Method for simulating relationship between ash density and corrosion rate based on finite element

Through the finite element simulation method, the relationship between gray density and porosity was constructed and metal corrosion simulation was carried out, which solved the shortcomings of the impact of insoluble pollutants on the corrosion performance of power transmission system equipment, improved the prediction accuracy of corrosion behavior and the reliable operation of the equipment sex.

CN119066922APending Publication Date: 2024-12-03GUANGDONG POWER GRID CO LTD +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411155534.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The prior art lacks systematicity and in-depthness when studying the impact of insoluble pollutants on the corrosion performance of power transmission system equipment, especially the difficulty in separating and studying the effects of gray density and salt density, resulting in insufficient corrosion rate prediction accuracy.

Method used

Using a method based on finite element simulation, the relationship between gray density and porosity is constructed, a finite element simulation model is established, and metal corrosion simulation is carried out under different porosities. The gray density is obtained through the relationship between corrosion current density, corrosion depth and corrosion rate. In relation to corrosion rate, the influence of insoluble pollutants on corrosion performance is systematically analyzed.

Benefits of technology

It improves the prediction accuracy of corrosion behavior, provides a scientific basis for the maintenance and protection strategies of the power delivery system, and improves the operating reliability and safety of the equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119066922A_ABST
    Figure CN119066922A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of material performance simulation, and particularly discloses a method for simulating the relation between ash density and corrosion rate based on a finite element. According to the method, a finite element model is established, the relation between the ash density and the porosity is established, and simulation analysis is performed on corrosion behaviors under different ash density conditions, so that the relation between the ash density and the corrosion rate is established. The method provided by the invention can effectively predict the corrosion behavior of the material under different ash density conditions, provides a scientific basis for material protection design, and has a wide application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of material performance simulation, and in particular relates to a method for simulating the relationship between ash density and corrosion rate based on finite element method. Background Art

[0002] In the power transmission system, especially in the long-term service of transmission station equipment, corrosion problems will cause serious damage to the equipment and affect the service status. During the service of these equipment, a large amount of pollutants will be deposited on the surface, which will significantly affect the corrosion behavior. It is of practical research significance to study the influence of pollutants on the corrosion performance of equipment, improve the prediction accuracy of corrosion behavior, and provide new technical solutions for material corrosion protection.

[0003] At present, the research on the effect of soluble salt pollutants on corrosion performance is relatively mature, and can be analyzed by analogy with the corrosion behavior in the solution. There are a large number of previous research papers for reference. The presence of insoluble pollutants such as dust will change the environment on the surface of the equipment and affect the corrosion reaction, but research in this area often lacks systematicity and in-depthness. Most of the research uses phenomenological theory to statistically calculate the corrosion rate under mixed pollutants. However, it is still difficult to restore and separate the effects of ash density and salt density experimentally, and the research on the effect of insoluble pollutants on corrosion performance is still relatively insufficient. Summary of the invention

[0004] In view of the above-mentioned deficiencies in the prior art regarding the study of the effect of insoluble pollutants on corrosion performance, the present invention provides a method for simulating the relationship between ash density and corrosion rate based on finite element method.

[0005] To achieve the above purpose, the following technical solutions are specifically included:

[0006] A method for simulating the relationship between ash density and corrosion rate based on finite element method comprises the following steps:

[0007] (1) Establishing the relationship between ash density and porosity: Collect dust-related information on the material surface in the field environment and determine the ash density data set used in the simulation; consider the dust as an insoluble component in the solution and the structure of the mixture of dust and solution as a porous structure to establish the relationship between ash density and porosity;

[0008] (2) Constructing a finite element simulation model: A finite element simulation model is constructed using computer software. The finite element simulation model includes a droplet region and a dust region. The shape of the droplet region is similar to or identical to the shape of the droplet on the surface of the metal substrate. There is an intersection between the droplet region and the dust region. The intersection is used as the actual research object, and the intersection is set as a pore layer region with pores.

[0009] (3) Simulation of metal corrosion under different porosities: Based on the finite element simulation model constructed above, simulation of metal corrosion under different porosities is performed to obtain the relationship between porosity and corrosion current density;

[0010] (4) Obtaining the relationship between ash density and corrosion rate: The relationship between porosity and corrosion rate is constructed through the relationship between corrosion current density, corrosion depth and corrosion rate. Finally, the relationship between ash density and corrosion rate is obtained through the relationship between ash density and porosity.

[0011] In the method of the present invention, the relationship between ash density and corrosion rate can be obtained by constructing a relationship between ash density and porosity, constructing a finite element simulation model, and simulating metal corrosion under different porosities. The method of the present invention is based on finite element model simulation, systematically analyzes the influence of insoluble pollutants on the corrosion performance of power transmission equipment, improves the prediction accuracy of corrosion behavior, provides a scientific basis for equipment maintenance and protection strategies, and thus improves the operational reliability and safety of the power transmission system.

[0012] Preferably, in step (1), the relationship between the ash density and the porosity is:

[0013] Where ε is the porosity, NSDD is the ash density, and S is the surface area of ​​the carrier on which the dust resides.

[0014] Preferably, in step (2), the shape of the droplet region is an ellipse, the shape of the dust region is a rectangle, and the finite element simulation model is meshed.

[0015] Preferably, in step (2), the computer software is COMSOL simulation software.

[0016] Preferably, in step (2), the effective diffusion coefficient of each substance in the porous layer region is determined according to the Bruggeman equation, which is:

[0017] D i,eff =D i *ε 1.5 (Formula 8), where D i represents the effective diffusion coefficient of species i in the current solution environment, and ε is the porosity.

[0018] Preferably, in step (3), tertiary current distribution is used as the physical field interface in the simulation.

[0019] Further preferably, in the tertiary current distribution, the Butler-Volmer formula is used to describe the electrode reaction kinetics, and the effective diffusion coefficient of each substance in the pore layer region is taken into account.

[0020] In step (4), the relationship between the corrosion current density, corrosion depth and corrosion rate includes the following formula:

[0021] The relationship between corrosion depth and current density at time t:

[0022] The expression of the maximum corrosion depth at time t is: max (t) = max(d(x, t)) (Equation 11),

[0023] The calculation formula for the average corrosion depth is:

[0024] The average corrosion rate calculation formula is:

[0025] In the above formula, i(x,τ) represents the corrosion current density, d(x,t) represents the corrosion depth, and d max (t) represents the maximum corrosion depth, represents the average corrosion depth, z is the charge, F is the Faraday constant, a represents the droplet width, and R represents the average corrosion rate.

[0026] Compared with the prior art, the present invention has the following beneficial effects: the method of the present invention further constructs the relationship between ash density and corrosion rate by establishing a finite element model, constructing the relationship between ash density and porosity, and simulating and analyzing the corrosion behavior under different ash density conditions. The method of the present invention can effectively predict the corrosion behavior of materials under different ash density conditions, provide a scientific basis for material protection design, and has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 It is a finite element simulation model constructed using COMSOL simulation software in Example 1.

[0028] Figure 2 This is a line graph of the total electrode thickness change and time obtained by simulation calculation in Example 1.

[0029] Figure 3 This is a diagram showing the relationship between electrode thickness change and arc length obtained by simulation calculation in Example 1. DETAILED DESCRIPTION

[0030] In order to better illustrate the purpose, technical scheme and advantages of the present invention, the present invention will be further described below through specific examples. The test methods used in the examples and / or comparative examples are conventional methods unless otherwise specified; the materials, reagents, etc. used can be obtained from commercial channels unless otherwise specified.

[0031] Example 1

[0032] (1) Collect information related to dust on insulators in the field environment: In the field environment, the thickness of pollutants on insulators is regarded as the thickness of dust, and water is used to dissolve this part of pollutants. Water will dissolve soluble substances such as salt in this part of pollutants. After drying, the remaining insoluble dust itself affects the diffusion and mass transfer of corrosive ions and thus affects the corrosion process. In this way, the state when the substrate surface is covered with droplets or water film and corrosion occurs is simulated, and the structure where corrosion occurs when the substrate surface is covered with droplets or water film and dust is regarded as a porous structure, and the dust density is associated with the porosity of the porous structure. The specific operation is as follows:

[0033] First, the contaminants on the surface of the insulator are partially removed, and the thickness of the contaminant gap on the surface of the insulator is measured using an optical microscope. The thickness is repeated several times to obtain the average value. Since the contaminants contain very little dust and its height can be ignored, the average height of the contaminants covering the surface of the substrate can be taken as the average height of the dust layer, that is, the height of the dust particles covering the surface of the substrate (in this embodiment, the insulator), expressed as h. 灰 mark.

[0034] Then use distilled water to partially dissolve the pollutants on the surface of the insulator. The soluble salts are dissolved in the water, and the dust is insoluble. The insoluble matter is filtered and dried and weighed to obtain the mass of the dust layer. After multiple measurements, the average value is taken, which is the mass of the dust layer, expressed in m 灰 express.

[0035] The coverage height of dust particles on the substrate (insulator) surface is h 灰 The product of the surface area S of the insulator is taken as the apparent volume V0 of the dust; the volume of the dust after dissolving the pollutants in distilled water and drying is taken as the actual volume V 灰 , the relationship between ash density and porosity ε is obtained according to the ash density and porosity formula:

[0036]

[0037] Gray density formula

[0038]

[0039] Among them, m 灰 represents the mass of the dust layer, S is the surface area of ​​the insulator, ρ0 is the apparent average density of the dust layer, and ρ 灰 is the actual average density of the dust layer, h 灰 It is the average coverage height of the dust layer on the substrate surface.

[0040] According to the above formula 1-3, by actually measuring the apparent volume V0, ρ of multiple groups of dust 灰and the actual volume V 灰 , multiple sets of ash density NSDD and porosity ε data can be obtained to determine the upper and lower limits of the ash density NSDD used in the simulation.

[0041] (2) Using COMSOL simulation software, a finite element simulation model was constructed with reference to the shape of the metal surface and the droplet:

[0042] Fe is selected as the metal matrix, and the modeling shape is determined by the shape of the droplet on the surface of the metal matrix. In this embodiment, a water droplet is selected as the droplet, and the modeling shape is an ellipse, wherein the major semi-axis of the ellipse is determined according to half of the maximum diameter of the water droplet in the actual experiment, and the minor semi-axis is determined according to the height of the water droplet. The contact angle between the water droplet and the metal surface is determined by experiment; the droplet is regarded as an axisymmetric shape, and a two-dimensional axisymmetric model is used to simplify the calculation when constructing the geometric model;

[0043] (3) Using the geometry toolbar in the COMSOL simulation software, an elliptical shape is constructed to represent the droplet, and a rectangular shape is constructed to represent the dust. The intersection of the two is constructed as the actual research object. In the constructed geometric model, the droplet is h from the surface. 灰 The part within is set as a porous pore layer area, and its porosity is ε. The schematic diagram of some models is shown in the attached figure. Figure 1 As shown, the lower part of the ellipse is the metal matrix, the blue part represents the pore layer with insoluble dust, and the upper part represents the part where the droplet is higher than the pore layer;

[0044] In this embodiment, the geometric parameters of the model are shown in Table 1:

[0045] Table 1

[0046]

[0047] (4) Based on the principle of corrosion electrochemistry, COMSOL simulation software is used to simulate metal corrosion under different porosities:

[0048] Since the 3D model has rotational symmetry, the model constructed by sectioning it uses a more detailed mesh division on the metal substrate surface. The results are as follows Figure 1 shown.

[0049] The Tertiary Current Distribution is used as the physics interface and the electrode reactions on the surface are modeled using H + The concentration-dependent Butler-Volmer equation describes the electrode reaction kinetics, including the following formula:

[0050]

[0051] n=α c +α a (Formula 6),

[0052] η=EE eq,ref (T)(Formula 7);

[0053] where i loc,expr is the local current density expression, i0 is the exchange current density, α a and α C is the polarizability of the cathode and anode, their sum is n, η is the overpotential, which is the distance of the current electrode potential E from the reference equilibrium electrode potential E eq,ref The size of i0ref(T) is the reference exchange current density at standard temperature, which is related to the concentration c i Reaction coefficient v with the substance i Related, T is the thermodynamic temperature, F is the Faraday constant, and R is the gas constant.

[0054] And use water-based electrical neutrality as the charge conservation model, set various physical parameters, including the diffusion coefficient of the initial ion concentration; when using the Butler-Volmer equation to describe the electrode reaction kinetics, input parameters such as the exchange current density, symmetry factor and reference potential of the oxygen reduction and iron dissolution reactions. The parameters applied to specific situations need to be fitted through actual electrochemical tests.

[0055] Among them, for the electrode reaction, it is set to occur in the solution on the metal surface. The cathode reaction considers the effect of oxygen concentration on the reaction rate, and the cathode reaction part is described by oxygen reduction reaction, and the solution part undergoes the hydrolysis reaction of metal ions; the boundary condition concentration is added and calculated in sequence; for the dissolution reaction of the anode iron, the generation and diffusion of iron ions and the effect of pH on the reaction rate are considered. For the non-Faraday reaction, it is set to occur in the solution domain, considering the hydrolysis reaction of iron ions and the self-dissociation reaction of water; for the setting of the porous layer, the effective diffusion coefficient of each substance is determined according to the Bruggeman equation:

[0056] D i,eff =D i *ε 1.5 (Formula 8),

[0057] Among them, D i represents the effective diffusion coefficient of species i in the current solution environment.

[0058] During the calculation process, multiple sets of data are substituted into the above formula (4-8) for simulation calculation. Each set of data includes O2, H + OH -, Na, Cl, Fe concentrations, reaction rates, equilibrium constants, rate constants and other parameters can determine multiple sets of data according to different conditions. One set of data used in this embodiment is shown in Table 2. Based on the above corrosion electrochemical principles and calculations, the corrosion current density of the iron-based metal material at time t can be obtained.

[0059] (5) Determine the relationship between ash density and corrosion rate change:

[0060] In step (4), the relationship between porosity and current density is constructed by continuously changing the settings of the porosity data in the model, and multiple groups of porosity and current density data are obtained. Then, through the relationship between current density, corrosion depth and corrosion rate (the following formula 9-13), the relationship between porosity and corrosion rate is constructed. The specific formula involved is as follows: Formula 9-13.

[0061] According to Faraday's law, the amount of substance reacting at time t and the current can be expressed as follows:

[0062] Where n is the amount of the substance that undergoes corrosion reaction, z is the charge, F is the Faraday constant, and I(τ) represents the current.

[0063] Then the relationship between corrosion depth change and current density is:

[0064] The expression of the maximum corrosion depth at time t is: d max (t) = max(d(x, t)) (Equation 11),

[0065] The calculation formula for the average corrosion depth is:

[0066] Average corrosion rate calculation formula R: ,

[0067] In the above formula, i(x,τ) represents the current density, d(x,t) represents the corrosion depth, and d max (t) represents the maximum corrosion depth, represents the average corrosion depth, z is the charge, F is the Faraday constant, a represents the droplet width, and R represents the average corrosion rate.

[0068] Table 2

[0069]

[0070]

[0071]

[0072]

[0073] In this example, a single set of parameters in Table 2 is used as a specific example to illustrate the principle and implementation method of the present invention. The calculated results are as follows: Figure 2 As shown in the figure, when dust exists as an insoluble substance, the electrode corrosion depth increases with time, and due to the influence of the diffusion effect, the corrosion changes with distance as shown in the figure. Figure 3 As shown, the arc length represents the length from a point on the metal substrate to the center of the ellipse, which represents the x-axis of the corrosion electrode. It can be found that under the influence of dust, the corrosion near the inside of the metal is slower, the higher oxygen concentration on the outside is mainly due to the cathode reaction, and the degree of corrosion reaches the maximum near the inner part.

[0074] The present invention models insoluble dust and droplets as porous structures, and establishes the correlation between ash density and metal corrosion rate in the presence of insoluble matter through the corrosion model of ash density, porosity and tertiary current distribution, thereby providing a new theoretical model and numerical calculation method for constructing a predictive corrosion rate model.

[0075] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A method for simulating the relationship between ash density and corrosion rate based on finite element method, characterized in that: The steps include: (1) Establishing the relationship between ash density and porosity: Collect dust-related information on the material surface in the field environment and determine the ash density data set used in the simulation; consider the dust as an insoluble component in the solution and the structure of the mixture of dust and solution as a porous structure to establish the relationship between ash density and porosity; (2) Constructing a finite element simulation model: A finite element simulation model is constructed using computer software. The finite element simulation model includes a droplet region and a dust region. The shape of the droplet region is similar to or identical to the shape of the droplet on the surface of the metal substrate. There is an intersection between the droplet region and the dust region. The intersection is used as the actual research object, and the intersection is set as a pore layer region with pores. (3) Simulation of metal corrosion under different porosities: Based on the finite element simulation model constructed above, simulation of metal corrosion under different porosities is performed to obtain the relationship between porosity and corrosion current; (4) Obtaining the relationship between ash density and corrosion rate: The relationship between porosity and corrosion rate is constructed through the relationship between corrosion current density, corrosion depth and corrosion rate. Finally, the relationship between ash density and corrosion rate is obtained through the relationship between ash density and porosity.

2. The method for simulating the relationship between ash density and corrosion rate based on finite element method according to claim 1, characterized in that: In step (1), the relationship between the ash density and the porosity is: Where ε is the porosity, NSDD is the ash density, and S is the surface area of ​​the carrier on which the dust resides.

3. The method for simulating the relationship between ash density and corrosion rate based on finite element method according to claim 1, characterized in that: In step (2), the shape of the droplet region is an ellipse, the shape of the dust region is a rectangle, and the finite element simulation model is meshed.

4. The method for simulating the relationship between ash density and corrosion rate based on finite element method according to claim 1, characterized in that: In step (2), the effective diffusion coefficient of each substance in the porous layer region is determined according to the Bruggeman equation, which is: D i,eff =D i *e 1.5 , Among them, D i represents the effective diffusion coefficient of species i in the current solution environment, and ε is the porosity.

5. The method for simulating the relationship between ash density and corrosion rate based on finite element method according to claim 1, characterized in that: In step (3), the tertiary current distribution is used as the physical field interface in the simulation.

6. The method for simulating the relationship between ash density and corrosion rate based on finite element method according to claim 5, characterized in that: In the tertiary current distribution, the Butler-Volmer formula is used to describe the electrode reaction kinetics, and the corrosion current density is calculated by considering the effective diffusion coefficient of each substance in the pore layer region.

7. The method for simulating the relationship between ash density and corrosion rate based on finite element method according to claim 1, characterized in that: In step (4), the relationship between the corrosion current density, corrosion depth and corrosion rate includes the following formula: The relationship between corrosion depth and current density at time t: The expression of the maximum corrosion depth at time t is: max (t) = max(d(x,t)), The calculation formula for the average corrosion depth is: The average corrosion rate calculation formula is: In the above formula, i(x,τ) represents the corrosion current density, d(x,t) represents the corrosion depth, and d max (t) represents the maximum corrosion depth, represents the average corrosion depth, z is the charge, F is the Faraday constant, a represents the droplet width, and R represents the average corrosion rate.

Citation Information

Cited By

  • Method for constructing relationship between non-soluble deposit density and corrosion rate on basis of finite element simulation