and a graded aging treatment on the casting to obtain the high-conductivity aluminum-silicon alloy, wherein the raw material alloy comprises an aluminum-silicon alloy; the graded aging treatment comprises: a primary aging treatment and a secondary aging treatment, wherein the primary aging treatment is to keep warm at 180°C-200°C for 6-10h, and the secondary aging treatment is to keep warm at 230°C-250°C for 6-10h, and the electrical conductivity of the high-conductivity aluminum-silicon alloy is not less than 42% IACS. The method can improve the electrical conductivity and plasticity of the obtained alloy and reduce casting defects by adding Sr elements to the alloy and performing solid solution treatment and graded aging treatment, thereby obtaining an aluminum-silicon alloy with high electrical conductivity and good deformation ability.

[0007] According to an embodiment of the present application, the raw material alloy includes ZL101 alloy, and the purity of the Sr source used for the added Sr element is not less than chemical purity. Thus, the performance of the obtained aluminum-silicon alloy can be further improved.

[0008] According to an embodiment of the present application, based on the total weight of the raw material alloy, the amount of the Sr element added is 0.03%-0.05%. When the amount of Sr added is within the above range, the Sr element can better play the role of a modifier.

[0009] According to an embodiment of the present application, before adding the Sr element to the smelting liquid, the process further comprises: detecting the content of Si and Mg in the raw alloy; when (0.05C1-C2)W y When Mg is greater than 0, Mg is added to the smelting liquid, wherein: C1 is the weight percentage content of Si in the raw material alloy; C2 is the weight percentage content of Mg in the raw material alloy; Wy is the original weight of the raw material alloy. In this way, the Mg element in the smelting liquid can be adjusted to a more appropriate range.

[0010] According to the embodiment of the present application, the content of the added Mg element is such that W m Satisfies: (0.05C1-C2)W y ≤W m ≤(0.07C1-C2)W y Thus, the Mg element in the smelting liquid can be adjusted to a more appropriate range.

[0011] According to the embodiment of the present application, after the added Mg is completely melted, the Sr element is added, and / or the purity of the Mg source used to add the Mg element is not less than industrial purity. Thus, the performance of the obtained aluminum silicon alloy can be further improved.

[0012] According to an embodiment of the present application, the temperature of the solution treatment is 520°C-540°C, and the holding time is 6-10 hours; and / or the solution treatment further includes oil quenching the casting after the solution treatment. Thus, the performance of the obtained aluminum silicon alloy can be further improved.

[0013] According to the embodiment of the present application, the raw material alloy is melted at a smelting temperature of 730° C.-750° C. and the holding time is 3 min-5 min. Thus, the performance of the obtained aluminum-silicon alloy can be further improved.

[0014] According to an embodiment of the present application, casting the newly prepared molten liquid includes: placing the newly prepared molten liquid in a preheated mold, the preheating temperature of the mold is 250° C.-300° C., and the temperature of the newly prepared molten liquid during casting is 720° C.-730° C. Thus, the performance of the obtained aluminum-silicon alloy can be further improved.

[0015] In another aspect of the present application, the present application provides a high-conductivity aluminum-silicon alloy, which is prepared based on the method described above. DETAILED DESCRIPTION

[0016] In the following, only some exemplary embodiments are briefly described. As those skilled in the art can appreciate, the described embodiments can be modified in various different ways without departing from the spirit or scope of the present disclosure, and different embodiments can be combined arbitrarily without conflict.

[0017] As a first aspect of the present application, the present application proposes a method for preparing a high-conductivity aluminum-silicon alloy. The method comprises the steps of melting a raw alloy to obtain a molten liquid, adding an Sr element to the molten liquid, casting the newly prepared molten liquid, and performing a solid solution treatment and a graded aging treatment on the casting. The high-conductivity aluminum-silicon alloy obtained by the method has the advantages of high conductivity and good deformation ability.

[0018] As a modifier, the Sr element can change the morphology of the eutectic Si phase in the aluminum-silicon alloy, thereby changing its coarse plate-like eutectic Si into a fibrous state, which is beneficial to improving the electrical conductivity and deformation ability of the alloy. In addition, in aluminum-silicon alloys, since the Si phase is the main factor that hinders the movement of electrons, the solid solubility of Si in Al is very small, and almost all Si atoms exist in the alloy matrix in the form of a second phase. Therefore, reducing the amount of Si phase or changing its morphology can significantly improve its electrical conductivity. Although the Mg element has a large solid solubility in Al, through the aging treatment of the present application, Mg can be precipitated from the Al matrix, thereby forming a Mg2Si phase with a much stronger electrical conductivity than the Si phase with the Si atoms in the alloy, which is equivalent to reducing the amount of Si phase in the organization, which has a promoting effect on the improvement of electrical conductivity.

[0019] Below, each step of the method is described in detail according to the specific embodiments of the present application.

[0020] First, the method proposed in the present application may include a step of melting the raw material alloy. The present invention has no special restrictions on the source of the alloy raw material, and commercially available products known to those skilled in the art can be used. Selecting commercially available alloys containing Al and Si, such as cast Al-Si alloys as raw materials, is conducive to reducing production costs. For example, the raw material alloy includes ZL101 alloy. ZL101 aluminum silicon alloy has good performance and appropriate Al and Si content, and the alloy obtained based on ZL101 alloy processing can have better performance.

[0021] The specific operation of melting the raw alloy is not particularly limited, as long as a molten liquid can be formed. For example, the raw alloy can be melted, and then the whole alloy can be melted and then kept warm. Specifically, the raw alloy can be melted at 730°C-750°C and kept warm for 3min-5min. In this way, the performance of the aluminum-silicon alloy obtained can be further improved, and a fully melted molten liquid can be obtained.

[0022] Subsequently, Sr element can be added to the molten liquid. As a modifier, Sr element can change the morphology of eutectic Si phase in aluminum silicon alloy, so that its coarse plate-like eutectic Si changes into fibrous. This change in the morphology of eutectic Si phase can reduce the scattering effect on electrons, increase the mean free path of electrons in the transmission process, and thus help to improve the conductivity of the obtained alloy. At the same time, the splitting effect of fibrous eutectic Si on the Al matrix is ​​much smaller than that of plate-like eutectic Si, so the alloy is less likely to crack during plastic deformation. Therefore, the addition of Sr element has the effect of improving both the electrical conductivity and plasticity of the alloy.

[0023] In the present application, based on the total mass of the raw material alloy, the amount of the added Sr element can be 0.03%-0.05%. When the amount of Sr added is within the above range, the Sr element can better play the role of a modifier. The purity of the Sr source used for the added Sr element can be no less than chemical purity. Thus, the performance of the aluminum silicon alloy obtained can be further improved.

[0024] In the present application, in order to further improve the performance of the alloy obtained, the method may further include the step of detecting the content of Si and Mg in the raw alloy before adding the Sr element, and judging whether the Mg element needs to be added according to the detection result. The inventors found that in the aluminum-silicon alloy, although the Mg element can form the Mg2Si phase to promote the improvement of electrical conductivity, when the Mg element content in the alloy system is too much, there will be too much Mg2Si phase in the matrix structure, which compresses the movement space of electrons in the Al matrix, and affects the movement of dislocations, resulting in a reduction in the electrical conductivity and deformation ability of the alloy. Therefore, it is necessary to control the Mg element in the system to have an appropriate ratio with the Si element. Taking ZL101 alloy as the raw alloy as an example, its composition already contains a part of Mg element, that is, 0.25%-0.45%, but its content is often not enough, so it is necessary to judge whether it needs to be added additionally according to the specific content of the remaining elements.

[0025] The inventors found that when (0.05C1-C2)W y When Mg>0, Mg element can be added to the smelting liquid. The purity of the Mg source used for adding Mg element is not less than industrial purity. In this way, the performance of the prepared aluminum silicon alloy can be further improved.

[0026] Wherein, C1 is the weight percentage content of Si element in the raw material alloy; C2 is the weight percentage content of Mg element in the raw material alloy; and Wy is the original weight of the raw material alloy.

[0027] When (0.05C1-C2)W y When >0, it means that the Mg content in the system is insufficient and can be appropriately added. y When ≤0, it means that the Mg content in the system is sufficient to form an appropriate amount of Mg2Si phase, and no additional addition is needed. Therefore, the Mg element in the smelting liquid can be adjusted to a more appropriate range.

[0028] According to the embodiment of the present application, the content of the added Mg element is W m satisfy:

[0029] (0.05C1-C2)W y ≤W m ≤(0.07C1-C2)W y .

[0030] For example, the content of added Mg element W m Can be:

[0031] W m =(0.056C1-C2)W y

[0032] According to an embodiment of the present application, after the added Mg is completely melted, the aforementioned operation of adding the Sr element may be performed.

[0033] After the operation of adding the above elements is completed, a new molten liquid can be obtained. The new molten liquid can then be cast. Specifically, the new molten liquid is placed in a preheated mold, the preheating temperature of the mold is 250°C-300°C, and the temperature of the new molten liquid during casting is 720°C-730°C. In this way, the performance of the obtained aluminum-silicon alloy can be further improved.

[0034] Subsequently, the castings obtained by casting can be subjected to solution treatment and graded aging treatment. During the solution treatment process, the Si phase will melt and spheroidize under the action of high temperature, and the average size will be greatly reduced, thereby increasing the contact area with the Al matrix, and the Al matrix plays the main conductive role. That is, the gap between the Si phases increases, the channel for electron transmission increases, and the conductivity of the alloy can be further improved. At the same time, the solution treatment can better uniform the organization, reduce casting defects, and make the Mg element evenly dissolved in the Al matrix, preparing for the subsequent graded aging.

[0035] According to an embodiment of the present application, the temperature of the solution treatment can be 520°C-540°C, and the holding time is 6-10h. In order to further improve the performance of the aluminum-silicon alloy obtained, the solution treatment can also include an operation of oil quenching the casting after the solution treatment. The temperature of the oil used for the oil quenching treatment can be 60°C-80°C, and the quenching oil well known to those skilled in the art can be used for the operation.

[0036] According to an embodiment of the present application, the graded aging treatment may include a primary aging treatment and a secondary aging treatment. The primary aging treatment is to keep the temperature at 180°C-200°C for 6-10 hours, and the secondary aging treatment is to keep the temperature at 230°C-250°C for 6-10 hours. After the aging treatment, the present invention preferably cools the casting at room temperature.

[0037] The high-conductivity aluminum-silicon alloy prepared in the present application has a conductivity of not less than 40% IACS, for example, not less than 42% IACS, and has good deformation capacity, for example, the elongation at break can be not less than 2.5%, for example, not less than 3.5%.

[0038] In another aspect of the present application, the present application proposes a highly conductive aluminum-silicon alloy. The highly conductive aluminum-silicon alloy is prepared based on the method described above. Therefore, the alloy has all the characteristics and advantages of the alloy known by the aforementioned method, which will not be repeated here. In general, the alloy has the advantages of high conductivity and good deformation ability.

[0039] The method proposed in the present application is described below according to specific embodiments. The alloy raw material ZL101 cast aluminum alloy is used as the test object, the mechanical properties of the alloy are tested according to the national standard GB / T 228.1-2010, and the electrical conductivity of the alloy is tested according to the national standard GB / T12966-2022.

[0040] Example 1 (the amount of each substance is in mass percentage)

[0041] Raw materials: Alloy raw materials are ZL101 cast aluminum silicon alloy; industrial pure magnesium with a purity of 99.9%; chemical pure strontium with a purity of 99.6%.

[0042] Step 1: Use GB / T 20975.25-2020 standard to detect the chemical composition of ZL101 alloy and determine whether Mg element needs to be added.

[0043] Step 2: Remove the oxide scale from the ZL101 aluminum silicon alloy, cut it into suitable sizes and place it in a melting furnace. Set the temperature to 740°C and keep it warm for 4 minutes after it is completely melted.

[0044] Step 3: Stir gently.

[0045] Step 4: Content of added Mg element W m W m =(0.056C1-C2)W y ,

[0046] After all Mg is melted, add Sr element at an amount of 0.04%, stir and keep warm for 4 minutes.

[0047] Step 5: Pour the newly obtained aluminum alloy melt into a mold preheated at 260° C. to obtain an aluminum-silicon alloy casting.

[0048] Step 6: The aluminum-silicon alloy casting is subjected to solution treatment and graded aging treatment. The solution treatment process is as follows: the aluminum-silicon alloy casting is heated to 530°C and kept warm for 8 hours, and then oil quenched in 70°C quenching oil; the graded aging treatment process is as follows: the aluminum-silicon alloy casting after solution treatment is reheated to 190°C and kept warm for 8 hours, and then the temperature is increased to 240°C, and after continuing to keep warm for 8 hours, it is taken out and cooled at room temperature (25°C).

[0049] Example 2

[0050] The remaining operations are the same as those in Example 1, except that the amount of Sr element added is 0.03%.

[0051] Example 3

[0052] The remaining operations are the same as in Example 1, except that the addition amount of Mg element is W m Wm =(0.06C1-C2)W y .

[0053] Example 4

[0054] The remaining operations are the same as those in Example 1, except that the solution treatment temperature after casting is 500 degrees Celsius, the holding time is 4 hours, and the aging treatment is the same as in Example 1.

[0055] Comparative Example 1

[0056] The remaining operations are the same as those in Example 1, except that no solution treatment and graded aging treatment are performed after casting.

[0057] Comparative Example 2

[0058] The remaining operations are the same as those in Example 1, except that solution treatment is performed after pouring, and graded aging treatment is not performed.

[0059] Comparative Example 3

[0060] The remaining operations are the same as those in Example 1, except that solution treatment is performed after pouring, and the graded aging treatment is performed by keeping the temperature at 150°C for 8 hours, and then the temperature is increased to 180°C for 8 hours.

[0061] The alloys obtained in the above examples and comparative examples were tested, and the test results are shown in Table 1 below:

[0062] Table 1 Mechanical properties and electrical conductivity results of castings obtained in the examples and comparative examples

[0063] category Elongation at break (%) Conductivity (%IACS) Example 1 5.1 45.8 Example 2 4.9 44.6 Example 3 4.8 46.0 Example 4 3.6 42.9 Comparative Example 1 2.3 39.5 Comparative Example 2 1.4 35.2 Comparative Example 3 2.4 37.7 ZL101 2.1 36.8

[0064] With reference to the test results in Table 1 above, it can be seen that the embodiments in which the Sr element is added and the solution treatment and graded aging treatment are treated all have good elongation at break and electrical conductivity, indicating that while maintaining high electrical conductivity, the embodiments of the present application obtain an alloy with better deformation ability. Specifically, relative to the raw alloy ZL101, the elongation at break and electrical conductivity of the comparative example 1 in which only the Sr element is added but no solution treatment and graded aging treatment are performed are both limited, indicating that only adding the Sr element as a modifier is not enough to significantly improve the performance of the alloy. It can be seen that the solution treatment and graded aging treatment play a decisive role in improving the electrical conductivity and elongation at break. And with reference to the test results of comparative examples 2 and 3, it can be seen that the graded aging treatment has a more significant effect on the improvement of electrical conductivity and elongation at break.

[0065] Referring to the test results of Examples 1-4, it can be seen that the electrical conductivity of Examples 1-4 is relatively high, but Example 1, which has an appropriate amount of Sr element and added with Mg element, has the best elongation at break. Comparing Example 1 and Example 4, it can be seen that the conditions of the solid solution treatment are appropriately selected, which can improve the effect of the graded aging treatment, thereby indicating that the solid solution treatment can provide better preparation for the graded aging treatment and assist in improving the effect of the graded aging treatment.

[0066] In the present disclosure, unless otherwise clearly specified and limited, a first feature being “above” or “below” a second feature may include that the first and second features are in direct contact, or may include that the first and second features are not in direct contact but are in contact through another feature between them. Moreover, a first feature being “above”, “above”, and “above” a second feature includes that the first feature is directly above and obliquely above the second feature, or simply indicates that the first feature is higher in level than the second feature. A first feature being “below”, “below”, and “below” a second feature includes that the first feature is directly above and obliquely above the second feature, or simply indicates that the first feature is lower in level than the second feature.

[0067] The disclosure above provides many different embodiments or examples to implement different structures of the present disclosure. In order to simplify the present disclosure, the components and settings of specific examples are described above. Of course, they are only examples, and the purpose is not to limit the present disclosure. In addition, the present disclosure can repeat reference numbers and / or reference letters in different examples, and this repetition is for the purpose of simplification and clarity, which itself does not indicate the relationship between the various embodiments and / or settings discussed.

[0068] The above are only specific embodiments of the present disclosure, but the protection scope of the present disclosure is not limited thereto. Any technician familiar with the technical field can easily think of various changes or substitutions within the technical scope disclosed in the present disclosure, which should be included in the protection scope of the present disclosure. Therefore, the protection scope of the present disclosure should be based on the protection scope of the claims.

Claims

1. A method for preparing a highly conductive aluminum-silicon alloy, characterized in that: include: Melting the raw alloy to obtain a molten liquid; Adding Sr element to the smelting liquid to obtain a new smelting liquid; Casting the newly prepared smelting liquid to obtain a casting; The casting is subjected to solution treatment and graded aging treatment to obtain the high-conductivity aluminum-silicon alloy, wherein: The raw material alloy includes aluminum silicon alloy; The graded aging treatment includes: primary aging treatment and secondary aging treatment. The primary aging treatment is to keep the temperature at 180°C-200°C for 6-10 hours, and the secondary aging treatment is to keep the temperature at 230°C-250°C for 6-10 hours. The electrical conductivity of the high-conductivity aluminum-silicon alloy is not less than 42% IACS.

2. The method according to claim 1, characterized in that The raw material alloy includes ZL101 alloy, The purity of the Sr source used to add the Sr element is not less than chemical purity.

3. The method according to claim 1, characterized in that The amount of the Sr element added is 0.03%-0.05% based on the total weight of the raw material alloy.

4. The method according to any one of claims 1 to 3, characterized in that: Before adding the Sr element to the smelting liquid, the method further comprises: The contents of Si and Mg in the raw alloy are detected. When (0.05C1-C2)W y >0 o'clock, Mg element is added to the smelting liquid, wherein: C1 is the weight percentage content of Si element in the raw material alloy; C2 is the weight percentage content of Mg element in the raw material alloy; Wy is the original weight of the raw materials.

5. The method according to claim 4, characterized in that The content of the added Mg element is such that W m satisfy: (0.05C1-C2)W y ≤In m ≤(0.07C1-C2)W y 。 6. The method according to claim 5, characterized in that After all the Mg to be added is melted, the Sr element is added, and / or The purity of the Mg source used to add the Mg element is not lower than industrial purity.

7. The method according to claim 1, characterized in that The solution treatment temperature is 520°C-540°C and the holding time is 6-10h; and / or After the solution treatment, the casting that has undergone the solution treatment is subjected to oil quenching treatment.

8. The method according to claim 1, characterized in that The raw alloy is melted at a temperature of 730°C to 750°C and the holding time is 3min to 5min.

9. The method according to claim 1, characterized in that: Casting the newly prepared molten liquid includes: placing the newly prepared molten liquid in a preheated mold, the preheating temperature of the mold is 250° C.-300° C., and the temperature of the newly prepared molten liquid during casting is 720° C.-730° C.

10. A highly conductive aluminum-silicon alloy, characterized in that: The high-conductivity aluminum-silicon alloy is prepared based on the method described in any one of claims 1-9.