Positive plate and battery

By using a positive electrode current collector and a positive electrode active layer of a specific thickness in the positive electrode sheet, including LiNixCoyMnzAlwMaO2 positive electrode active material and additive, forming C=C double bond and carboxyl characteristic peaks, the lithium salt volatile and alkali in the preparation of high nickel ternary materials is solved. The basic attack problem improves the cycle and power performance of the battery.

CN119069639APending Publication Date: 2024-12-03ZHUHAI COSMX BATTERY CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411189554.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

During the preparation process, the existing positive electrode active materials with high nickel ternary materials have a low sintering temperature, resulting in a decrease in the volatility of lithium salts. The residual lithium salt reacts with CO2 and H2O in the air to form Li2CO3, and reacts with electrolyte to form HF, which damages the damage. Battery performance, and base attacks the binder leads to gelation, increasing processing difficulty and affecting electrochemical performance.

Method used

Using a positive electrode current collector with a thickness of 8-16μm and a positive electrode active layer with a thickness of 80-130μm, it contains LiNixCoyMnzAlwMaO2 positive electrode active material and additives, such as maleic acid and catechol acid, to form C=C double bond and carboxyl characteristic peaks, and enhance the Interaction forces and chemical bonds improve stability and electron transport performance.

Benefits of technology

It improves the electron and ion transmission performance of the positive electrode sheet, reduces resistance, improves the cycle performance and power performance of the battery, and is suitable for a wide range of applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069639A_ABST
    Figure CN119069639A_ABST
Patent Text Reader

Abstract

The invention provides a positive plate and a battery. The positive plate comprises a positive current collector and a positive active layer positioned on at least one surface of the positive current collector, the thickness of the positive electrode current collector is 8-16 [mu] m, the thickness of the positive electrode active layer is 80-130 [mu] m, and in an infrared spectrum curve, the positive plate has a first characteristic peak with the wavelength of 2500cm <-1 >-3500cm <-1 > and a second characteristic peak with the wavelength of 1500cm <-1 >-2000cm <-1 >; the peak area S1 of the first characteristic peak and the peak area S2 of the second characteristic peak meet the condition that S1 / S2 is more than 1 and less than 2. When the positive plate is applied to the battery, the cycle performance and the power performance of the battery can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of new energy technology, and in particular to a positive electrode sheet and a battery. Background Art

[0002] Lithium-ion batteries are widely used in various electronic devices and electric vehicles due to their high energy density, long cycle life and environmental protection. The positive electrode active material in lithium-ion batteries has a crucial influence on the performance of lithium-ion batteries. At present, in order to further improve the energy density of lithium-ion batteries, high-nickel ternary materials with high specific capacity are often used as positive electrode active materials.

[0003] However, during the preparation process of the existing high-nickel ternary materials, the volatilization amount of lithium salts is reduced due to the low sintering temperature, and the lithium salt content remaining on the surface of the high-nickel ternary materials will increase, thereby forming lithium oxides (for example, Li2O). Lithium oxides easily adsorb CO2 and H2O in the air to form Li2CO3 and LiOH on the surface of the high-nickel ternary materials. Among them, Li2CO3 will cause the battery to decompose and produce gas when it is stored at high temperature, fully charged and at high potential, and LiOH will react with the lithium salt in the electrolyte to generate HF, which deteriorates the battery performance. In addition, during the homogenization process, the high-nickel The bases on the surface of the ternary material will also attack the CH bond and CF bond of the binder (for example, PVDF), causing the CH bond and CF bond to undergo elimination reactions, thereby forming C=C bonds. The formed C=C bonds will produce chemical cross-links. Since the regularity of the binder chain is very high, continuous HF removal reactions are likely to occur, which will eventually lead to the gelation of the positive electrode slurry including the high-nickel ternary material, increasing the difficulty of processing the positive electrode slurry, resulting in poor coating performance of the positive electrode slurry, which is not conducive to the electrochemical properties of the positive electrode sheet, making the positive electrode sheet unfavorable to the battery's cycle performance and power performance when used in the battery.

[0004] At present, the following methods are mainly used to improve the "jellying" of the positive electrode slurry to improve the electrochemical performance of the positive electrode sheet: ① Optimize the sintering process, control the sintering environment, or try surface coating and water washing to reduce the residual alkali content on the surface of the material; ② High-temperature baking of various materials before dry powder mixing to remove adsorbed moisture and reduce the impact of alkalinity; ③ Strictly control the ambient humidity during the coating process, the lower the better to prevent gelation; ④ Improve the binder, introduce hydrophilic groups such as sulfonic acid, carboxyl or amine groups into the binder, inhibit the HF removal reaction, and improve the alkali resistance of the binder. However, these methods increase the difficulty of the process to varying degrees, not only increasing the production cost, but also limiting the degree of anti-gelation. Summary of the invention

[0005] The present invention provides a positive electrode sheet, which can improve the cycle performance and power performance of a battery when applied to the battery.

[0006] The present invention provides a battery having excellent cycle performance and power performance.

[0007] The present invention provides a positive electrode sheet, wherein the positive electrode sheet comprises a positive electrode current collector and a positive electrode active layer located on at least one surface of the positive electrode current collector;

[0008] The thickness of the positive electrode current collector is 8-16 μm, and the thickness of the positive electrode active layer is 80-130 μm;

[0009] In the infrared spectrum curve, the positive electrode has a wavelength of 2500cm -1 -3500cm -1 The first characteristic peak of -1 -2000cm -1 The second characteristic peak of

[0010] The peak area S1 of the first characteristic peak and the peak area S2 of the second characteristic peak satisfy: 1<S1 / S2<2.

[0011] The positive electrode sheet as described above, wherein the positive electrode active layer further comprises a positive electrode active material, and the molecular formula of the positive electrode active material is shown in Formula 1;

[0012] LiNi x Co y Mn z Al w M a O2 formula 1;

[0013] In Formula 1, 0.8≤x<1, 0<y<0.2, 0<z<0.2, 0≤w≤0.05, 0≤a≤0.1, x+y+z+w+a=1;

[0014] M is selected from at least one of Mg, Ti, Zr, Y, B, W, and Sr.

[0015] The positive electrode sheet as described above, wherein the particle size of the positive electrode active material is 2-5 μm.

[0016] The positive electrode sheet as described above, wherein the positive electrode active layer comprises an additive, and the additive is selected from at least one of maleic acid, catechol acid, phenolic acid, succinic acid and a copolymer formed by at least two of the foregoing substances.

[0017] The positive electrode sheet as described above, wherein the molecular weight of the additive is 98-2000 g / mol.

[0018] The positive electrode sheet as described above, wherein the resistivity of the positive electrode sheet is 0.2-5KΩ·cm; and / or the surface resistance of the positive electrode sheet is 20-600mΩ.

[0019] The positive electrode sheet as described above, wherein in the positive electrode sheet, the average peeling force between the positive electrode active layer and the positive electrode current collector is 0.01-0.2 kgf.

[0020] The positive electrode sheet as described above, wherein the porosity of the positive electrode active layer is 20-40%.

[0021] The positive electrode sheet as described above, wherein the tensile strength of the positive electrode current collector is ≥150 MPa.

[0022] The positive electrode sheet as described above, wherein in the X-ray diffraction spectrum, the positive electrode active layer has a crystal plane index peak of (-2, 0, 2) with 2θ of 25-30°;

[0023] And / or, the space group of the positive electrode active layer is P1 21 / c 1.

[0024] The present invention also provides a battery, wherein the battery comprises the positive electrode sheet as described above.

[0025] The positive electrode of the present invention has a wavelength of 2500cm in the infrared spectrum curve. -1 -3500cm -1 The first characteristic peak of -1 -2000cm -1 The second characteristic peak of the first characteristic peak; the peak area S1 of the first characteristic peak and the peak area S2 of the second characteristic peak satisfy: 1<S1 / S2<2. The special structure of the positive electrode sheet can improve the electron and ion transmission performance and stability of the positive electrode sheet. Furthermore, matching the positive electrode current collector with a thickness of 8-16μm and the positive electrode active layer with a thickness of 10-100μm can further improve the electronic conductivity of the positive electrode sheet and reduce the resistance of the positive electrode sheet, thereby improving the cycle performance and power performance of the battery.

[0026] The battery of the present invention, because it includes the above-mentioned positive electrode sheet, has excellent cycle performance and power performance and is suitable for wide promotion and application. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] In order to more clearly illustrate the technical solutions in the embodiments of the present invention or related technologies, the following briefly introduces the drawings required for use in the embodiments of the present invention or related technologies. Obviously, the drawings described below are only some embodiments of the present invention, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0028] Figure 1 is the SEM image of maleic acid;

[0029] Figure 2 is the infrared spectrum curve of maleic acid;

[0030] Figure 3 1 is the infrared spectrum curve of the positive electrode sheet in Example 1 of the present invention and Comparative Example 1;

[0031] Figure 4 is the XRD curve of maleic acid;

[0032] Figure 5 XRD curves of the positive electrode active layer in Example 1 and Comparative Example 1 of the present invention;

[0033] Figure 6 for Figure 5 A partial enlarged view of . DETAILED DESCRIPTION

[0034] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0035] A first aspect of the present invention provides a positive electrode sheet, comprising a positive electrode current collector and a positive electrode active layer located on at least one surface of the positive electrode current collector;

[0036] The thickness of the positive electrode current collector is 8-16 μm, and the thickness of the positive electrode active layer is 80-130 μm;

[0037] In the infrared spectrum curve, the positive electrode has a wavelength of 2500cm -1 -3500cm -1 The first characteristic peak of -1 -2000cm -1 The second characteristic peak of

[0038] The peak area S1 of the first characteristic peak and the peak area S2 of the second characteristic peak satisfy: 1<S1 / S2<2.

[0039] In the present invention, the surface of the positive electrode current collector refers to the two surfaces of the positive electrode current collector that are arranged opposite to each other and have the largest area. It can be understood that in the present invention, a positive electrode active layer can be arranged on one surface of the positive electrode current collector to form a positive electrode sheet; or positive electrode active layers can be arranged on both surfaces of the positive electrode current collector to form a positive electrode sheet.

[0040] The positive electrode active layer of the present invention comprises at least a positive electrode active material, a conductive agent and a binder, wherein the conductive agent may be conductive carbon black SP and / or carbon nanotubes CNT; and the binder may be polyvinylidene fluoride PVDF.

[0041] The positive electrode current collector of the present invention may be Al foil, and the thickness of the positive electrode active layer refers to the average thickness of the single-sided positive electrode active layer. In some embodiments, the positive electrode slurry may be applied to at least one surface of the positive electrode current collector, and the single-sided coating thickness is 50-300 μm, and after roller drying, a single-sided positive electrode active layer with a thickness of 10-100 μm is obtained.

[0042] In the positive electrode sheet of the present invention, the first characteristic peak is the stretching vibration peak of the OH bond of the carboxyl group; the second characteristic peak is the stretching vibration peak of the C=C double bond.

[0043] The positive electrode sheet of the present invention can improve the electron and ion transmission performance and stability of the positive electrode sheet, and improve the cycle performance and power performance of the battery. The inventor analyzed the reason and believed that it may be because: the C=C double bond in the positive electrode sheet has a strong polarity, which can form a strong interaction force between the components in the positive electrode active layer, for example, forming hydrogen bonds and dipole-dipole interactions. These interactions can reduce the probability of agglomeration of the components in the positive electrode active layer and improve the stability of the positive electrode sheet. In addition, the C=C double bond in the positive electrode sheet can harden with the groups on the surface of the positive electrode active material and the adhesive to form a stable chemical bond or complex, thereby changing the crystal structure or surface chemical state of the positive electrode active material and the adhesive, and improving the electron and ion transmission performance of the positive electrode sheet; and the carboxyl group, as a reaction site, can chemically react with the residual alkali or other groups in the positive electrode active material, which helps to remove impurities in the positive electrode active material, improve the purity, stability and electrochemical activity of the positive electrode active material, thereby improving the cycle performance and power performance of the battery. When the ratio of S1 to S2 meets the above range, the C=C double bond in the positive electrode sheet can better match the carboxyl group to give full play to the role of the C=C double bond and the carboxyl group, and improve the cycle performance and power performance of the battery. Further matching the positive electrode current collector with a thickness of 8-16 μm and the positive electrode active layer with a thickness of 10-100 μm, the positive electrode active material and the conductive agent in the positive electrode sheet can form a tight three-dimensional conductive network while ensuring the volume energy density of the battery, thereby improving the electronic conductivity of the positive electrode sheet, making the capacity of the positive electrode active material more fully utilized, and alleviating the phenomenon of poor conductivity between the positive electrode active materials caused by the continuous deintercalation of lithium ions during the battery cycle, thereby improving the battery cycle performance; and the positive electrode current collector within the above thickness range can be in closer contact with the positive electrode active layer, reducing the contact impedance between the positive electrode active layer and the positive electrode current collector, and reducing the probability of polarization during battery charging and discharging, thereby improving the battery power performance. Therefore, when the positive electrode sheet of the present invention is applied to a battery, it can improve the battery cycle performance and power performance.

[0044] It is worth mentioning that the positive electrode sheet of the present invention does not require modification of the positive electrode active material or the binder, which can avoid the cost increase caused by the modification.

[0045] The present invention can further improve the electrochemical performance of the positive electrode sheet by further selecting the positive electrode active material. In some embodiments of the present invention, the molecular formula of the positive electrode active material is as shown in Formula 1;

[0046] LiNi x Co y Mn z Al w M a O2 formula 1;

[0047] In Formula 1, 0.8≤x<1, 0<y<0.2, 0<z<0.2, 0≤w≤0.05, 0≤a≤0.1, x+y+z+w+a=1;

[0048] M is selected from at least one of Mg, Ti, Zr, Y, B, W, and Sr.

[0049] The positive electrode active material of the present invention is a metal oxide including at least Li, Ni, Co, and Mn. The positive electrode active material may further include at least one of Al and M.

[0050] In the present invention, the positive electrode active material represented by Formula 1 has a higher gram capacity, which can further improve the energy density of the battery, so that the battery has better cycle performance, power performance and energy density.

[0051] In some embodiments of the present invention, the particle size of the positive electrode active material is 2-5 μm.

[0052] In the present invention, the particle size of the positive electrode active material refers to the average particle size of the positive electrode active material. When the particle size of the positive electrode active material meets the above range, the positive electrode active material can be prevented from being broken during long-term cycling while improving the lithium ion extraction efficiency of the positive electrode sheet, thereby improving the cycle performance of the battery.

[0053] Furthermore, when the specific surface area of ​​the positive electrode active material is 0.5-1m 2 / g, the contact area between the positive electrode active material and the conductive agent and the binder is larger, which can improve the kinetic performance of the positive electrode sheet, make the positive electrode sheet have better lithium ion insertion and extraction ability, and thus improve the lithium precipitation window and rate performance of the battery.

[0054] The positive electrode active material of the present invention can be a polycrystalline positive electrode active material or a single crystal positive electrode active material. Compared with polycrystalline positive electrode active materials, single crystal positive electrode active materials are less likely to have grain boundary cracking and secondary particle crushing during the charge and discharge process of the battery, thereby improving the cycle performance of the battery; it can also reduce the probability of side reactions and avoid the increase in the impedance of the positive electrode sheet; and the single crystal positive electrode active material can also increase the compaction density of the positive electrode active layer, thereby increasing the energy density of the battery.

[0055] In some embodiments of the present invention, the positive electrode active layer includes an additive, and the additive is selected from at least one of maleic acid, catechol acid, phenolic acid, succinic acid, and a copolymer formed by at least two of the foregoing substances.

[0056] The positive electrode active layer of the present invention includes an additive, and the carboxyl group in the additive can effectively neutralize the alkali content on the surface of the positive electrode active material, thereby preventing the alkali on the surface of the positive electrode active material from attacking the CH bond and the CF bond in the binder during the homogenization process, thereby causing the CH bond and the CF bond to undergo an elimination reaction to form a C=C bond, which can further prevent the C=C bond from chemically cross-linking, thereby causing the positive electrode slurry to gel and jelly, thereby improving the processing difficulty of the positive electrode slurry, and improving the stability and coating performance of the positive electrode slurry; and because the additive can reduce the residual alkali content of the positive electrode active layer, it helps to further improve the cycle performance of the battery.

[0057] In the present invention, the additive can neutralize the residual alkali content on the surface of the positive electrode active material. In particular, when the pH of the positive electrode active material satisfies: 8≤pH≤12.5, the additive can still neutralize the residual alkali content on the surface of the positive electrode active material.

[0058] The inventors found in their research that when the relative molecular mass of the additive is 98-2000 g / mol, the additive can better neutralize the residual alkali on the surface of the positive electrode active material, improve the coating property of the positive electrode slurry, reduce the residual alkali content of the positive electrode active layer, and improve the cycle performance of the battery. Furthermore, the smaller the relative molecular mass of the additive, the more significant the improvement in the performance of the positive electrode sheet, and the more conducive to improving the cycle performance of the battery.

[0059] In some embodiments, in the additive, the particle size of the secondary particles is 10-1000 μm, and the particle size of the primary particles is 2-10 μm.

[0060] Normally, the primary particles of additives are composed of carbon, hydrogen, and oxygen atoms in a certain proportion, forming a specific molecular structure. This structure determines the chemical properties and reaction characteristics of the additive. Secondary particles are larger structural units formed by the aggregation of multiple primary particles. At the secondary particle level, there are generally multiple primary particles aggregated together to form a microscopic particle structure. This structure affects the physical properties of the secondary particles, such as particle size and shape, and thus affects their performance and performance in the positive electrode sheet. By combining primary and secondary particles of specific particle sizes, the stability of the positive electrode slurry can be improved, the stability of the positive electrode sheet can be improved, and the overall performance of the battery can be improved. Figure 1 is the SEM image of maleic acid. Figure 1 It can be seen that maleic acid consists of primary particles and secondary particles, and the particle size of the primary particles is 2-10 μm, and the particle size of the secondary particles is 10-1000 μm.

[0061] In some embodiments of the present invention, the resistivity of the positive electrode sheet is 0.2-5 KΩ·cm; and / or the surface resistance of the positive electrode sheet is 20-600 mΩ.

[0062] When the resistivity of the positive electrode sheet and / or the surface resistance of the positive electrode sheet meets the above range, it indicates that the microstructure uniformity of the positive electrode active layer is better, for example, the adhesion between the positive electrode collector and the positive electrode active layer is tighter, the conductive agent in the positive electrode active layer is more evenly distributed, and the contact between the positive electrode active material particles and between the positive electrode active material particles and the conductive agent particles is tighter. The obtained positive electrode sheet has more excellent kinetic properties and excellent lithium ion deintercalation ability, which can improve the lithium plating window and rate performance of the battery.

[0063] In some embodiments of the present invention, in the positive electrode sheet, the average peeling force between the positive electrode active layer and the positive electrode current collector is 0.01-0.2 kgf.

[0064] The inventors found that when the average peeling force between the positive electrode active layer and the positive electrode current collector meets the above range, during the cycle of the battery, the bonding performance between the positive electrode active layer and the positive electrode current collector is still excellent, which can ensure the electrical connection between the positive electrode active layer and the positive electrode current collector, so that the positive electrode sheet can transmit current more effectively, improve the cycle performance of the battery, and extend the service life of the battery.

[0065] The inventors also found that when the porosity of the positive electrode active layer is 20-40%, the electrolyte can more fully infiltrate the positive electrode active layer, improve the ionic conductivity of the positive electrode sheet, reduce the internal resistance of the battery, and significantly improve the rate performance and cycle performance of the battery.

[0066] In some embodiments of the present invention, the tensile strength of the positive electrode current collector is ≥150 MPa.

[0067] When the tensile strength of the positive electrode current collector meets the above range, the positive electrode current collector has a better conductivity, can transmit electrons from the positive electrode sheet of the battery to the external circuit, can also reduce the internal resistance of the battery, and improve the energy utilization rate of the battery. And when the positive electrode current collector with the tensile strength in the above range is applied to the battery, it is not easy to deform, break or tear with the volume expansion and contraction of the positive electrode active material during the charge and discharge cycle of the battery, and it is not easy to damage the internal structure of the battery, thereby improving the structural stability of the battery, improving the safety of the battery, and extending the service life of the battery.

[0068] Furthermore, when the surface roughness of the positive electrode current collector is 0.1-1.5 μm, the adhesion between the positive electrode active layer and the positive electrode current collector can be improved, local poor contact or microscopic gaps between the positive electrode active layer and the positive electrode current collector can be avoided, the conductivity of the positive electrode sheet can be improved, and the possibility of side reactions on the surface of the positive electrode current collector (for example, oxidation reaction of the positive electrode active material, reduction reaction of the positive electrode active material) can be reduced, thereby improving the cycle performance of the battery.

[0069] In some embodiments, when the thickness of the positive electrode collector is 8-16 μm, the tensile strength of the positive electrode collector is ≥150 MPa, and the surface roughness of the positive electrode collector is 0.1-1.5 μm, the positive electrode slurry can be more evenly and effectively coated and distributed on the surface of the positive electrode collector, reducing the uneven stacking of the positive electrode active material and the local thickness difference of the positive electrode active layer, improving the structural stability of the positive electrode sheet, and reducing the risk of stress concentration and structural damage caused by the expansion of the positive electrode active material during the charge and discharge process of the battery. The cycle life of the battery is extended, and the increase in the internal voids of the battery due to deformation of the positive electrode collector and the occurrence of problems such as peeling of the positive electrode active layer are reduced, thereby improving the energy density and cycle performance of the battery.

[0070] In some embodiments of the present invention, in the X-ray diffraction spectrum, the positive electrode active layer has a crystal plane index peak of (-2, 0, 2) with 2θ of 25-30°.

[0071] The (-2, 0, 2) crystal plane index peak with 2θ of 25-30° in the XRD graph of the positive electrode active layer of the present invention indicates that an additive exists in the positive electrode active layer, and the additive is a monoclinic crystal system.

[0072] Furthermore, by refining the XRD spectrum of the positive electrode active layer, it can be obtained that the space group of the positive electrode active layer is P1 21 / c 1.

[0073] In some embodiments, the positive electrode sheet of the first aspect can be prepared by a method comprising the following steps:

[0074] The binder, the conductive agent, the positive electrode active material and the additive are fully mixed in the solvent to obtain a positive electrode slurry;

[0075] Placing the positive electrode slurry on at least one surface of the positive electrode current collector, and forming a positive electrode sheet including a positive electrode active layer after drying and rolling;

[0076] The additive is selected from at least one of maleic acid, catechol acid, phenolic acid, succinic acid and copolymers formed by at least two of the foregoing substances;

[0077] The thickness of the positive electrode current collector is 8-16 μm; the thickness of the positive electrode active layer is 10-100 μm.

[0078] Furthermore, in the positive electrode active layer, the mass percentages of the positive electrode active material, the conductive agent, the adhesive and the additive are 94%-97%: 0.5%-3%: 1%-2%: 0.01%-1%. In the present invention, the amount of additives added is relatively small, which can improve the power performance and cycle performance of the battery while ensuring the energy density of the battery.

[0079] In some embodiments, the positive electrode slurry can be prepared by a method comprising the following steps:

[0080] dissolving the additive in a solvent to obtain an additive solution;

[0081] dissolving the adhesive in a solvent to obtain an adhesive glue solution;

[0082] Adding a conductive agent to the binder glue solution, stirring evenly, and then adding a positive electrode active material, stirring evenly, to obtain a positive electrode glue solution;

[0083] Adding the additive solution to the positive electrode glue solution and stirring evenly to obtain a positive electrode slurry;

[0084] The solvent may be N-methylpyrrolidone. In the process of preparing the additive solution, the additive may be added into the N-methylpyrrolidone while being added with stirring. After the addition is completed, stirring is continued for 20 minutes to obtain the additive solution.

[0085] A second aspect of the present invention provides a battery, comprising the positive electrode sheet of the first aspect.

[0086] It can be understood that the battery also includes a negative electrode sheet, a separator, an electrolyte and an outer packaging.

[0087] In the present invention, the positive electrode sheet, separator and negative electrode sheet of the first aspect can be stacked to obtain an electrode assembly of a laminated structure, and then the electrode assembly of the laminated structure can be placed in an outer package, electrolyte is injected into the outer package, and a battery is obtained after drying and sealing; the positive electrode sheet, separator and negative electrode sheet of the first aspect can also be stacked, and then wound to obtain an electrode assembly of a wound structure, and then the electrode assembly of the wound structure can be placed in an outer package, electrolyte is injected into the outer package, and a battery is obtained after drying and sealing.

[0088] The battery of the present invention comprises the positive electrode sheet of the first aspect, so the battery has excellent cycle performance and power performance, and is suitable for wide promotion and application.

[0089] The technical solution of the present invention will be further described below in conjunction with specific embodiments.

[0090] Example 1

[0091] The battery of this embodiment is prepared by a method comprising the following steps:

[0092] 1) Preparation of positive electrode slurry

[0093] First, the adhesive polyvinylidene fluoride PVDF is added to N-methylpyrrolidone and stirred to obtain PVDF glue; then a conductive agent (conductive carbon black) is added to the PVDF glue and stirred to obtain a positive electrode glue; then the positive electrode active material NCM811 is added and stirred to obtain a positive electrode glue;

[0094] Add the additive to the positive electrode glue solution, stir while adding, and continue stirring for 20 minutes after the addition is completed to fully dissolve it to obtain an additive solution; then add the additive solution to the positive electrode glue, stir it thoroughly and evenly to obtain a positive electrode slurry;

[0095] Among them, the mass ratio of positive electrode active material, conductive agent, binder and additive is 96.4%:2%:1.6%:0.05% (due to the low content of additives, they can be excluded from the formula).

[0096] 2) Preparation of positive electrode

[0097] The positive electrode slurry is evenly coated on both surfaces of the aluminum foil; then baked in an oven with 5 different temperature gradients, and then dried in an oven at 120°C for 8 hours, and then rolled and cut to obtain the positive electrode sheet;

[0098] Other parameters of the positive electrode sheet of this embodiment are shown in Table 1.

[0099] 3) Preparation of negative electrode

[0100] The negative electrode active material (including SiC and artificial graphite, the mass ratio of SiC to artificial graphite is 5:95), thickener sodium carboxymethyl cellulose (CMC-Na), binder styrene butadiene rubber, single-walled carbon nanotubes, and conductive agent acetylene black are mixed in a weight ratio of 96.5:1:1.5:0.4:0.6, deionized water is added, and the negative electrode slurry is obtained under the action of a vacuum mixer; the negative electrode slurry is evenly coated on both surfaces of a copper foil with a thickness of 5 μm; then after drying at room temperature, it is transferred to an oven at 80°C for drying for 10 hours, and the desired negative electrode sheet is obtained through cold pressing and slitting.

[0101] 4) Preparation of electrolyte

[0102] In a glove box filled with argon and with a qualified water and oxygen content, ethylene carbonate, propylene carbonate, and n-propyl propionate are uniformly mixed in a mass ratio of 15:10:75 (the solvent and the additive need to be normalized together), 14 wt% of fully dried lithium hexafluorophosphate (LiPF6) is quickly added thereto, stirred evenly, and cooling measures are taken to ensure that the temperature of the batching kettle is below 10°C during the addition of LiPF6, and then 15% of fluoroethylene carbonate, 4% of 1,3-propanesulfonate, 2% of succinonitrile, 3% of 1,3,6-hexanetrinitrile are added, and 2% of siloxane additive A5 is added at the same time. Stir again until uniform, and after passing the moisture and free acid tests, the electrolyte is obtained.

[0103] 5) Preparation of batteries

[0104] The positive electrode sheet, the separator, and the negative electrode sheet are stacked in order, ensuring that the separator is between the positive electrode sheet and the negative electrode sheet, and then the electrode assembly without liquid injection is obtained by winding; the electrode assembly is placed in an outer packaging foil, and the electrolyte is injected into the dried electrode assembly. After vacuum packaging, standing, forming, shaping, sorting and other processes, a battery is obtained, and the charging cut-off voltage of the obtained battery is 4.2V;

[0105] The separator is a polyethylene separator with a thickness of 8 μm (provided by Asahi Kasei Corporation).

[0106] Examples 1-18, Comparative Examples 1-4

[0107] The preparation methods of the batteries of Examples 1-18 and Comparative Examples 1-4 are substantially the same as that of Example 1, and the differences are shown in Table 1.

[0108] Performance Testing

[0109] The following performance tests were performed on the positive electrode slurries, positive electrode sheets and batteries in the examples and comparative examples, and the results are shown in Table 2-3;

[0110] 1. Cathode slurry stability test

[0111] The positive electrode slurry of Example 1 was placed in an environment with a temperature of 25° C. and a humidity of ≤5%. The viscosity and solid content of the slurry were tested every 6 hours. The test results are shown in Table 2.

[0112] 2. Surface resistance and resistivity test of positive electrode

[0113] Surface resistance test: Cut the rolled positive electrode sheet into a rectangular size of about 5cm×10cm and place it between the two electrodes of the membrane resistance meter. Set the test pressure to 0.4t and the holding time to 3s on the MRMS software. Start the test and read the resistance data of the positive electrode sheet. Randomly select 10 positions for each membrane for testing. The test results are shown in Table 3.

[0114] Resistivity test: Cut the rolled positive electrode sheet into a rectangular size of about 5 cm × 10 cm, place it on the sample table of a multifunctional digital four-probe tester, set the measurement parameters, test for 5 seconds, read the resistivity data of the positive electrode sheet, and randomly select 3 positions for each electrode sheet for single-sided and double-sided resistivity tests. The test results are shown in Table 3.

[0115] 3. Battery liquid level, battery capacity, battery internal resistance, ED test

[0116] Weigh the battery after filling and after leaving the stage, the liquid retention amount = the weight after filling - the weight after leaving the stage;

[0117] The lithium-ion battery is charged to full capacity at constant current and constant voltage at 25°C, and then discharged to 2.5V at 0.2C. The discharged capacity is recorded as the battery capacity.

[0118] Charge the lithium-ion battery to 30% SOC at 25°C and use an internal resistance tester to test the internal resistance of the battery;

[0119] Charge the lithium-ion battery to 30% SOC at 25°C and use 600g PPG to test the battery thickness; calculate the volume energy density = battery capacity * platform voltage / battery length / width / thickness;

[0120] The above test results are shown in Table 3.

[0121] 4. Lithium Separation Window

[0122] The lithium-ion battery was charged and discharged for 20T using the following system and then dissected to confirm the lithium precipitation window: 25 degrees 3C / 10C-20T, 0℃1C / 10C-20T, -10℃0.3C / 10C-20T; the test results are shown in Table 3.

[0123] 5. Rate discharge test

[0124] The lithium-ion battery was discharged at different rates at 25°C to test the discharge capacity retention rate and discharge temperature rise. The test results are shown in Table 3.

[0125] 6. Cycle performance test

[0126] The lithium-ion battery was subjected to a 1C / 7C cycle test at 25°C to test its retention rate and expansion rate. The test results are shown in Table 3.

[0127] 7. Infrared spectrum measurement of positive electrode

[0128] Maleic acid and the positive electrode were characterized using an infrared spectrometer, infrared spectrum curves of maleic acid and the positive electrode were obtained, and the peak area in the infrared spectrum curve was calculated using Origin data analysis software. The following is a detailed description of the specific steps: First, the infrared spectrum data obtained from the experiment was imported into the worksheet of the Origin software, with the wavelength (or wave number) as the X-axis variable and the corresponding infrared absorption intensity as the Y-axis variable; then, the infrared spectrum was drawn in the Graph window of Origin using the data in the worksheet. In the spectrum, the characteristic absorption peaks corresponding to different functional groups or compounds will be displayed with different intensities and positions. In order to calculate the area of ​​these peaks, the "PeakAnalyzer" advanced analysis tool built into the Origin software was used. The peaks in the spectrum are automatically identified, and the peak position, width and baseline are fine-tuned as needed to ensure the accuracy of peak identification. After completing peak identification and baseline correction, the Origin software will automatically perform an integral operation on each selected peak to calculate its corresponding peak area.

[0129] Figure 2 is the infrared spectrum curve of maleic acid; Figure 3 : is the infrared spectrum curve of the positive electrode sheet in Example 1 of the present invention and Comparative Example 1. Figure 2 and Figure 3 It can be seen that Example 1 at 2500cm -1 -3500cm -1 The first characteristic peak in the range is obviously broadened, at 1500cm -1 -2000cm -1 A second characteristic peak appears in the range of , and the ratio of the peak area of ​​the first characteristic peak to the peak area of ​​the second characteristic peak is 1.41, indicating that the positive electrode sheet in the embodiment has a carboxyl group and a C=C double bond, and the content of the carboxyl group and the C=C double bond is appropriate, which can improve the cycle performance and power performance of the battery.

[0130] 8. XRD test

[0131] XRD was used to characterize maleic acid and the positive electrode active layer.

[0132] Figure 4 is the XRD curve of maleic acid; Figure 5 XRD curves of the positive electrode active layer in Example 1 and Comparative Example 1 of the present invention; Figure 6 for Figure 5 A partial enlarged view of the Figure 4-6 It can be seen that the positive electrode active layer in the embodiment of the present invention has a crystal plane index peak of (-2,0,2) at 27.97°, and the crystal plane index peak is caused by the addition of maleic acid. Since the positive electrode sheet has this crystal plane index peak, the cycle performance and power performance of the battery can be further improved.

[0133] Table 1

[0134]

[0135]

[0136]

[0137] Table 2

[0138]

[0139] It can be seen from Table 2 that by adding 0.05% of the additive, the stability of the positive electrode slurry of Example 1 is significantly improved, and no gel jelly appears in the positive electrode slurry, indicating that the use of the additive can reduce the alkali content on the surface of the positive electrode active material and avoid the elimination reaction of CH and CF of PVDF.

[0140] Table 3

[0141]

[0142]

[0143]

[0144] It can be seen from Table 3 that, compared with the comparative example, the battery in the embodiment of the present invention has lower internal resistance, excellent cycle performance and rate performance; in particular, compared with comparative example 1, the resistance of the positive electrode sheet of embodiment 1 is reduced by one time compared with the resistance of the positive electrode sheet of comparative example 1, indicating that the introduction of the additive can enhance the adhesion between the positive electrode active material particles, while reducing the impedance between the positive electrode collector and the positive electrode active layer, so that the resistance of the positive electrode sheet is significantly reduced; the resistivity of the positive electrode sheet of embodiment 1 is reduced to a certain extent compared with the resistivity of the positive electrode sheet of comparative example 1, indicating that the introduction of the additive can enhance the adhesion between the positive electrode active material particles, while reducing the impedance between the positive electrode collector and the positive electrode active layer, so that the resistance of the positive electrode sheet is significantly reduced. The battery in the embodiment has improved liquid retention capacity, capacity, and energy density, and its internal resistance is significantly reduced, indicating that the addition of additives can improve the absorption rate of the positive electrode sheet to the electrolyte, the electrochemical stability of the positive electrode sheet, and reduce the impedance between the positive electrode collector and the positive electrode active layer, thereby improving the battery's liquid retention energy, the battery's internal conductivity, the battery's capacity, and reducing the battery's internal resistance; the battery in Example 1 has a significantly improved lithium precipitation window at low temperatures, indicating that the addition of additives can reduce the polarization of the positive electrode active material of the battery at low temperatures, improve the battery's kinetic performance, and thus broaden the battery's lithium precipitation window; the rate discharge temperature of the battery in Example 1 is significantly reduced, indicating that the addition of additives improves the battery's absorption rate to the electrolyte, improves the ion conduction energy, reduces the impedance between the positive electrode collector and the positive electrode active layer, and reduces the internal impedance of the battery cell. From the formula Q=I 2 RT, internal resistance is reduced, heat generation is reduced, and discharge temperature rise is reduced; the cycle capacity retention rate of the battery in Example 1 is significantly improved, indicating that the positive electrode active material and the conductive agent are firmly adhered to the positive electrode current collector during the cycle, so that the positive electrode active material and the positive electrode current collector maintain good contact, forming a good conductive electron network, and at the same time, due to better absorption of electrolyte energy, a good ion conductive network is formed between the positive electrode active material and the electrolyte; in addition, since the residual alkali in the high-nickel ternary material is neutralized, the side reaction on the positive electrode side is significantly reduced, and the stability of the positive electrode active material is improved, thereby improving the cycle life of the battery; compared with Comparative Example 2, the battery in the embodiment of the present invention has a better performance in terms of compatibility. In the case of having lower internal resistance, excellent cycle performance and rate performance, it also has better energy density, indicating that by adding additives to the positive electrode active layer, matching the thickness of the positive electrode active layer, and further matching the thickness of the positive electrode current collector, the battery can have lower internal resistance, excellent cycle performance, rate performance and energy density; compared with Comparative Example 3, the battery in the embodiment of the present invention has lower internal resistance and better cycle performance, indicating that by adding additives to the positive electrode active layer, matching the thickness of the positive electrode current collector, and further matching the thickness of the positive electrode active layer, the internal resistance of the battery can be further reduced and the cycle performance of the battery can be improved;

[0145] It can be seen from Examples 1, 8, 9 and 10 that by selecting the particle size of the positive electrode material, the internal resistance of the battery can be further reduced, and the cycle performance, rate performance and energy density of the battery can be improved;

[0146] It can be seen from Examples 1, 14, 15 and 16 that the energy density and cycle performance of the battery can be improved by further selecting the porosity of the positive electrode active layer;

[0147] It can be seen from Examples 1, 17 and 18 that the energy density and cycle performance of the battery can be further improved by further selecting the tensile strength of the positive electrode current collector.

[0148] Each embodiment in this specification is described in a related manner, and the same or similar parts between the embodiments can be referred to each other, and each embodiment focuses on the differences from other embodiments. The above are only preferred embodiments of the present invention and are not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention are included in the scope of protection of the present invention.

Claims

1. A positive electrode sheet, It is characterized in that The positive electrode sheet comprises a positive electrode current collector and a positive electrode active layer located on at least one surface of the positive electrode current collector; The thickness of the positive electrode current collector is 8-16 μm, and the thickness of the positive electrode active layer is 80-130 μm; In the infrared spectrum curve, the positive electrode has a wavelength of 2500cm -1 -3500cm -1 The first characteristic peak of -1 -2000cm -1 The second characteristic peak of The peak area S1 of the first characteristic peak and the peak area S2 of the second characteristic peak satisfy: 1<S1 / S2<2.

2. The positive electrode sheet according to claim 1, It is characterized in that The positive electrode active layer further includes a positive electrode active material, and the molecular formula of the positive electrode active material is shown in Formula 1; LiNi x Co y Mn z Al w M a O 2 Formula 1; In Formula 1, 0.8≤x<1, 0<y<0.2, 0<z<0.2, 0≤w≤0.05, 0≤a≤0.1, x+y+z+w+a=1; M is selected from at least one of Mg, Ti, Zr, Y, B, W, and Sr.

3. The positive electrode sheet according to claim 2, It is characterized in that The particle size of the positive electrode active material is 2-5 μm.

4. The positive electrode sheet according to any one of claims 1 to 3, It is characterized in that The positive electrode active layer includes an additive, and the additive is selected from at least one of maleic acid, catechol acid, phenolic acid, succinic acid, and a copolymer formed by at least two of the foregoing substances.

5. The positive electrode sheet according to claim 4, It is characterized in that The relative molecular mass of the additive is 98-2000 g / mol.

6. The positive electrode sheet according to any one of claims 1 to 5, It is characterized in that The resistivity of the positive electrode sheet is 0.2-5 KΩ·cm; and / or the surface resistance of the positive electrode sheet is 20-600 mΩ.

7. The positive electrode sheet according to any one of claims 1 to 6, It is characterized in that In the positive electrode sheet, an average peeling force between the positive electrode active layer and the positive electrode current collector is 0.01-0.2 kgf.

8. The positive electrode sheet according to any one of claims 1 to 7, It is characterized in that The porosity of the positive electrode active layer is 20-40%.

9. The positive electrode sheet according to any one of claims 1 to 8, It is characterized in that The tensile strength of the positive electrode current collector is ≥150 MPa.

10. The positive electrode sheet according to any one of claims 1 to 9, It is characterized in that In the X-ray diffraction spectrum, the positive electrode active layer has a crystal plane index peak of (-2, 0, 2) with 2θ of 25-30°; And / or, the space group of the positive electrode active layer is P1 21 / c 1.

11. A battery, It is characterized in that The battery comprises the positive electrode sheet according to any one of claims 1 to 10.

Citation Information

Cited By

  • Positive pole piece, secondary battery and electronic device

    CN119673957A

  • A positive electrode sheet, a secondary battery, and an electronic device

    CN119673957B