Battery and preparation method thereof

By installing a modified epoxy resin insulating layer on the inner wall surface of the battery case, the problem of reducing the liquid retention of the battery cell caused by the thickening of the nano-injection-molded composite polymer film is solved, and the battery cell cycle life is improved and the metal shell corrosion is avoided. Effect.

CN119069901APending Publication Date: 2024-12-03JIANGSU ZENIO NEW ENERGY BATTERY TECH CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411376173.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-30
Publication Date
2024-12-03

Smart Images

  • Figure CN119069901A_ABST
    Figure CN119069901A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of batteries, in particular to a battery and a preparation method thereof. The battery comprises a shell, wherein the inner wall of the shell is provided with a plurality of first hole structures; the insulating layer is arranged on the surface of the inner wall of the shell and in the first hole structure, and the insulating layer is provided with a pore structure; the insulating layer comprises modified epoxy resin, and the modified epoxy resin is a condensation product of epoxy resin and a liquid retaining agent. The epoxy resin insulating layer containing the liquid retaining agent is arranged on the surface of the inner wall of the shell of the battery, so that the liquid retaining property of the insulating layer can be greatly improved, meanwhile, the corrosion condition of the metal shell is avoided, and the cycle life of a battery cell is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of battery technology, and in particular to batteries and methods for preparing the same. Background Art

[0002] At present, aluminum shell batteries mainly use Mylar film (insulating film), bottom support sheet (bottom support plate) and rubber encapsulation to achieve reliable sealing and protection of the battery cells, so that the battery cells and the inside of the aluminum shell are insulated, avoiding the formation of aluminum-lithium alloy and other side reactions when the battery is in use, thereby avoiding corrosion to the inside of the aluminum shell.

[0003] At present, some researchers use nano injection molding technology to set a layer of injection molding material on the inner wall surface of the aluminum shell to replace the Mylar film and the bottom support sheet, so as to achieve the sealing and protection of the battery cell. The binder used in the injection molding material is epoxy resin. Epoxy resin has excellent bonding properties to metal materials such as aluminum, iron, and copper. The molecular chain of epoxy resin contains hydroxyl groups, ether groups, and active epoxy groups. The epoxy groups react with the free bonds on the metal surface to form chemical bonds, which greatly improves the bonding force between the injection molding material and the inner wall and bottom of the aluminum shell, making the inner wall and bottom of the aluminum shell composite polymer film with the advantages of chemical corrosion resistance, strong adsorption, heat resistance, and electrical insulation. This technology can eliminate the design of the Mylar film and the bottom support sheet, reduce the battery cell process, and reduce the weight of the battery, thereby better promoting the further development of aluminum shell batteries.

[0004] However, the nano-injection-molded composite polymer film thickens the thickness of the aluminum shell, resulting in a significant decrease in the liquid retention capacity of the battery cell. The reduction in the amount of electrolyte accelerates the attenuation of the cycle life of the battery cell. Summary of the invention

[0005] In view of this, the present invention provides a battery and a method for preparing the same. The present invention can greatly improve the liquid retention of the insulation layer by arranging an epoxy resin insulation layer containing a liquid retaining agent on the inner wall surface of the battery shell, while avoiding corrosion of the metal shell and improving the cycle life of the battery core.

[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions: In a first aspect, the present invention provides a battery, comprising: A shell, the inner wall of which has a plurality of first hole structures; The insulating layer is arranged on the inner wall surface of the shell and in the first hole structure, and the insulating layer has a pore structure; the insulating layer includes modified epoxy resin, and the modified epoxy resin is a condensation product of epoxy resin and a liquid retaining agent.

[0007] In an embodiment of the present invention, the monomer of the epoxy resin includes at least one of bisphenol diglycidyl ether and polyphenol glycidyl ether.

[0008] In an embodiment of the present invention, the liquid retaining agent includes at least one of chitosan, chitin, carboxymethyl chitosan, and cyclodextrin.

[0009] Preferably, the diameter of the first hole structure is 500-800 nm.

[0010] Preferably, the inner wall of the first hole structure has a plurality of second hole structures.

[0011] Preferably, the diameter of the second hole structure is 10-500 nm.

[0012] In an embodiment of the present invention, the shell is a square shell, which includes a large shell surface, a shell side wall and a shell bottom; the thickness of the insulating layer on the inner wall surface of the large shell surface is recorded as H1, and the thickness of the insulating layer on the inner wall surface of the shell bottom is recorded as H2, and the ratio of H1 to H2 is (2-4): (7-13).

[0013] Preferably, the porosity of the insulating layer is 2% to 5%.

[0014] In a second aspect, the present invention provides a method for preparing the above-mentioned battery, comprising the following steps: S1, performing alkaline etching treatment on the inner wall of the shell to obtain an alkaline-etched shell; S2, performing pickling treatment on the inner wall of the shell after the alkaline etching treatment to obtain a shell having a first hole structure; S3, subjecting the epoxy resin and the liquid retaining agent to a ring-opening condensation reaction in a solvent to obtain a reaction product including a modified epoxy resin; The reaction product including the modified epoxy resin, the pore-forming additive, the antioxidant, the antistatic agent and the curing agent are uniformly mixed, and after degassing treatment, an insulating layer slurry is obtained; The insulating layer slurry is disposed on the inner wall surface and the hole structure of the shell obtained in step S2, and after drying, a shell composited with the insulating layer is obtained; S4, uses a shell with a composite insulating layer to assemble the battery.

[0015] In an embodiment of the present invention, in step S1, the reagent used for the alkaline etching treatment is an alkaline etching solution.

[0016] In an embodiment of the present invention, in step S2, the reagent used for the pickling treatment is a pickling solution.

[0017] In the embodiment of the present invention, between step S2 and step S3, the method further includes: electrochemically treating the inner wall of the first hole structure to etch out the second hole structure.

[0018] In an embodiment of the present invention, the reagent used for the electrochemical treatment is an electrochemical solution.

[0019] In an embodiment of the present invention, the alkaline etching solution includes at least one of a tromethamine solution, a potassium hydroxide solution, a barium hydroxide solution, and a sodium carbonate solution.

[0020] Preferably, the pH value of the alkaline etching solution is 8-11.

[0021] Preferably, the concentration of the alkaline etching solution is 20wt% to 40wt%.

[0022] Preferably, the temperature of the alkaline etching treatment is 30 to 70° C., and the time of the alkaline etching treatment is 80 to 90 s.

[0023] In an embodiment of the present invention, the pickling solution includes at least one of a methanesulfonic acid solution, a hydrochloric acid solution, and a hydrofluoric acid solution.

[0024] Preferably, the concentration of the pickling solution is 30 wt % to 50 wt %.

[0025] Preferably, the temperature of the pickling treatment is 30 to 50° C., and the time of the pickling treatment is 110 to 120 s.

[0026] In an embodiment of the present invention, the electrochemical solution includes at least one of acetic acid solution, carbonic acid solution, silicic acid solution, nitrous acid solution, hydrosulfuric acid solution, hypochlorous acid solution, sulfurous acid solution, hydrocyanic acid solution, and oxalic acid solution.

[0027] Preferably, the concentration of the electrochemical solution is 10 wt % to 20 wt %.

[0028] Preferably, the temperature of the electrochemical treatment is 50 to 60° C., and the time of the electrochemical treatment is 10 to 20 min.

[0029] Preferably, in step S3, the reaction temperature of the ring-opening condensation reaction is 50 to 80° C., and the reaction time of the ring-opening condensation reaction is 6 to 12 h.

[0030] In an embodiment of the present invention, the solvent includes at least one of dimethylformamide and dichloromethane.

[0031] Preferably, the insulating layer comprises the following raw material components in parts by weight: Epoxy resin 40-60 parts 8-20 portions of liquid retaining agent Pore-forming additive 5-30 parts 2-8 parts of antioxidant Antistatic agent 0.5-5 parts 5 to 20 parts of curing agent.

[0032] Compared with the prior art, the present invention has the following beneficial effects: 1. The present invention generates a modified epoxy resin by a ring-opening condensation reaction between an epoxy resin and a liquid retaining agent, and then uses the modified epoxy resin to prepare an insulating layer on the inner wall surface of a battery shell. The liquid retaining agent enables the insulating layer to have a higher liquid retention property, thereby improving the injection coefficient of the nano injection molded metal shell; At the same time, liquid retaining agents such as chitosan also have good film-forming properties and permeability, which are more conducive to the film-forming properties of the insulating layer, reduce the amount of epoxy resin used, reduce the thickness of the insulating layer, and further improve the injection coefficient of the metal shell; Moreover, since liquid retaining agents such as chitosan can chelate with metal ions, the functionality of the epoxy resin binder can be further improved after the epoxy resin and the liquid retaining agent undergo a ring-opening condensation reaction. The insulating layer will not spontaneously fall off from the surface of the metal shell, and the lithium ions can be prevented from reacting with the metal shell to form an alloy and cause corrosion of the shell.

[0033] 2. The present invention adopts nano-injection molding technology to prepare an insulating layer on the inner wall surface of the battery shell, which has a simple synthesis process, low manufacturing cost, and is easy to use commercially. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 Schematic diagram of the nano injection molding process of the present invention. DETAILED DESCRIPTION

[0035] The present invention discloses a battery and a method for preparing the same. Those skilled in the art can refer to the contents of this article and appropriately improve the process parameters to achieve the same. It should be particularly noted that all similar substitutions and modifications are obvious to those skilled in the art and are deemed to be included in the present invention. The methods and applications of the present invention have been described through preferred embodiments, and relevant personnel can obviously modify or appropriately change and combine the methods and applications described herein without departing from the content, spirit and scope of the present invention to implement and apply the technology of the present invention.

[0036] In the description of the present invention, it should be noted that the terms "first", "second", etc. are only used for descriptive purposes, and do not indicate or imply relative importance.

[0037] In the description of the present invention, a list of items connected by the term "at least one of" or other similar terms may mean any combination of the listed items. For example, if items A, B are listed, the phrase "at least one of A, B" means only A; only B; or A and B. In another example, if items A, B, C are listed, the phrase "at least one of A, B, C" means only A; or only B; only C; A and B (excluding C); A and C (excluding B); B and C (excluding A); or all of A, B, and C. Item A may include a single element or multiple elements. Item B may include a single element or multiple elements. Item C may include a single element or multiple elements.

[0038] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range or the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0039] If not otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.

[0040] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.

[0041] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.

[0042] Specifically, the present invention adopts the following technical solutions: In a first aspect, the present invention provides a battery, comprising: A shell, the inner wall of which has a plurality of first hole structures; The insulating layer is arranged on the inner wall surface of the shell and in the first hole structure, and the insulating layer has a pore structure; the insulating layer includes modified epoxy resin, and the modified epoxy resin is a condensation product of epoxy resin and a liquid retaining agent.

[0043] The present invention arranges an insulating layer on the inner wall surface of the battery shell and in the first hole structure, wherein the insulating layer comprises a condensation product of an epoxy resin and a liquid retaining agent. The insulating layer has a pore structure, and the liquid retaining agent has a high liquid retaining property, so that the insulating layer has a high liquid retaining property, and the injection coefficient of the nano injection molded metal shell is improved.

[0044] In the embodiment of the present invention, the monomer of the epoxy resin includes at least one of bisphenol diglycidyl ether and polyphenol type glycidyl ether. The epoxy resin prepared by using the above monomers has excellent bonding properties to metal materials such as aluminum, iron, and copper. The molecular chain of the epoxy resin contains hydroxyl groups, ether groups, and active epoxy groups. The epoxy groups react with the free bonds on the metal surface to form chemical bonds, which greatly improves the bonding force between the injection molding material and the metal shell, so that the inner wall and the bottom of the shell are composited with a polymer film, which has the advantages of chemical corrosion resistance, strong adsorption, heat resistance, and electrical insulation.

[0045] In an embodiment of the present invention, the liquid retaining agent includes at least one of chitosan, chitin, carboxymethyl chitosan, and cyclodextrin. The above liquid retaining agent has good affinity and hydrophilicity with the electrolyte, and has excellent liquid absorption and retention function and electronic insulation.

[0046] In the present invention, the presence of the first hole structure has the function of anchoring the insulating layer, which is beneficial to improving the bonding strength between the insulating layer and the shell. Preferably, the diameter of the first hole structure is 500-800nm. Exemplarily, the diameter of the first hole structure is any value among 500nm, 550nm, 600nm, 650nm, 700nm, 750nm, 800nm ​​or any value within the range of any two of the above values.

[0047] Preferably, the inner wall of the first hole structure has a plurality of second hole structures. The second hole structures can provide the insulating layer with tensile resistance, thereby making the insulating layer more adhesive to the housing.

[0048] Preferably, the diameter of the second hole structure is 10-500 nm. Exemplarily, the diameter of the second hole structure is any value among 10 nm, 30 nm, 50 nm, 100 nm, 150 nm, 200 nm, 250 nm, 300 nm, 350 nm, 400 nm, 450 nm, 500 nm, or any value within the range formed by any two of the above values.

[0049] In an embodiment of the present invention, the shell is a square shell, and the square shell includes a large shell surface, a shell side wall and a shell bottom. The shell contains a battery cell, and the two side surfaces arranged in the thickness direction of the battery cell are the large shell surfaces, which are also the two surfaces with the largest area among the six surfaces of the square battery shell, and the two side surfaces arranged in the length direction of the battery cell are the shell side walls. Since the large shell surface is usually in contact with the battery cell, and the shell side wall is not in contact with the battery cell, in an embodiment of the present invention, the insulating layer only needs to be arranged on the inner wall of the large shell surface and the shell bottom, and the inner wall of the shell side wall may not be provided with an insulating layer.

[0050] In an embodiment of the present invention, the thickness of the insulating layer on the inner wall surface of the large surface of the shell is recorded as H1, and the thickness of the insulating layer on the inner wall surface of the bottom of the shell is recorded as H2. The ratio of H1 to H2 is (2-4): (7-13). Exemplarily, the ratio of H1 to H2 is any value among 2:7, 4:13, 3:10, 2:13, 4:7 or any value within the range of values ​​composed of any two of the above values. Under this thickness control, not only can the battery cell be completely insulated from the battery shell, but also the thicker insulating layer at the bottom of the shell can also raise the battery cell. The insulating layer is consistent with the R angle height, so that the bottom of the battery cell tends to be flat, avoiding the R angle at the bottom of the shell from squeezing the battery cell, and preventing the positive and negative electrodes from being squeezed at the bottom of the battery cell and contacting the metal at the bottom of the shell to cause a short circuit.

[0051] In the present invention, the insulating layer has a porous structure, which can accommodate electrolyte and improve the liquid retention of the insulating layer. Preferably, the porosity of the insulating layer is 2% to 5%. Exemplarily, the porosity of the insulating layer is any value among 2%, 3%, 4%, 5%, or any value within the range of any two of the above values.

[0052] In an embodiment of the present invention, the housing is a metal housing, and the material of the metal housing includes but is not limited to one of aluminum, iron, and copper, preferably aluminum.

[0053] In the embodiment of the present invention, the battery further comprises a battery cell and an electrolyte. The present application has no particular limitation on the battery cell and the electrolyte, and those skilled in the art can select them according to actual needs, as long as the purpose of the present application can be achieved.

[0054] In a second aspect, the present invention provides a method for preparing the above-mentioned battery, comprising the following steps: S1, performing alkaline etching treatment on the inner wall of the shell to obtain an alkaline-etched shell; S2, performing pickling treatment on the inner wall of the shell after the alkaline etching treatment to obtain a shell having a first hole structure; S3, subjecting the epoxy resin and the liquid retaining agent to a ring-opening condensation reaction in a solvent to obtain a reaction product including a modified epoxy resin; The reaction product including the modified epoxy resin, the pore-forming additive, the antioxidant, the antistatic agent and the curing agent are uniformly mixed, and after degassing treatment, an insulating layer slurry is obtained; The insulating layer slurry is disposed on the inner wall surface and the hole structure of the shell obtained in step S2, and after drying, a shell composited with the insulating layer is obtained; S4, uses a shell with a composite insulating layer to assemble the battery.

[0055] In the present invention, the alkaline etching treatment can remove the aluminum oxide film, grease and other impurities inside the shell. In an embodiment of the present invention, in step S1, the reagent used for the alkaline etching treatment is an alkaline etching solution.

[0056] In the present invention, on the one hand, the pickling treatment can etch a larger first hole structure on the inner wall surface of the shell; on the other hand, the pickling treatment can also remove the alkaline film remaining after step S1. In an embodiment of the present invention, in step S2, the reagent used for the pickling treatment is a pickling solution.

[0057] In the embodiment of the present invention, in order to etch a second hole structure with a smaller diameter in the first hole structure, between step S2 and step S3, it further includes: electrochemically treating the inner wall of the first hole structure to etch the second hole structure.

[0058] In an embodiment of the present invention, the reagent used for the electrochemical treatment is an electrochemical solution.

[0059] In the embodiment of the present invention, the alkaline etching solution includes but is not limited to at least one of tromethamine solution, potassium hydroxide solution, barium hydroxide solution, and sodium carbonate solution. As long as it is an alkaline solution, the purpose of alkaline etching treatment can be achieved.

[0060] Preferably, the pH value of the alkaline etching solution is 8 to 11. Exemplarily, the pH value of the alkaline etching solution is any value among 8, 9, 10, 11 or any value within the range of any two of the above values. When the pH value is greater than 11, the alkaline etching solution is too corrosive, the shell is corroded too much, and leakage is likely to occur.

[0061] Preferably, the concentration of the alkaline etching solution is 20 wt % to 40 wt %. Exemplarily, the concentration of the alkaline etching solution is any value among 20 wt %, 25 wt %, 30 wt %, 35 wt %, 40 wt % or any value within the range consisting of any two of the above values.

[0062] Preferably, the temperature of the alkaline etching treatment is 30-70°C, and the time of the alkaline etching treatment is 80-90 s. Exemplarily, the temperature of the alkaline etching treatment is any value among 30°C, 40°C, 50°C, 60°C, 70°C, or any value within the range of any two of the above values, and the time of the alkaline etching treatment is any value among 80s, 82s, 84s, 86s, 88s, 90s, or any value within the range of any two of the above values. When the temperature of the alkaline etching treatment is higher than 70°C, or the time of the alkaline etching treatment is greater than 90s, the shell is corroded too much and leakage is likely to occur.

[0063] In an embodiment of the present invention, the pickling solution includes but is not limited to at least one of a methanesulfonic acid solution, a hydrochloric acid solution, and a hydrofluoric acid solution.

[0064] Preferably, the concentration of the pickling solution is 30 wt % to 50 wt %. Exemplarily, the concentration of the pickling solution is any value among 30 wt %, 35 wt %, 40 wt %, 45 wt %, 50 wt % or any value within the range consisting of any two of the above values.

[0065] Preferably, the temperature of the pickling treatment is 30-50°C, and the time of the pickling treatment is 110-120 s. Exemplarily, the temperature of the pickling treatment is any value among 30°C, 35°C, 40°C, 45°C, 50°C, or any value within the range of any two of the above values, and the time of the pickling treatment is any value among 110 s, 112 s, 114 s, 116 s, 118 s, 120 s, or any value within the range of any two of the above values.

[0066] In an embodiment of the present invention, the electrochemical solution includes but is not limited to at least one of acetic acid solution, carbonic acid solution, silicic acid solution, nitrous acid solution, hydrosulfuric acid solution, hypochlorous acid solution, sulfurous acid solution, hydrocyanic acid solution, and oxalic acid solution.

[0067] Preferably, the concentration of the electrochemical solution is 10 wt% to 20 wt%. Exemplarily, the concentration of the electrochemical solution is any value among 10 wt%, 12 wt%, 14 wt%, 16 wt%, 18 wt%, 20 wt%, or any value within the range consisting of any two of the above values.

[0068] Preferably, the temperature of the electrochemical treatment is 50-60°C, and the time of the electrochemical treatment is 10-20 min. Exemplarily, the temperature of the electrochemical treatment is any value among 50°C, 52°C, 54°C, 56°C, 58°C, 60°C, or any value within the range of any two of the above values, and the time of the electrochemical treatment is any value among 10 min, 12 min, 14 min, 16 min, 18 min, 20 min, or any value within the range of any two of the above values. When the temperature of the electrochemical treatment is higher than 60°C, or the time of the electrochemical treatment is greater than 20 min, the shell is corroded too much and leakage is likely to occur.

[0069] In an embodiment of the present invention, the current intensity of the electrochemical treatment is 0.5-5A.

[0070] In the embodiment of the present invention, in step S1 or S2, after the alkaline etching treatment, the pickling treatment or the electrochemical treatment, a first cleaning and a first drying step are included.

[0071] In an embodiment of the present invention, the first cleaning is to use water to stir and clean the inner wall of the shell for 2 to 5 times.

[0072] In the embodiment of the present invention, the first drying is carried out by drying at a temperature of 60-70°C.

[0073] In order to remove residual impurities and enhance the water washing effect, in an embodiment of the present invention, after the first drying of step S2 and before step S3, a second washing and a second drying step are also included, the water temperature of the second washing is 50-60°C, the time of the second washing is 25-35 s; the temperature of the second drying is 70-90°C.

[0074] Preferably, in step S3, the reaction temperature of the ring-opening condensation reaction is 50 to 80°C, and the reaction time of the ring-opening condensation reaction is 6 to 12 h. Exemplarily, the reaction temperature of the ring-opening condensation reaction is any value of 50°C, 60°C, 70°C, 80°C, or any value within the range of any two of the above values, and the reaction time of the ring-opening condensation reaction is any value of 6 h, 7 h, 8 h, 9 h, 10 h, 11 h, 12 h, or any value within the range of any two of the above values.

[0075] In an embodiment of the present invention, the solvent includes but is not limited to at least one of dimethylformamide and dichloromethane.

[0076] In an embodiment of the present invention, the amount of solvent used is a conventional amount, for example, the mass ratio of epoxy resin, liquid retaining agent, and solvent is (40-60): (8-20): (30-50).

[0077] Preferably, the insulating layer comprises the following raw material components in parts by weight: Epoxy resin 40-60 parts 8-20 portions of liquid retaining agent Pore-forming additive 5-30 parts 2-8 parts of antioxidant Antistatic agent 0.5-5 parts 5 to 20 parts of curing agent.

[0078] In the embodiment of the present invention, the pore-forming additives include but are not limited to polyethylene glycol 200, white oil, C 6-15 Alkanes, C 8-15 Aliphatic carboxylic acid, C 1-4 At least one of the alkyl esters.

[0079] In an embodiment of the present invention, the antioxidant includes but is not limited to at least one of 4,4-thiobis(6-tert-butyl-m-cresol) and dibutylhydroxytoluene.

[0080] In the embodiment of the present invention, the antistatic agent includes but is not limited to octadecyl quaternary ammonium sodium, quaternary ammonium salts, and ethoxylated aliphatic alkylamines.

[0081] In an embodiment of the present invention, the curing agent includes but is not limited to at least one of diaminodicyclohexylmethane, triethylene glycol amine, boron trifluoride glycerol, and boron trifluoride aniline.

[0082] In an embodiment of the present invention, the mixing temperature of the pore-forming additive is 55 to 65° C., and the mixing and stirring time is 1 to 3 hours.

[0083] In an embodiment of the present invention, the degassing treatment is performed under vacuum conditions, and the temperature of the degassing treatment is 50-60°C.

[0084] In the embodiment of the present invention, the insulating layer slurry is disposed on the inner wall surface of the shell after the etching process by any one of spraying, scraping and coating.

[0085] In an embodiment of the present invention, in step S3, the drying temperature is 110-120° C., and the drying time is 20-40 min.

[0086] The reagents, instruments or materials used in the present invention can be obtained through commercial channels.

[0087] The present invention will be further described below in conjunction with embodiments: Example 1 (1) The prepared aluminum shell is subjected to alkaline etching, and the alkaline etching solution is selected to be a 30% tromethamine solution, the alkaline etching temperature is controlled at 30°C, and the time is controlled at 90s; after the alkaline etching is completed, it is stirred and washed three times with distilled water, and dried at 60°C; (2) The aluminum shell treated in step (1) is pickled, and the pickling solution is selected to be 40% methanesulfonic acid, the pickling temperature is controlled at 30°C, and the time is controlled at 120s to etch larger nanopores (nanopores are about 500-600 nm); after the pickling is completed, it is stirred and washed three times with distilled water, and dried at 60°C; (3) The aluminum shell treated in step (2) is subjected to electrochemical treatment (TRI), wherein the electrochemical treatment solution is 15% acetic acid, the temperature is controlled at 50°C, the current is 1.5A, the time is controlled at 20 min, and smaller nanopores (nanopores are about 30 to 150 nm) are etched; after etching, it is quickly washed three times with deionized water and dried at 60°C; then, it is washed with 50°C deionized water to enhance the washing effect, the time is controlled at 35s, and then transferred to an oven, the drying temperature is controlled at 80°C, and after drying, it is taken out and cooled to room temperature; (4) Injection molding material preparation: bisphenol diglycidyl ether (epoxy resin) 40kg, chitosan (liquid retaining agent) 8kg, polyethylene glycol 200 (pore-forming additive) 20kg, diaminodicyclohexylmethane (curing agent) 10kg, 4,4-thiobis(6-tert-butyl-m-cresol) (antioxidant) 6kg, octadecyl quaternary ammonium sodium (antistatic agent) 4kg, dimethylformamide (solvent) 30kg; Add epoxy resin and chitosan to dimethylformamide to carry out ring-opening condensation reaction, the reaction temperature is 50°C, and the reaction time is 12h; stir the reaction product and pore-forming additive at 65°C for 1h until they are evenly mixed, then add antioxidant and antistatic agent, continue to stir and mix evenly, finally add curing agent, stir for 15min with residual temperature, put into vacuum dryer for degassing treatment, and control the temperature at 55°C to obtain epoxy resin slurry; (5) Apply the epoxy resin slurry at 55±2℃ in step (4) to Figure 1 The large surface of the aluminum shell (① and ②) and the bottom of the aluminum shell (③) shown have a slurry thickness of 1.5 mm for the large surface of the aluminum shell and a slurry thickness of 5.25 mm for the bottom of the aluminum shell, with a thickness ratio of 2:7; they are then placed in an oven to dry with the temperature controlled at 115°C and the drying time of 30 minutes, and finally an aluminum shell with an insulating layer on the inner wall is prepared for use in aluminum shell batteries.

[0088] Example 2 (1) The prepared aluminum shell is subjected to alkaline etching. The alkaline etching solution is a 30% tromethamine solution. The alkaline etching temperature is controlled at 40°C and the time is controlled at 85s. After the alkaline etching is completed, it is stirred and washed three times with distilled water and dried at 60°C. (2) The aluminum shell treated in step (1) is pickled, and the pickling solution is selected to be 40% methanesulfonic acid, the pickling temperature is controlled at 40°C, and the time is controlled at 115s to etch larger nanopores (nanopores are about 500-600 nm); after the pickling is completed, it is stirred and washed three times with distilled water, and dried at 60°C; (3) The aluminum shell treated in step (2) is subjected to electrochemical treatment (TRI), wherein the electrochemical treatment solution is 15% acetic acid, the temperature is controlled at 55°C, the current is 1.5A, the time is controlled at 10 min, and smaller nanopores (nanopores are about 30 to 150 nm) are etched; after etching, it is quickly washed with deionized water three times with stirring, and dried at 60°C; then, it is washed with 55°C deionized water to enhance the washing effect, the time is controlled at 30s, and then transferred to an oven, the drying temperature is controlled at 80°C, and after drying, it is taken out and cooled to room temperature; (4) Injection molding material preparation: bisphenol diglycidyl ether (epoxy resin) 50kg, chitosan (liquid retaining agent) 14kg, polyethylene glycol 200 (pore-forming additive) 20kg, diaminodicyclohexylmethane (curing agent) 15kg, 4,4-thiobis(6-tert-butyl-m-cresol) (antioxidant) 6kg, octadecyl quaternary ammonium sodium (antistatic agent) 4kg, dimethylformamide (solvent) 40kg; Add epoxy resin and chitosan to dimethylformamide to carry out ring-opening condensation reaction, the reaction temperature is 65°C, and the reaction time is 9h; stir the reaction product and pore-forming additive at 65°C for 1h until they are evenly mixed, then add antioxidant and antistatic agent, continue to stir and mix evenly, finally add curing agent, stir for 15min with residual temperature, put into vacuum dryer for degassing treatment at 55°C, and obtain epoxy resin slurry; (5) Apply the epoxy resin slurry at 55±2°C in step (4) to the large surface and the bottom of the aluminum shell. The slurry thickness of the large surface of the aluminum shell is 1.5 mm, and the slurry thickness of the bottom of the aluminum shell is 5.25 mm, with a thickness ratio of 2:7. Then, dry it in an oven at a temperature of 115°C for 30 minutes. Finally, an aluminum shell with an insulating layer on the inner wall is prepared for use in aluminum shell batteries.

[0089] Example 3 (1) The prepared aluminum shell is subjected to alkaline etching, and the alkaline etching solution is selected to be a 30% tromethamine solution, the alkaline etching temperature is controlled at 70°C, and the time is controlled at 80s; after the alkaline etching is completed, it is stirred and washed three times with distilled water, and dried at 60°C; (2) The aluminum shell treated in step (1) is pickled, and the pickling solution is selected to be 40% methanesulfonic acid, the pickling temperature is controlled at 50°C, and the time is controlled at 110s to etch larger nanopores (nanopores are about 500-600nm); after the pickling is completed, it is stirred and washed three times with distilled water, and dried at 60°C; (3) The aluminum shell treated in step (2) is subjected to electrochemical treatment (TRI), wherein the electrochemical treatment solution is 15% acetic acid, the temperature is controlled at 60°C, the current is 1.5A, the time is controlled at 10 min, and smaller nanopores (nanopores are about 30 to 150 nm) are etched; after etching, it is quickly washed three times with deionized water and dried at 60°C; then, it is washed with 60°C deionized water to enhance the washing effect, the time is controlled at 25s, and then transferred to an oven, the drying temperature is controlled at 80°C, and after drying, it is taken out and cooled to room temperature; (4) Injection molding material preparation: 60 kg of bisphenol diglycidyl ether (epoxy resin), 20 kg of chitosan (liquid retaining agent), 20 kg of polyethylene glycol 200 (pore-forming additive), 20 kg of diaminodicyclohexylmethane (curing agent), 6 kg of 4,4-thiobis(6-tert-butyl-m-cresol) (antioxidant), 4 kg of sodium octadecyl quaternary ammonium (antistatic agent), and 50 kg of dimethylformamide (solvent); Add epoxy resin and chitosan to dimethylformamide to carry out ring-opening condensation reaction, the reaction temperature is 80°C, and the reaction time is 6 hours; stir the reaction product and pore-forming additive at 65°C for 1 hour until they are evenly mixed, then add antioxidant and antistatic agent, continue to stir and mix evenly, finally add curing agent, stir for 15 minutes with residual temperature, put into vacuum dryer for degassing treatment, and control the temperature at 55°C to obtain epoxy resin slurry; (5) Apply the epoxy resin slurry at 55±2°C in step (4) to the large surface and the bottom of the aluminum shell. The slurry thickness of the large surface of the aluminum shell is 2 mm, and the slurry thickness of the bottom of the aluminum shell is 7 mm, with a thickness ratio of 2:7. Then, dry it in an oven with a temperature controlled at 115°C and a drying time of 30 min. Finally, an aluminum shell with an insulating layer on the inner wall is prepared for use in aluminum shell batteries.

[0090] Example 4 The only difference between this embodiment and embodiment 1 is that chitosan is replaced by chitin.

[0091] Example 5 The only difference between this embodiment and embodiment 1 is that carboxymethyl chitosan is used to replace chitosan.

[0092] Example 6 The only difference between this embodiment and embodiment 1 is that cyclodextrin is used to replace chitosan.

[0093] Comparative Example 1 This comparative example uses a conventional aluminum shell, which contains a Mylar film (insulating film) and a bottom support sheet (bottom support plate).

[0094] Comparative Example 2 In this comparative example, chitosan was not added, and the ring-opening condensation reaction was not performed. The amount of epoxy resin was adjusted to 48 kg, and the rest was consistent with Example 1.

[0095] Battery performance test 1. Peel force test: The test was carried out using a stretching machine at room temperature. The aluminum shells of the embodiment and the comparative example were cut into aluminum sheets of the same size and subjected to a peel strength test. The sample width was 25 mm and the stretching was carried out at 180°C.

[0096] 2. Liquid retention test: Under room temperature conditions, the hollow nano-injection aluminum shell and the uninjection aluminum shell were fully welded, filled with electrolyte, inserted into the sealing pins and left still for 12 hours, and then the injection was repeated until no more electrolyte could be injected, and the electrolyte consumption was statistically compared.

[0097] 3. Cycle test At 25°C, charge the battery at 1C constant current and constant voltage to 3.65V with a cut-off condition of 0.05C; after standing for 60 minutes, discharge at 1C to 2.5V. Continue the above process until the capacity decays to 80% of the initial test capacity, and record the number of cycles.

[0098] Table 1 Parameters and results of examples and comparative examples Compared with the comparative example, the aluminum shells of Examples 1-6 have an insulating layer containing a liquid retaining agent, which greatly increases the liquid retention capacity of the insulating layer. At the same time, the aluminum shells can be prevented from being corroded, thereby increasing the cycle life of the battery cells.

[0099] Moreover, the addition of the liquid retaining agent can also improve the functionality of the epoxy resin adhesive, so that the insulating layer will not fall off spontaneously, avoiding the alloy reaction between lithium ions and the aluminum shell that causes corrosion of the shell and ensuring the integrity of the aluminum shell.

[0100] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A battery, It is characterized in that The battery comprises: A shell, wherein the inner wall of the shell has a plurality of first hole structures; The insulating layer is arranged on the inner wall surface of the shell and in the first hole structure, and the insulating layer has a pore structure; the insulating layer includes modified epoxy resin, and the modified epoxy resin is a condensation product of epoxy resin and a liquid retaining agent.

2. The battery according to claim 1, It is characterized in that The monomer of the epoxy resin includes at least one of bisphenol diglycidyl ether and polyphenol type glycidyl ether; And / or, the liquid retaining agent includes at least one of chitosan, chitin, carboxymethyl chitosan and cyclodextrin.

3. The battery according to claim 1, It is characterized in that The diameter of the first hole structure is 500-800 nm; And / or, the inner wall of the first hole structure has a plurality of second hole structures; The diameter of the second hole structure is 10-500 nm.

4. The battery according to claim 1, It is characterized in that The shell is a square shell, and the square shell includes a shell large surface, a shell side wall and a shell bottom; The thickness of the insulating layer on the inner wall surface of the shell is recorded as H 1 The thickness of the insulating layer on the inner wall surface of the bottom of the shell is recorded as H 2 , H 1 With H 2 The ratio is (2~4): (7~13).

5. The battery according to claim 1, It is characterized in that The porosity of the insulating layer is 2% to 5%.

6. A method for preparing a battery according to any one of claims 1 to 5, It is characterized in that The steps include: S1, performing alkaline etching treatment on the inner wall of the shell to obtain an alkaline-etched shell; S2, performing pickling treatment on the inner wall of the shell after the alkaline etching treatment to obtain a shell having a first hole structure; S3, subjecting the epoxy resin and the liquid retaining agent to a ring-opening condensation reaction in a solvent to obtain a reaction product including a modified epoxy resin; The reaction product including the modified epoxy resin, the pore-forming additive, the antioxidant, the antistatic agent and the curing agent are uniformly mixed, and after degassing treatment, an insulating layer slurry is obtained; The insulating layer slurry is disposed on the inner wall surface and the hole structure of the shell obtained in step S2, and after drying, a shell composited with the insulating layer is obtained; S4, assembling a battery using the composite shell with an insulating layer.

7. The preparation method according to claim 6, It is characterized in that In step S1, the reagent used for the alkaline etching treatment is an alkaline etching solution; And / or, in step S2, the reagent used for the pickling treatment is a pickling solution; And / or, between step S2 and step S3, the method further includes: electrochemically treating the inner wall of the first hole structure to etch a second hole structure; The reagent used in the electrochemical treatment is an electrochemical solution.

8. The preparation method according to claim 7, It is characterized in that The alkaline etching solution includes at least one of a tromethamine solution, a potassium hydroxide solution, a barium hydroxide solution, and a sodium carbonate solution; And / or, the pH value of the alkaline etching solution is 8 to 11; and / or, the concentration of the alkaline etching solution is 20wt% to 40wt%; And / or, the temperature of the alkali etching treatment is 30-70° C., and the time of the alkali etching treatment is 80-90 s; And / or, the pickling solution includes at least one of a methanesulfonic acid solution, a hydrochloric acid solution, and a hydrofluoric acid solution; and / or, the concentration of the pickling solution is 30wt% to 50wt%; And / or, the temperature of the pickling treatment is 30-50° C., and the time of the pickling treatment is 110-120 s; and / or, the electrochemical solution comprises at least one of acetic acid solution, carbonic acid solution, silicic acid solution, nitrous acid solution, hydrosulfuric acid solution, hypochlorous acid solution, sulfurous acid solution, hydrocyanic acid solution, and oxalic acid solution; and / or, the concentration of the electrochemical solution is 10wt% to 20wt%; And / or, the temperature of the electrochemical treatment is 50-60° C., and the time of the electrochemical treatment is 10-20 min.

9. The preparation method according to claim 6, It is characterized in that In step S3, the reaction temperature of the ring-opening condensation reaction is 50 to 80° C., and the reaction time of the ring-opening condensation reaction is 6 to 12 h; And / or, the solvent includes at least one of dimethylformamide and dichloromethane.

10. The preparation method according to claim 6, It is characterized in that The insulating layer comprises the following raw material components in parts by weight: Epoxy resin 40-60 parts 8-20 portions of liquid retaining agent Pore-forming additive 5-30 parts 2-8 parts of antioxidant Antistatic agent 0.5-5 parts 5 to 20 parts of curing agent.

Citation Information

Patent Citations

  • Cylindrical lithium ion power battery shell and manufacturing method thereof

    CN109585714A

  • Epoxy resin composite coating material, metal composite shell, preparation method of metal composite shell, battery and electric equipment

    CN116396655A

  • Protection structure and battery

    CN218731178U