Fireproof material containing fibers

By adding specific fibers and fillers to the fiber matrix, a fire-resistant composite with compressibility and mechanical strength is formed, which solves the problem of fire-resistant material collapse caused by expansion of lithium-ion batteries, and realizes the full life of lithium-ion batteries with fire-resistant performance and thermal runaway control. reduce.

CN119072522APending Publication Date: 2024-12-03UNIFRAX I LLC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380035638.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-02-24
Filing Date
2023-02-23
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Existing fire-resistant materials are brittle and collapsed during the expansion of lithium-ion batteries, and cannot effectively maintain fire-resistant performance, resulting in thermal runaway and flame propagation.

Method used

Using fiber-containing fire-resistant materials, by adding microglass fibers, low-biological persistent fibers, refractory ceramic fibers, etc. to the fiber matrix, combined with organic adhesives and inorganic fillers, a fire-resistant composite material with compressibility and mechanical strength is formed. Ensure that the material maintains low thermal conductivity and fire resistance throughout the life of the lithium-ion battery.

Benefits of technology

The material maintains fire resistance throughout the life of the lithium-ion battery, avoids collapse and thermal runaway, reduces flame propagation, and reduces the occurrence of thermal runaway through low thermal conductivity and low electrical conductivity. It is suitable for high impact applications such as electric loading Tool.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119072522A_ABST
    Figure CN119072522A_ABST
Patent Text Reader

Abstract

A fire protection material comprising at least 10% by weight of inorganic fibers, at least 5% by weight of an additive dispersed within the inorganic fibers, the additive selected from the group consisting of fibers, particles, flakes, aerogels, foams, or combinations thereof; and at least 2% by weight of a binder dispersed within the inorganic fibers. The inorganic fibers, additives, and binders comprise at least 60% by weight of the fire retardant material.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims priority to U.S. Provisional Application No. 63 / 268,434, filed on February 24, 2022, entitled “Fiber-Containing Fireproofing Material,” which is incorporated herein by reference in its entirety. Field of the Invention

[0003] The present disclosure relates to a fiber-containing composition for fire protection between cells of a lithium-ion battery. The fiber-containing fire protection material is compressible so that the fire protection performance can be maintained when the lithium-ion battery expands over time. Background Art

[0004] Lithium-ion batteries (LiB) are increasingly used in various industries, including electric vehicles (EVs), due to their high energy density and cycling characteristics. LiB batteries have known disadvantages, such as being susceptible to thermal runaway, where a fault in a single cell can propagate to surrounding cells and cause the LiB to burn.

[0005] Typically, fireproof materials are brittle and inflexible. That is, many fireproof materials will break when exposed to stresses such as shock or vibration. This is problematic in LiB applications because the LiB cell expands both during cycling and over time. Therefore, there is still a need for fireproof materials that can maintain low thermal conductivity during the life of the LiB. BRIEF DESCRIPTION OF THE DRAWINGS

[0006] Various embodiments of the present disclosure will be more fully understood from the detailed description and drawings given below. In the drawings, the same reference numerals may represent the same or functionally similar elements. The embodiments are described in detail below with reference to the drawings, in which:

[0007] FIG. 1 is a prior art fire retardant material disposed between cells of a lithium-ion battery.

[0008] Figure 2 A fiber-containing fireproof material according to one embodiment of the present disclosure.

[0009] Figure 3 A fiber-containing fireproof material according to one embodiment of the present disclosure.

[0010] Figure 4 A fiber-containing fireproof material according to one embodiment of the present disclosure is disposed between lithium-ion battery cells.

[0011] Figure 5 is a graph comparing the compressive strain measured in Example 1 and Comparative Example 1.

[0012] Figure 6is a graph comparing the compressive strain measured in Example 2 and Comparative Example 2.

[0013] Figure 7 is a graph comparing the compressive strain measured in Example 3 and Comparative Example 3.

[0014] Detailed Description

[0015] The following disclosure provides many different embodiments or examples. Specific examples of components and arrangements are described below to simplify the disclosure. Of course, these are merely examples and are not intended to be limiting. In addition, the disclosure may repeat reference numerals and / or letters in various examples. This repetition is for simplicity and clarity purposes and does not in itself represent a relationship between the various embodiments and / or configurations discussed.

[0016] 1, existing fire-resistant composite materials 12 are brittle and, when located in the gap between lithium-ion batteries 14a, 14b, can be damaged by the expansion of the batteries 14a, 14b and the subsequent closing of the gap therebetween. Such damage to the fire-resistant composite material 12 can cause the fire-resistant composite material 12 to collapse as the batteries 14a, 14b expand and contract during cycling, such that the area within the gap is no longer covered by the fire-resistant composite material 12. This is particularly true in high impact applications such as electric vehicles, as the vibration and movement of the electric vehicle will accelerate the collapse of the fire-resistant composite material 12.

[0017] According to an embodiment of the present disclosure, a fiber-containing fireproof material is provided that has sufficient compressibility and mechanical strength to maintain thermal properties from the beginning of life (BoL) to the end of life (EoL) of the LiB. As used herein, EoL is the end of the working life of a battery pack including the fireproof material, where the capacity decreases to the point where the battery pack needs to be replaced. For example, the moment may be reached after a set number of cycles (e.g., 1,000, 5,000, or 10,000 cycles), after a set number of years of operation of the battery pack (e.g., 2, 5, 8, or 10 years), after a set number of miles driven in an electric vehicle using the battery pack (e.g., 50,000 miles, 100,000 miles, 200,000 miles, or 250,000 miles), after the capacity drops below a set percentage of the peak capacity of the battery pack (e.g., 85%, 80%, 75%, 70%, 65%, 60%, 50%, 40%, or 30% of the peak capacity), or a combination of these thresholds. For example, in some embodiments, the EoL may be set to the earliest moment when the EV using the battery pack reaches 100,000 miles, 8 years, or when the battery pack drops below 70% of the peak capacity. Maintaining sufficient compressibility and mechanical strength from BoL to EoL avoids the issues regarding the above collapse, thus enabling the fireproof material to suppress thermal runaway throughout the lifetime of the LiB.

[0018] Flammability

[0019] The fireproof material of the present disclosure is fireproof and, when used in LiB, can help reduce the flame propagation between cells of LiB. In some embodiments, the fireproof material is classified as V-2, V-1, V-0, 5VB or 5VB material according to UL94. In some embodiments, the fireproof material is fireproof (i.e., does not melt) at a temperature of at least 600°C, at least 700°C, at least 800°C, at least 900°C, at least 1000°C, at least 1100°C, at least 1150°C, at least 1200°C, at least 1250°C, at least 1260°C or at least 1300°C. In some embodiments, the fireproof material is certified to be fireproof according to UL 723, ASTM E84, ASTM E136, ASTME1529 and / or UL 1709. In some embodiments, the fireproof material is rated as A2-s1, d0 or better according to EN13501-1. The fire retardant material may exhibit any one or more of the aforementioned properties at both the BoL of a battery pack including the fire retardant material and the EoL of the battery pack.

[0020] Thermal conductivity

[0021] The fireproof material of the present disclosure has low thermal conductivity, which allows the material to be as thin as possible, consuming a minimum amount of space in the LiB battery pack. This allows manufacturers to minimize the size of the pack (including multiple battery cells) and maximize the energy density of the pack. In some embodiments, the fireproof material has a thermal conductivity of at most 0.10, at most 0.08, at most 0.06, at most 0.05, at most 0.04, at most 0.035, at most 0.03, at most 0.025, at most 0.02, at most 0.015 or at most 0.01 W / m·K at 0°C, 10°C, 20°C, 30°C, 40°C, 50°C, 60°C, 70°C, 80°C, 90°C and / or 100°C (measured according to ASTM C201). In some embodiments, the fire resistant material has a thermal conductivity of at most 0.14, at most 0.12, at most 0.10, at most 0.08, at most 0.07, at most 0.05, at most 0.04, at most 0.035, at most 0.03, at most 0.025, at most 0.02, at most 0.015, or at most 0.01 W / m·K at 100° C., 200° C., 300° C., 400° C., 500° C., 600° C., 700° C., 800° C., 900° C., and / or 1000° C. The fire resistant material may exhibit any one or more of the foregoing properties at both the BoL of a battery including the fire resistant material and the EoL of the battery.

[0022] Conductivity

[0023] The fireproof material of the present disclosure has low electrical conductivity, which can reduce the occurrence of thermal runaway (which is usually caused by internal and external short circuits). Fireproof material can also maintain this performance even after thermal runaway. In some embodiments, fireproof material has at least 5kV / mm, at least 6kV / mm, at least 7kV / mm, at least 8kV / mm, 5kV / mm to 15kV / mm, 6kV / mm to 12kV / mm or 7kV / mm to 10kV / mm dielectric strength measured according to ASTM D14-method C. Fireproof material can show the aforementioned performance at both the BoL of the battery pack including the fireproof material and the EoL of the battery pack.

[0024] Compressibility

[0025] The fireproof material of the present disclosure has controlled compression performance, which allows the material to have good fire resistance, low thermal conductivity and low electrical conductivity even under compression. In some embodiments, the fireproof material maintains or improves its fire resistance, thermal conductivity and / or electrical conductivity when under compression. When the battery is installed in the LiB bag and expands over time, these controlled compression performances maintain the load, thereby limiting the damage to the fireproof material of common brittleness. In some embodiments, the fireproof material has at least 50%, at least 55%, at least 60%, at least 65%, at least 70% or at least 75% compression recovery measured according to ASTM D3574-Test C at the BoL of LiB. In some embodiments, the fireproof material has at least 5%, at least 10%, at least 15%, at least 20%, at least 25% or at least 30% compression recovery at the EoL of LiB.

[0026] The compressive strain of the fiber-containing fireproof material can be measured in the range of 1mm / min to a compression speed of up to 100mm / min (usually tested according to ASTM D3574). The material to be evaluated can be cut into a square of 50mm×50mm and compressed between two parallel plates at ambient pressure and temperature. The compression curve can be generated from the strain, which is 0% to a typical EoL value such as 80% seen in LiB. In some embodiments, the fireproof material has a compressive strain of 50kPa to 2,500kPa at 60% compression, a compressive strain of 200kPa to 4,000kPa at 70% compression, and a compressive strain of 1,000kPa to 8,000kPa at 80% compression. In some embodiments, the fireproof material has a compressive strain of at least 100kPa or at least 200kPa in the entire compression range of 20% to 50%.

[0027] Explosion-proof

[0028] Thermal runaway events in EV battery packs are not quiet or controlled events. There can be violent emissions of gases, flames, and even particle expulsion from the battery cells. Therefore, there is a need for insulating materials within the battery pack that can function as explosion protection. Such materials can be positioned, for example, between the top of the battery array and the pack cover or between individual cells of the battery pack. The material must be able to remain intact and maintain thermal insulation while withstanding high pressure flames and particles.

[0029] According to some embodiments, the fireproof material may be an explosion-proof material. Explosion-proofness generally relates to the ability of a material to withstand thermal and mechanical forces, and it may be tested, for example, by subjecting the material to a blowtorch (e.g., at about 1100° C.) and feeding alumina sand through the blowtorch. The explosion-proof material should remain intact for a predetermined time while keeping the cold face temperature below a set threshold.

[0030] refer to Figure 2 In one or more embodiments, the fire-resistant material 100 may include a fiber matrix 110 having one or more additives 120, 130 dispersed or suspended therein. The fiber matrix 110 includes fibers having an aspect ratio of at least 3. The fiber matrix 110 may be composed of a single type of fiber, or may include a combination of different types of fibers. Suitable fibers that may be included in the fiber matrix 110 include microglass fibers, low biopersistent fibers (LBP), refractory ceramic fibers (RCF), and / or polycrystalline wool (PCW).

[0031] The microglass fibers may include A-glass fibers, B-glass fibers, C-glass fibers, and / or E-glass fibers. In some embodiments, the microglass fibers have an average diameter of about 0.25 microns to 5 microns. In other embodiments, the microglass fibers have a diameter of at least about 3 microns, at least about 4 microns, at least about 5 microns, or at least about 6 microns.

[0032] LBP fibers exhibit a minimum of 30 ng / cm when exposed to simulated lung fluid at a flow rate of 0.3 ml / min at 37°C with a 0.1 g sample. 2 -hr solubility. Suitable LBP fibers include alkaline earth silicate (AES) fibers, such as those described in U.S. Pat. Nos. 8,663,774 and 8,551,897, each of which is incorporated herein by reference in its entirety. One useful LBP fiber is available under the registered trademark Commercially available from Alkegen (Tonawanda, NY). The fibers generally comprise the fiberization product of about 61 to about 67 weight percent silica, about 27 to about 33 weight percent calcia, and about 2 to about 7 weight percent magnesia.

[0033] Refractory ceramic fibers (RCF) comprise alumina and silica. In some embodiments, the RCF may comprise about 50% by weight alumina. In some embodiments, the RCF may comprise about 45 to about 60% by weight alumina and about 40 to about 55% by weight silica. In some embodiments, the RCF may comprise about 29 to about 31% by weight alumina, about 53 to about 55% by weight silica, and about 15 to about 17% by weight zirconia. In some embodiments, the RCF may have an average length of about 3 to about 6.5 mm, typically less than about 5 mm, and an average fiber diameter of about 0.5 microns to about 14 microns. A useful RCF is marketed under the registered trademark Commercially available from Unifrax I LLC (Niagara Falls, NY). The ceramic fibers comprise the fiberization product of a melt comprising from about 45 to about 75 weight percent alumina and from about 25 to about 55 weight percent silica. Ceramic fibers exhibit operating temperatures up to about 1540°C and melting points up to about 1870°C.

[0034] PCW is an aluminosilicate fiber having an alumina content greater than 70 wt. % or from about 72 to about 96 wt. %. PCW is mechanically strong and, when included, can reduce the brittleness of the fireproof material 100 (and the material loss during vibration). In some embodiments, the PCW has an average diameter of at least about 3 microns, at least about 4 microns, at least about 5 microns, or at least about 6 microns. In some embodiments, suitable PCW includes those sold under the trade name Alumina fibers are commercially available from Unifrax I LLC (Tonawanda, NY).In some embodiments, the PCW may include alumina fibers, such as those described in US Pat. Nos. 4,792,478 and 5,176,857, each of which is incorporated herein by reference in its entirety.

[0035] Other fibers that may be included in the fiber matrix 110 include silica yarns (continuous or chopped) and / or organic fibers, such as nylon fibers, polyvinyl alcohol (PVA) fibers, aramid fibers, polyester fibers, and the like. In some embodiments, the fiber matrix 110 comprises long fibers having an average length of at least about 5 mm, at least about 10 mm, at least about 25 mm, at least about 40 mm, at least about 50 mm, at least about 70 mm, or at least about 100 mm. In some embodiments, the fiber matrix comprises a woven material that can help trap additives 120, 130 within the fiber matrix 110.

[0036] In one or more embodiments, each of the aforementioned fibers may account for up to 100% by weight of the fiber matrix 110. In some embodiments, the fiber matrix 110 comprises microglass fibers or LBP fibers in an amount of at least 50% by weight, and comprises up to 50% by weight of long fibers and / or strong fibers selected from PCW, silica yarns, and / or organic fibers. In such embodiments, the strong fibers may have an average diameter of at least about 3 microns, at least about 4 microns, at least about 5 microns, or at least about 6 microns. In some embodiments, the fiber matrix 110 comprises LBP fibers as the main fibers (at least 50% by weight). In other embodiments, the fiber matrix 110 comprises microglass fibers as the main fibers due to their excellent insulating properties.

[0037] In some embodiments, the fireproof material 100 is in the form of paper having a thickness of greater than about 0.1 mm to about 10 mm, about 1 mm, about 2 mm, or about 3 mm. In some embodiments, the fireproof material 100 has a basis weight of about 40 gsm (grams / square meter) to about 3000 gsm, about 100 gsm to about 2500 gsm, about 200 gsm to about 1500 gsm, about 100 gsm, about 200 gsm, about 300 gsm, or about 400 gsm. In some embodiments, the fireproof material has a basis weight of about 50 kg / m 3 About 500kg / m 3 , about 100kg / m 3 About 350kg / m 3 , or about 100kg / m 3 About 250kg / m 3 density.

[0038] In some embodiments, the additives 120, 130 may include an organic binder that maintains the flexibility of the fire-resistant material 100 and contributes to the bond strength to hold the fire-resistant material 100 in place during normal operation of the device using the material (e.g., to withstand vibration forces in an EV LiB). In some embodiments, the additives 120, 130 actively affect one or more properties of the fire-resistant material 100. For example, in some embodiments, the additives 120, 130 may reduce the thermal conductivity of the fire-resistant material 100, increase the dielectric strength of the fire-resistant material 100, and / or increase the compressive strain of the fire-resistant material 100.

[0039] In some embodiments, the binder material comprises latex, cellulose, silicone, PVA, polyester or its combination. In some embodiments, the binder comprises organic fiber. In such embodiments, the fireproof material 100 can be hot pressed to melt organic fiber and bonding material at least in part. In some embodiments, based on the gross weight of the fireproof material 100, the binder is included with the amount of about 0.5 wt % to about 10 wt %, about 1 wt % to about 20 wt % or about 5 wt % to about 15 wt %.

[0040] In some embodiments, additives 120, 130 include microporous materials, flakes, aerogels, mica, microspheres, expanded materials, opacifiers or opacifiers, heat absorbing materials, phase change materials, or other inorganic filler materials that will be used to enhance the thermal conductivity performance of the fireproof material 100 compared to the fiber matrix 110 alone. Suitable opacifiers may include, but are not limited to, silicon carbide, graphite, TiO2, Fe2O3, and ilmenite. These opacifiers are used to block IR radiation from passing through the fireproof material 100, which becomes a larger component of heat transfer when the temperature rises. Additives 120, 130 can allow the paper thickness of the fireproof material 100 to be reduced, leaving more space for battery cells (i.e., increased energy density) or reducing the size of the entire battery pack.

[0041] The microporous material may have a diameter of at least about 100 m 2 / g, at least about 200m 2 / g or at least 300m 2 / g surface area. In some embodiments, the microporous material may have an average particle size of about 1 nm to about 500 microns, about 50 nm to about 50 microns, about 1 micron to about 5 microns. Suitable inorganic filler materials include silica materials, such as fumed silica, precipitated silica, silica gel, silica aerogel, alumina materials, zirconia materials, titanium dioxide materials or combinations thereof. The inorganic filler may have a chemically modified surface that imparts hydrophobicity. For example, the inorganic filler may have a hydrophobic agent on its surface. Suitable hydrophobic agents include, but are not limited to, the chemical formula R n SiX 4-n Organic halogenated silanes, such as methyldichlorosilane, dimethyldichlorosilane, ethyltrichlorosilane, diethyldichlorosilane, chemical formula R n Si(OR) 4-n Organic (organic oxygen) silanes, such as ethyl triethoxysilane, hexadecyl trimethoxysilane, chemical formula R n S H 4-n Organo-H-silanes such as methylsilane, dimethylsilane, trimethylsilane, ethylsilane, diethylsilane, triethylsilane and the chemical formula R n S H m X 4-(m+n)Organic-H-halosilanes and organic-H-alkoxysilanes, such as chlorodimethylsilane, chloro(ethoxy) (methyl) silane. Suitable flakes include but are not limited to coated or uncoated vermiculite, mica, clay or talc flakes. Suitable mica may include but is not limited to muscovite, phlogopite, biotite, lepidolite, glauconite, sodium mica and ferrolithium mica, and may include synthetic mica such as fluorphlogopite. Available clay flakes include but are not limited to ball clay, bentonite, smectite, hectorite, kaolinite, montmorillonite, soapstone, sepiolite, sauconite or its combination. In some embodiments, whether it is a flake form or other forms of mica can be included in the fireproof material 100 to provide improved explosion resistance. In some embodiments, the microporous material may include anisotropic materials, which have different thermal conductivity depending on their orientation. In some embodiments, the microporous material may include expansion material.

[0042] Any one or more of the aforementioned microporous materials, flakes, aerogels, mica, microspheres, intumescent materials, endothermic materials, phase change materials, or other inorganic filler materials may be included in the fire-proof material 100 in an amount of greater than 0 to about 60 wt %, about 0.1 wt % to about 50 wt %, about 5 wt % to about 30 wt %, or about 10 wt % to about 25 wt %, based on the total weight of the fire-proof material 100.

[0043] In some embodiments, the fireproof material 100 includes a compression additive, which can be included as an additive 120, 130 entrained in the fiber matrix 100, or can be included as a layer adhered to the fiber matrix 110. The compression additive may include a foam, such as an open-cell or closed-cell foam formed by polyurethane, polyethylene, ethylene propylene diene monomer (EPDM), polyethylene terephthalate (PET), silicone, etc. In some embodiments, the compression additive is paper, such as organic fiber paper (e.g., formed by nylon). In some embodiments, the compression additive is an organic fiber, such as those described above. In some embodiments, the compression additive may include acrylic latex. In some embodiments, based on the total weight of the fireproof material 100, the compression additive may be present in an amount of about 2% by weight to about 50% by weight, at least about 2% by weight, at least about 5% by weight, at least about 10% by weight, at least about 15% by weight, at least about 20% by weight, at most about 50% by weight, at most about 40% by weight, at most about 30% by weight, or at most about 25% by weight.

[0044] In one or more embodiments, fireproof material 100 can be formed by papermaking technology, and the papermaking technology includes dry laying (dry laying), batch sheet (batch sheet) process or the process using triangle former, rotary former, long wire former or cylindrical machine.In some embodiments, fireproof material 100 can be formed using dry laying technology, and without any adhesive, it can optionally include needle punching (needling) process.In such embodiments, fireproof material 100 can include long fibers with a length of at least 10mm (for example, 20-30mm), which can be continuous or discontinuous fibers.In some embodiments, fireproof material 100 is formed using wet laying process, wherein additive 120,130 includes adhesive well dispersed in fiber matrix 110, and its migration is controlled using controlled drying system such as convection oven, radio frequency (RF) and / or microwave dryer. In some embodiments, the heated drum can be used to limit migration (e.g., using alternative side heating or progressive heating) or intentionally migrate materials, so the components are selected to be optionally toward or away from adjacent batteries to maximize protection. Inorganic materials, such as those added as gel phases, can migrate and be used on the hot side of the application to provide additional protection. In some embodiments, organic materials can migrate away from the core of the material to enhance the thermal properties of low temperatures (i.e., temperatures in normal operation) and enhance the adhesion of optional backing or laminated layers. In some embodiments, the drying method can control the migration of the organic binder so that the organic binder is evenly distributed through the thickness of the fireproof material 100.

[0045] In some embodiments, the fireproof material 100 comprises about 0.1 wt % to about 50 wt % of long fibers in the fiber matrix 110 and does not comprise an organic binder material. In such embodiments, the long fibers can provide a structural framework to allow the wet-laid product to be flexible in the absence of an organic binder material. In some embodiments, the fireproof material 100 does not comprise an organic binder and is prepared using different vacuum pressures when forming a wet-laid sheet to affect the density of the resulting wet-laid sheet. In some embodiments, the fireproof material 100 has a density of at most 10 g / cm 3 , up to 7g / cm 3 , up to 5g / cm 3 , up to 4g / cm 3 , up to 2g / cm 3 , up to 1g / cm 3 , up to 0.5g / cm 3 , at least 0.025g / cm 3 , at least 0.05g / cm 3 , at least 0.1g / cm 3, at least 0.25g / cm 3 , at least 0.5g / cm 3 , at least 1g / cm 3 Or any logical combination of the above upper and lower bounds (e.g. 0.025 g / cm 3 Up to 5g / cm 3 or 0.1g / cm 3 Up to 5g / cm 3 ) density.

[0046] In some embodiments, the fireproof material 100 can be formed into a complex 3D shape rather than a flat sheet. For example, the fireproof material 100 can be molded by press molding or vacuum forming to match the shape of a battery cover, a side plate, or the spacing between batteries.

[0047] In any embodiment, fireproof material 100 can include tape backing (not shown).If battery failure, then tape backing can provide enhancement, and need some explosion resistance to help slow down the fire propagation between battery.In some embodiments, tape backing can have the thickness of about 10 microns to about 1mm, about 10 microns to about 700 microns, about 10 microns to about 400 microns, about 10 microns, about 20 microns, about 30 microns, about 40 microns, about 50 microns, about 60 microns, about 70 microns, about 80 microns, about 90 microns or about 100 microns.Can use melt or pressure-sensitive adhesive tape backing directly adhere to fireproof material 100 (paper).In some embodiments, tape backing can be the loose nonwoven fabric of organic foil (for example, those formed by polypropylene, polyethylene terephthalate, polytetrafluoroethylene, etc.) or metal foil (for example, those formed by Al, Sn, Cu, etc.).In some embodiments, tape backing can include mica to improve the explosion resistance of fireproof material 100.

[0048] In some embodiments, the fire resistant material 100 comprises, based on the total weight of the fire resistant material 100:

[0049] 10 to 95 wt%, 10 to 90 wt%, 20 to 90 wt%, 30 to 80 wt%, 40 to 70 wt%, 40 to 60 wt%, at least 20 wt%, at least 30 wt%, at least 40 wt%, at least 50 wt%, at least 60 wt%, or at least 70 wt% inorganic fibers;

[0050] In greater than 0 to 60 wt %; 0.1 to 50 wt %, 5 to 30 wt %, 10 to 25 wt %, at least 1 wt %; at least 5 wt %; at least 10 wt %, at least 20 wt %, at least 30 wt % of microporous materials, flakes, aerogels, mica, microspheres, expanded materials, opacifiers or opacifiers, heat absorbing materials, phase change materials, other inorganic filler materials or combinations thereof;

[0051] Between 0 and 50 wt%, at least 2 wt%, at least 5 wt%, about 10 wt%, at least 15 wt%, at least 20 wt%, up to 50 wt%, up to 40 wt%, up to 30 wt%, or up to 25 wt% of a compression additive; and

[0052] 1 to 20 wt%, 5 to 15 wt%, at least 2 wt%, at least 5 wt%, or at least 10 wt% of a binder (inorganic, organic, or a combination thereof).

[0053] In any embodiment, the fire resistant material 100 may include an explosion resistant coating. In some embodiments, the coating may have a thickness of at most 20 mm, at most 10 mm, at most 5 mm, 0.05 to 20 mm, 0.1 to 10 mm, or 0.1 to 5 mm.

[0054] In some embodiments, the explosion-proof coating is applied as a viscous dispersion or gel of a hydrated inorganic material and dried to form a protective surface. Examples of inorganic materials include bentonite and dispersible Al 2 O 3 (e.g., colloidal alumina). Without being bound by theory, it is believed that the surface hydroxyl groups of these materials allow for inter-particle adhesion when drying, thereby creating a hard, rigid surface coating that can withstand impacts from small particles, even when subjected to flames as hot as 1100° C. This not only leaves an intact barrier, but also protects the insulating layer of the fireproofing material 100, which impedes the propagation of thermal events.

[0055] In some embodiments, the explosion-proof coating comprises a silicone blend. The silicone blend coating allows the fireproof material 100 to remain flexible throughout the manufacturing process. In the case of thermal runaway, the silicon blend coating is immediately subjected to extreme temperatures, which will oxidize the coating and ceramicize it into a hard rigid layer that can withstand the impact from particles. In some embodiments, the silicone blend comprises a cross-linked system of polysiloxanes, such as poly (dimethylsiloxane), poly (diphenylsiloxane), poly (methylphenylsiloxane) and copolymers thereof. The silicone blend may also include at least one inorganic additive or filler. These additives and fillers may include, but are not limited to, endothermic materials (e.g., aluminum hydroxide, magnesium hydroxide, CaCO 3 ), expansion additives (e.g., expandable vermiculite, CaCO 3 ), fluxing agents (e.g., glass frit, zinc borate), reinforcing additives (e.g., glass fiber, wollastonite, mica), aerogels, or combinations thereof. Additives and fillers can help form a strong ceramicized layer when the coating is fired. For example, in a silicone blend containing a flux, the flux can cause the surface of the fibers within the silicone blend or fireproof material 100 to melt. This helps to bond the network to the oxidized silicone (SiO2 ) to form an extended rigid coating and prevent cracking. For low viscosity blends, the blended resinous silicone coating can be applied by spraying, or for low to high viscosity blends, it can be applied by roller coating equipment, knife coater or slot die coater. Silicones using room temperature vulcanization (RTV) chemistry can cure for up to 24 hours, where the cure rate is accelerated by increasing humidity, temperature or using appropriate catalysts. Low temperature vulcanization (LTV) silicones will cure at slightly elevated temperatures, which takes up to 10 hours, using peroxide free radical initiators and vinyl, acrylate or methacrylate silicone pendant functional groups. The curing temperature of LTV silicones depends on the activation temperature of the catalyst, but can also be between 30-250°C. Alternatively, ultraviolet-activated free radical initiators can be used to cure the resin via UV lamps.

[0056] Go to Figure 3 In some embodiments, the fireproof material 200 can be a laminate comprising a compression layer 220 and one or more fireproof layers 210a, 210b. In some embodiments, one or more fireproof layers 210a, 210b can be the same as the fireproof material 100 described above. In one or more embodiments, the compression layer 220 comprises the same material as the above-mentioned compression additive. The compression layer 220 can be adhered to the one or more fireproof layers 210a, 210b using a melt or pressure-sensitive adhesive. In some embodiments, any one of the compression layer 220 and the one or more fireproof layers 210a, 210b can include a backing, such as the above-mentioned backing. In some embodiments, the compression layer 220 does not include inorganic fibers. In some embodiments, the compression layer 220 consists of a compression additive.

[0057] The laminated form of the fire barrier material 200 optimizes the compressibility of the material according to the changing environment on a battery pack constructed from multiple battery cells. It is known that batteries expand during use, resulting in a reduction in gap size, which can compress and damage the fire barrier material. Some compression is required to ensure that the material remains in place (i.e., does not collapse) through vibration during use, such as in EV applications. Figure 4 As shown in FIG, when the fireproof material 200 is used between LiB cells, the expansion of the cells does not damage the fireproof material 200 due to the compression characteristics of the fireproof material 200. Although not shown, the fireproof material 100 can provide Figure 4 Similar results are shown in .

[0058] In some embodiments, the fireproof material is formed into a fireproof film. The fireproof film can be a film that can be impregnated and sprayed onto the housing of the battery pack to provide heat and electrical protection. The fireproof film is formed by fibers (such as those described for the fiber matrix 110 above) and additives (such as the above-mentioned additives 110, 120). In some embodiments, a mixer (dry or wet, low shear or high shear, etc.) can be used to prepare the fireproof film. In some embodiments, the fireproof film includes colloids and / or other inorganic adhesives and organic adhesives, such as latex and / or cellulose. In any embodiment, the fireproof film can be formed into a wet solution that dries to a surface (e.g., a surface of a battery or battery pack or another substrate).

[0059] In some embodiments, the fire barrier film can be applied to a tape backing, such as the tape backing described above. In such embodiments, the fire barrier film can be applied to the tape backing by spraying, rolling or dipping a solution of fibers and additives onto the tape backing, the solution comprising an organic binder, such as cellulose, latex and / or PVA.

[0060] In any embodiment, the fireproof material described herein can be used to selectively cover 10% to 100% of the battery contact surface, and can be directly adhered to the battery using a melt or pressure-sensitive adhesive. In some embodiments, the combination of fireproof materials described herein (fireproof materials 100, 200 and fireproof films) can be used in LiB battery packs. In such embodiments, the fireproof material can be positioned in the LiB battery pack as needed, for example, between the batteries or between the array of batteries and the cover of the housing. Example

[0061] Comparative Example 1

[0062] 32.83 g of E-glass microfibers with an average diameter of 0.6 μm were broken into 3 gallons of water and stirred vigorously until uniformly dispersed. 3.94 mL of 50% anionic acrylic dispersion (Hycar 26083, Lubrizol) was added to the slurry. Finally, 5.65 mL of 5% alum was added to the slurry. The mixture was transferred to a waterproof casting machine on top of a metal mesh screen. A vacuum was drawn from below to dewater the slurry through the metal screen. The resulting wet paper was compressed and then dried at 65°C.

[0063] The dried paper had an average thickness of 2.59 mm and a 3 Then according to ASTM C518 at 204kg / m 3 The thermal conductivity of the fireproofing medium was tested at a density of . The measured thermal conductivities are listed in Table 1 below.

[0064] Example 1

[0065] Hi-Sil ABS (PPG Industries, Inc.) is a commercial precipitated silica with an average particle size of 40 μm. 22.44 g of Hi-Sil ABS was dispersed into 3 gallons of water by vigorous stirring. 14.21 g of E-glass microfibers with an average diameter of 0.6 μm were dispersed into a mixing container and stirred until uniformly dispersed. 4.26 mL of 50% anionic acrylic dispersion (Hycar 26083, Lubrizol) was added to the slurry. Finally, 6.11 mL of 5% alum was added to the slurry. The mixture was transferred to a waterproof casting machine on top of a metal mesh screen. A vacuum was drawn from below and the slurry was dehydrated through a metal screen. The resulting wet paper was compressed and then dried at 65°C.

[0066] The dried composite paper had an average thickness of 2.11 mm and a 3 Then according to ASTM C518 at 250kg / m 3 The thermal conductivity of the fireproof medium was tested at a density of . The measured thermal conductivities are listed in Table 1.

[0067] The compressive strain of the fire retardant media of Example 1 and Comparative Example 1 was tested according to a modified version of ASTM D3574 Test C. The results are shown in Figure 5 middle.

[0068] In addition to improving thermal insulation properties, the compression properties of the battery pack fireproofing material are also enhanced by the silica additive. Although silica is a brittle, inelastic material, the addition of precipitated silica particles improves the compression behavior of the material. This is due to Figure 5 The data shown in demonstrates that the fiber / silica composite exhibits a greater elastic response under compression when compared to the material of Comparative Example 1 lacking filler.

[0069] Comparative Example 2

[0070] 92 g of Insulfrax 3010 glass fiber (Alkegen) with a fiber index of >70% was broken into 3 gallons of water and stirred vigorously until uniformly dispersed. 13 mL of 42% cationic acrylic dispersion (Ottopol K-12T, Gellner Industrial) was added to the slurry. The mixture was transferred to a waterproof casting machine on top of a metal mesh screen. A vacuum was drawn from below to dewater the slurry through the metal screen. The resulting wet paper was compressed and then dried at 65°C.

[0071] Then according to ASTM C518 at 148kg / m 3 The thermal conductivity of the fireproof medium was tested at a density of . The measured thermal conductivities are listed in Table 1.

[0072] Example 2

[0073] Hi-Sil ABS (PPG Industries, Inc.) is a commercial precipitated silica with an average particle size of 40 μm. 46 g of Hi-Sil ABS was broken into 2 gallons of water with vigorous stirring. 46 g of Insulfrax 3010 glass fiber (Alkegen) with a fiber index of >90% was broken into a mixing container and stirred until uniformly dispersed. 13 mL of 42% cationic acrylic dispersion (Ottopol K-12T, Gellner Industrial) was added to the slurry. The mixture was transferred to a waterproof casting machine on top of a metal mesh screen. A vacuum was drawn from below and the slurry was dehydrated through a metal screen. The resulting wet paper was compressed and then dried at 65°C.

[0074] The dried composite paper had an average thickness of 5 mm and a 3 Then according to ASTM C518 at 286kg / m 3 The thermal conductivity of the fireproofing medium was tested at a density of . The measured thermal conductivities are listed in Table 1 below.

[0075] The compressive strain of the fire retardant media of Example 2 and Comparative Example 2 was tested according to a modified version of ASTM D3574 Test C. The results are shown in Figure 6 middle.

[0076] In addition to improving thermal insulation properties, the compression properties of the battery pack fireproofing material are also enhanced by the silica additive. Again, although silica is a brittle, inelastic material, the addition of precipitated silica particles improves the compression behavior of the material. This is due to Figure 6 The data shown in demonstrates that the fiber / silica composite exhibits a greater elastic response under compression when compared to the material of Comparative Example 2 lacking filler.

[0077] Comparative Example 3

[0078] 40.09 g of Isofrax 4010 glass fiber (Alkegen) with a fiber index of >85% was broken into 3 gallons of water and stirred vigorously until uniformly dispersed. 4.22 mL of 50% anionic acrylic dispersion (Hycar 26083, Lubrizol) was added to the slurry. Finally, 4.22 mL of 5% alum was added to the slurry. The mixture was transferred to a waterproof casting machine on top of a metal mesh screen. A vacuum was drawn from below and the slurry was dehydrated through a metal screen. The resulting wet paper was compressed and then dried at 65°C.

[0079] The dried paper had an average thickness of 3.30 mm and a 3Then according to ASTM C518 at 334kg / m 3 The thermal conductivity of the fireproof medium was tested at a density of . The measured thermal conductivities are listed in Table 1.

[0080] Example 3

[0081] 10.12 g of silicon carbide (particle size 4-7 μm) was dispersed in 2 gallons of water by vigorous stirring. 54 g of Isofrax 4010 glass fiber (Alkegen) with a fiber index > 85% was broken into a mixing container and stirred until uniformly dispersed. 6.75 mL of 50% anionic acrylic dispersion (Hycar 26083, Lubrizol) was added to the slurry. Finally, 6.75 mL of 5% alum was added to the slurry. The mixture was transferred to a waterproof casting machine on top of a metal mesh screen. A vacuum was drawn from below and the slurry was dehydrated through a metal screen. The resulting wet paper was compressed and then dried at 65°C.

[0082] The dried composite paper had an average thickness of 3.17 mm and a 3 Then according to ASTM C518 at 314kg / m 3 The thermal conductivity of the fire protection medium was tested at a density of . The measured thermal conductivities are listed in Table 1. The improved compression behavior Figure 7 , where the fiber / silicon carbide composite material exhibits a greater elastic response under compression when compared to the material of Comparative Example 3 lacking filler.

[0083] Table 1

[0084]

[0085] As described herein, the fireproof material is a controlled compression tolerant material that exists during the life of the battery cell without affecting the thermal, electrical and fireproof properties of the material. The fireproof material described herein can be thinner than the prior art, thereby maximizing the energy density of the LiB battery pack.

Claims

1. A fireproof material comprising: at least 10% by weight of inorganic fibers; at least 5% by weight of an additive dispersed within the inorganic fibers, the additive selected from fibers, particles, flakes, aerogels, foams, or combinations thereof; and at least 2 weight percent of a binder dispersed within said inorganic fibers; The inorganic fibers, additives and binders account for at least 60% by weight of the fireproof material.

2. The fireproof material according to claim 1, wherein the inorganic fiber comprises refractory ceramic fiber (RCF), low biopersistence (LBP) fiber, alkaline earth silicate (AES) fiber, polycrystalline wool (PCW) or a combination thereof.

3. The fireproof material according to claim 1, wherein the additive comprises 5 to 60 wt% of precipitated silica.

4. The fireproof material of claim 1, wherein the binder comprises latex, cellulose, silicone, polyvinyl alcohol, organic fiber, or a combination thereof.

5. The fireproof material according to claim 4, comprising 5 to 15% by weight of the binder. 6 . The fireproof material according to claim 4 , wherein the binder comprises organic fibers which are dispersed in the inorganic fibers and are heated to bind the fireproof material.

7. The fireproof material according to claim 1, further comprising 2 to 50 wt% of a compression additive dispersed in the inorganic fiber, the compression additive being selected from polyurethane, polyethylene, ethylene propylene diene monomer (EPDM), polyethylene terephthalate (PET), silicone, acrylic latex, organic fiber or a combination thereof.

8. A fireproof product comprising The fireproof material according to claim 1; and a coating disposed on at least one surface of the fire resistant material; The coating comprises bentonite, dispersible Al2O3, cross-linkable silicone, or a combination thereof.

9. The fireproof product according to claim 8, wherein the coating comprises polysiloxane and an additive selected from aluminum hydroxide, magnesium hydroxide, CaCO3, expandable vermiculite, a flux, inorganic fiber, wollastonite, mica, aerogel or a combination thereof.

10. The fire resistant article of claim 9, wherein the coating comprises the fluxing agent and the inorganic fibers.

11. The fire resistant article of claim 9, wherein the coating is configured to ceramize at a temperature of 650°C or higher.

12. The fire resistant article of claim 9, wherein the coating comprises the cross-linkable silicone and is cured using heat or ultraviolet radiation.

13. A fireproof product comprising: A first layer of the fireproof material of claim 1; and a compression layer laminated to the first layer of fire-resistant material; wherein the compression layer comprises polyurethane, polyethylene, ethylene propylene diene monomer (EPDM), polyethylene terephthalate (PET), silicone, acrylic latex, organic fibers, or a combination thereof; and wherein the compression layer does not contain inorganic fibers.

14. The fire resistant article of claim 13 further comprising a second layer of the fire resistant material laminated to the compression layer opposite the first layer of the fire resistant material.

15. The fire resistant article of claim 13, further comprising a coating disposed on at least one surface of the first layer of fire resistant material, wherein the coating comprises bentonite, dispersible Al2O3, cross-linkable silicone, or a combination thereof.

16. The fire resistant article of claim 15, wherein the coating comprises a fluxing agent and inorganic fibers.

17. A lithium ion battery pack comprising: a housing including a cover; a plurality of batteries housed within the housing; and The fireproof material of claim 1, which is disposed between at least two of the plurality of batteries or between the plurality of batteries and the cover.

18. A lithium ion battery pack comprising: a housing including a cover; a plurality of batteries housed within the housing; and The fire-resistant product according to claim 8, which is disposed between at least two of the plurality of batteries or between the plurality of batteries and the cover.

19. A lithium ion battery pack comprising: a housing including a cover; a plurality of batteries housed within the housing; and The fire resistant product of claim 13, which is disposed between at least two of the plurality of batteries or between the plurality of batteries and the cover.