Thermoplastic composition comprising blend of polyetheretherketone and polyetherimide

By adding polyetherimide (PEI) and glass fibers to polyether ether ketone (PEEK) to form a blend, the warping problem caused by uneven direction shrinkage of PEEK molded products is solved, and the dimensional stability is improved It also reduces the amount of warpage, achieving a more efficient production process.

CN119072530APending Publication Date: 2024-12-03SHPP GLOBAL TECH BV
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202380034833.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-20
Filing Date
2023-04-11
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Polyether ether ketone (PEEK) is warping due to uneven shrinkage in different directions after molding, which is difficult to effectively solve the problem of warping in the prior art, resulting in increased production costs and reduced productivity.

Method used

Using a blend comprising about 50% to 70% by weight of PEEK, about 5% to 20% by weight of polyetherimide (PEI) and about 20% to 40% by weight of glass fiber, a blend with improved dimensional stability is formed by molding. Composition.

Benefits of technology

It significantly reduces the amount of warpage of the molded product, improves dimensional stability, and has no negative impact on the crystallization behavior and mechanical properties of PEEK.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005090613260000071
    Figure BDA0005090613260000071
  • Figure BDA0005090613260000081
    Figure BDA0005090613260000081
  • Figure HDA0005090613270000011
    Figure HDA0005090613270000011
Patent Text Reader

Abstract

A thermoplastic composition includes: from about 50 wt% to about 70 wt% of a PEEK (polyetheretherketone) component; from about 5 wt% to about 20 wt% of a PEI (polyetherimide) component; and from about 20 wt% to about 40 wt% of a glass fiber component. The combined weight percentage value of all components does not exceed 100 wt%, and all weight percentage values are based on the total weight of the composition. A method of forming a molded article including the thermoplastic composition is described.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to glass-filled thermoplastic compositions including blends of polyetheretherketone (PEEK) and polyetherimide (PEI) having good dimensional stability and mechanical properties. Background Art

[0002] Polyetheretherketone (PEEK) is a high temperature semi-crystalline polymer that exhibits a very high degree of part shrinkage after cooling from the mold. PEEK can be blended with high aspect ratio fillers such as glass fibers; this significantly reduces shrinkage in the flow direction, but the degree of shrinkage of the molded product in the cross-flow (x-flow) direction is still much higher than in the flow direction. This differential shrinkage causes the molded part to warp due to uneven shrinkage in different directions. In order to solve this warping problem, post-molding operations (secondary operations) can be applied to the product to improve its flatness. If this is unsuccessful, the product needs to be discarded, reducing yield and productivity and increasing production costs.

[0003] These and other disadvantages are addressed by aspects of the present disclosure. Summary of the invention

[0004] The present disclosure describes compositions comprising blends of PEEK and polyetherimide (PEI). It has been found that compositions comprising blends of PEEK and PEI have improved dimensional stability and lower part warpage compared to compositions comprising only PEEK. In addition, it has no negative impact on PEEK crystallization behavior or mechanical properties.

[0005] Aspects of the present disclosure relate to a thermoplastic composition comprising: about 50 wt% to about 70 wt% of a PEEK (polyetheretherketone) component; about 5 wt% to about 20 wt% of a PEI (polyetherimide) component; and about 20 wt% to about 40 wt% of a glass fiber component. The combined weight percentage values ​​of all components do not exceed 100 wt%, and all weight percentage values ​​are based on the total weight of the composition.

[0006] A further aspect of the present disclosure relates to a method of forming a molded article, comprising: combining (a) about 50 wt % to about 70 wt % of a PEEK (polyetheretherketone) component, (b) about 5 wt % to about 20 wt % of a PEI (polyetherimide) component, and (c) about 20 wt % to about 40 wt % of a glass fiber component to form a mixture; and molding the mixture to form a molded article. The combined weight percentage values ​​of all components do not exceed 100 wt %, and all weight percentage values ​​are based on the total weight of the article. BRIEF DESCRIPTION OF THE DRAWINGS

[0007] In the accompanying drawings (which are not necessarily drawn to scale), like numbers may describe similar components in different views. Like numbers with different letter suffixes may represent different instances of similar components. The drawings illustrate various aspects discussed in this document generally by way of example and not by way of limitation.

[0008] Figure 1 is an example of an exemplary injection molded part showing the four corners used to determine and calculate total part warpage. DETAILED DESCRIPTION

[0009] Before the present compounds, compositions, articles, systems, devices and / or methods are disclosed and described, it should be understood that they are not limited to specific synthetic methods unless otherwise specified, or specific reagents unless otherwise specified, as these may of course vary. It should also be understood that the terminology used herein is for the purpose of describing particular aspects only, and is not intended to be limiting.

[0010] The present disclosure encompasses various combinations of elements of the present disclosure, for example, combinations of elements from dependent claims that depend on the same independent claim.

[0011] Furthermore, it should be understood that unless otherwise expressly stated, it is not intended in any way that any method described herein be interpreted as requiring that its steps be performed in a specific order. Therefore, if a method claim does not actually limit the order in which its steps are to be followed, or if the claim or description does not otherwise specifically state that the steps are to be limited to a specific order, then no order is intended to be inferred in any way in any respect. This applies to any possible non-express basis for interpretation, including: logical issues regarding the arrangement of steps or operational flows; ordinary meaning derived from grammatical organization or punctuation; and the number or type of aspects described in the specification.

[0012] All publications mentioned herein are incorporated herein by reference to disclose and describe the methods and / or materials in connection with which the publications are cited.

[0013] definition

[0014] It should also be understood that the terms used herein are used to describe specific aspects only and are not intended to be limiting. As used in the specification and claims, the term "comprising" may include aspects of "consisting of" and "consisting essentially of". Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which the present disclosure belongs. Throughout this specification and the appended claims, reference will be made to a number of terms that will be defined herein.

[0015] As used in the specification and the appended claims, the singular forms "a," "an," and "the" include plural referents unless the context clearly dictates otherwise. Thus, for example, reference to "a glass fiber component" includes a mixture of two or more glass fibers.

[0016] As used herein, the term "combination" is inclusive of blends, mixtures, alloys, reaction products, and the like.

[0017] Range can be expressed as from a value (first value) to another value (second value) in this article. When expressing such a range, the range includes one or both of the first value and the second value in some aspects. Similarly, when a value is expressed as an approximation by using the antecedent "about", it will be understood that the specific value constitutes another aspect. It will be further understood that the endpoints of each range are meaningful relative to the other endpoint and independently of the other endpoint. It should also be understood that multiple values ​​are disclosed herein, and in addition to the value itself, each value is also disclosed as "about" this specific value in this article. For example, if the value "10" is disclosed, "about 10" is also disclosed. It should also be understood that each unit between two specific units is also disclosed. For example, if 10 and 15 are disclosed, 11, 12, 13 and 14 are also disclosed.

[0018] As used herein, the terms "about" and "at or about" mean that the amount or value may be the specified value, approximate the specified value, or approximately equal to the specified value. It is generally understood that as used herein, it is the nominal value shown ± 10% variation, unless otherwise specified or derived. The term is intended to convey that similar values ​​contribute to the equivalent results or effects recorded in the claims. That is, it should be understood that the content, size, formula, parameters, and other quantities and features are not and need not be precise, but may be approximate and / or larger or smaller as needed, reflecting tolerances, conversion factors, rounding, measurement errors, etc., and other factors known to those skilled in the art. In general, the content, size, formula, parameter, or other quantity or feature is "approximately" or "approximately", whether or not it is explicitly stated as such. It should be understood that when "about" is used before a quantitative value, the parameter also includes the specific quantitative value itself, unless otherwise specifically stated.

[0019] Disclosed are components for preparing the compositions of the present disclosure and compositions themselves for the methods disclosed herein. These and other materials are disclosed herein, and it should be understood that when the combinations, subsets, interactions, groupings, etc. of these materials are disclosed, and the specific mention of the individual and collective combinations and arrangements of these compounds cannot be clearly disclosed, each is specifically considered and described herein. For example, if a specific compound is disclosed and discussed and the various modifications that can be made to various molecules including the compound are discussed, each combination and arrangement of the compound and possible modifications are specifically considered, unless there is a clear contrary description. Therefore, if a class of molecules A, B and C are disclosed and a class of molecules D, E and F and a combined molecule example AD are disclosed, each is also considered individually and collectively, even if each is not narrated separately, meaning that combinations AE, AF, BD, BE, BF, CD, CE and CF are considered to be disclosed. Similarly, any subset or combination of these is also disclosed. Therefore, for example, it is considered that subgroups AE, BF and CE are disclosed. This concept applies to all aspects of the application, including but not limited to steps in the method for preparing and using the disclosed compositions. Thus, if there are a variety of additional steps that can be performed it should be understood that each of these additional steps can be performed with any specific aspect or combination of aspects of the methods of the present disclosure.

[0020] References to parts by weight of a particular element or component in a composition or article in the specification and the appended claims represent the weight relationship between the element or component and any other elements or components in the composition or article in which the parts are expressed. Thus, in a compound comprising 2 parts by weight of component X and 5 parts by weight of component Y, X and Y are present in a weight ratio of 2:5, and are present in this ratio regardless of whether additional components are contained in the compound.

[0021] Unless expressly stated otherwise, the weight percentage of a component is based on the total weight of the formulation or composition in which the component is included.

[0022] As used herein, the terms "weight percent," "wt%," and "wt. %," which are used interchangeably, refer to the weight percent of a given component based on the total weight of the composition, unless otherwise specified. That is, all wt% values ​​are based on the total weight of the composition, unless otherwise specified. It should be understood that the sum of the wt% values ​​of all components in a disclosed composition or formulation equals 100.

[0023] Unless otherwise indicated herein to the contrary, all test standards are the most recent standards in effect at the time this application was submitted.

[0024] Each of the materials disclosed herein is commercially available and / or its preparation methods are known to those skilled in the art.

[0025] It is understood that the compositions disclosed herein have certain functions. Certain structural requirements are disclosed herein to perform the disclosed functions, and it is understood that there are multiple structures that can perform the same functions associated with the disclosed structures, and these structures generally achieve the same results.

[0026] Thermoplastic composition

[0027] Aspects of the present disclosure relate to a thermoplastic composition comprising: about 50 wt% to about 70 wt% of a PEEK (polyetheretherketone) component; about 5 wt% to about 20 wt% of a PEI (polyetherimide) component; and about 20 wt% to about 40 wt% of a glass fiber component. The combined weight percentage values ​​of all components do not exceed 100 wt%, and all weight percentage values ​​are based on the total weight of the composition.

[0028] In some aspects, the composition includes about 55wt% to about 65wt% of a PEEK component, about 5wt% to about 15wt% of a PEI component, and about 25wt% to about 35wt% of a glass fiber component. In a specific aspect, the composition includes about 58wt% to about 60wt% of a PEEK component, about 10wt% of a PEI component, and about 30wt% to about 32wt% of a glass fiber component.

[0029] In some aspects, the PEEK component includes, but is not limited to, a high flow grade of polyetheretherketone.In one aspect, the PEEK component has a melt viscosity of 120 to 180 Pascal-seconds (Pa-s) at 400°C as determined according to ISO 11443.

[0030] Exemplary PEIs include, but are not limited to, ULTEM available from SABIC TM .

[0031] The glass fibers may include, but are not limited to, chopped glass fibers, flat glass fibers, or a combination thereof. In certain aspects, the glass fiber component includes glass fibers having a length of about 3 millimeters (mm).

[0032] Articles formed from thermoplastic compositions according to aspects of the present disclosure have improved shrinkage properties compared to conventional compositions that do not include a PEI component. In some aspects, a rectangular sample of the composition, injection molded into a mold having a length of 8 in (inches), a width of 6 in (inches) and a thickness of 3.2 mm (millimeters), exhibits a shrinkage of less than 0.5% in length and less than 0.5% in width at 23°C. In certain aspects, the rectangular sample exhibits a shrinkage of less than 0.45% in length and less than 0.45% in width. In further aspects, the rectangular sample exhibits a shrinkage of about 0.35% in length and about 0.4% in width.

[0033] In specific aspects, the rectangular sample exhibits a total warpage of less than 1.0 mm, wherein the total warpage is determined by measuring the warpage at each of the 4 corners of the rectangular sample and adding the warpage at the 4 corners to determine the total warpage. In specific aspects, the rectangular sample exhibits a total warpage of less than 0.9 mm, or less than 0.8 mm, or less than 0.7 mm, or less than 0.6 mm, or less than 0.5 mm, or less than 0.4 mm, or less than 0.3 mm, or less than 0.2 mm, or less than 0.1 mm, or 0.0 mm warpage, or substantially no warpage.

[0034] In some aspects, the rectangular sample presents a total warpage amount less than at least 50% compared to a comparative sample not including a PEI component, wherein the total warpage amount is determined by measuring the warpage amount at each of the 4 corners of the rectangular sample and adding the warpage amount at the 4 corners to determine the total warpage amount. In a further aspect, the rectangular sample presents a warpage amount less than at least 55% compared to a comparative sample not including a PEI component, or a warpage amount less than at least 60%, or a warpage amount less than at least 65%, or a warpage amount less than at least 70%, or a warpage amount less than at least 75%, or a warpage amount less than at least 80%, or a warpage amount less than at least 85%, or a warpage amount less than at least 90%, or a warpage amount less than at least 95%, or a warpage amount less than at least 99%. As described herein, a comparative sample not including a PEI component includes all components of the example composition and the same content of the example composition, except that the PEI component is replaced by an equal amount of other polymer resins (e.g., a PEEK component) in the composition.

[0035] Manufacturing method

[0036] One or any of the foregoing components described herein may be dry blended with each other or with any combination of the foregoing components prior to being fed into the extruder from one or more feeders or individually from one or more feeders. The fillers employed in the present invention may also be processed into a masterbatch prior to being fed into the extruder. The components may be fed into the extruder from a throat hopper or any side feeder.

[0037] The extruder used in the present disclosure can have a single screw, multiple screws, intermeshing co-rotating or counter-rotating screws, non-intermeshing co-rotating or counter-rotating screws, reciprocating screws, pinned screws, screen screws, pinned barrels, rollers, plungers, helical rotors, co-kneaders, disc-pack processors, various other types of extrusion equipment, or a combination comprising at least one of the foregoing.

[0038] The components may also be mixed together and then melt blended to form the thermoplastic composition. Melt blending of the components involves the use of shear forces, extensional forces, compressive forces, ultrasonic energy, electromagnetic energy, thermal energy, or a combination comprising at least one of the foregoing forces or energy forms.

[0039] The barrel temperature of the extruder during compounding can be set at a temperature at which at least a portion of the polymer reaches greater than or equal to about the melting temperature if the resin is a semicrystalline organic polymer, or the flow point (e.g., glass transition temperature) if the resin is an amorphous resin.

[0040] If desired, the mixture comprising the aforementioned components can be subjected to multiple blending and forming steps. For example, the thermoplastic composition can be first extruded and formed into pellets. The pellets can then be fed into a molding machine where they can be formed into any desired shape or product. Alternatively, the thermoplastic composition from a single melt blender can be formed into sheets or strands and subjected to post-extrusion processes such as annealing, uniaxial or biaxial orientation.

[0041] The melt temperature in this process can be kept as low as possible in some aspects to avoid excessive thermal degradation of the components. In some aspects, the melt temperature is maintained between about 230°C and about 350°C, although higher temperatures can be used - provided that the residence time of the resin in the processing equipment is kept relatively short. In some aspects, the melt-processed composition leaves the processing equipment such as an extruder through a small exit hole in the die. The resulting molten resin strands can be cooled - by passing the strands through a water bath. The cooled strands can be cut into pellets for packaging and further processing.

[0042] In some aspects, a method of forming a molded article comprises: combining (a) about 50 wt % to about 70 wt % of a PEEK (polyetheretherketone) component, (b) about 5 wt % to about 20 wt % of a PEI (polyetherimide) component, and (c) about 20 wt % to about 40 wt % of a glass fiber component to form a mixture; and molding the mixture to form a molded article. The combined weight percentage values ​​of all components do not exceed 100 wt %, and all weight percentage values ​​are based on the total weight of the article.

[0043] In specific aspects, molding includes injection molding, extrusion, rotational molding, blow molding, thermoforming, or a combination thereof.

[0044] Products

[0045] In certain aspects, the present disclosure relates to shaped, formed or molded articles comprising thermoplastic compositions. Thermoplastic compositions can be molded into useful shaped articles by a variety of means, such as injection molding, extrusion, rotational molding, blow molding and thermoforming to form articles and structural parts, such as articles and structural parts of personal or commercial electronic devices, including but not limited to cellular phones, tablet computers, personal computers, notebook and portable computers and other such devices, medical applications, RFID applications, automotive applications, etc. In specific aspects, the article is a compressor plate, a housing for a telecommunication device, a bracket for an automotive sensor, or any article requiring a polymer-based material with good dimensional stability and mechanical properties.

[0046] In a further aspect, the article is extrusion molded.In a still further aspect, the article is injection molded.

[0047] The present disclosure encompasses various combinations of elements of the present disclosure, for example, combinations of elements from dependent claims that depend on the same independent claim.

[0048] Aspects of the Disclosure

[0049] In various aspects, the present disclosure relates to and includes at least the following aspects.

[0050] Aspect 1. A thermoplastic composition comprising, consisting of, or consisting essentially of:

[0051] about 50 wt % to about 70 wt % of a PEEK (polyetheretherketone) component;

[0052] about 5 wt % to about 20 wt % of a PEI (polyetherimide) component; and

[0053] about 20 wt % to about 40 wt % of a glass fiber component,

[0054] The combined weight percentage values ​​of all components do not exceed 100 wt %, and all weight percentage values ​​are based on the total weight of the composition.

[0055] Aspect 2. The thermoplastic composition according to aspect 1, wherein the composition comprises about 55 wt % to about 65 wt % of a PEEK component, about 5 wt % to about 15 wt % of a PEI component, and about 25 wt % to about 35 wt % of a glass fiber component.

[0056] Aspect 3. The thermoplastic composition according to aspect 1 or 2, wherein the composition comprises about 58 wt% to about 60 wt% of a PEEK component, about 10 wt% of a PEI component, and about 30 wt% to about 32 wt% of a glass fiber component.

[0057] Aspect 4. The thermoplastic composition according to any one of aspects 1 to 3, wherein the glass fiber component comprises chopped glass fibers, flat glass fibers, or a combination thereof.

[0058] Aspect 5. The thermoplastic composition according to aspect 4, wherein the glass fiber component comprises glass fibers having a length of about 3 mm (millimeter).

[0059] Aspect 6. The thermoplastic composition according to any one of aspects 1 to 5, wherein the PEEK component has a melt viscosity of 120 to 180 Pascal-seconds (Pa-s) at 400°C as determined according to ISO 11443.

[0060] Aspect 7. A thermoplastic composition according to any one of Aspects 1 to 6, wherein a rectangular sample of the composition injection molded into a mold having a length of 8 in (inches), a width of 6 in and a thickness of 3.2 mm (millimeters) exhibits a shrinkage of less than 0.5% in length and less than 0.5% in width at 23°C.

[0061] Aspect 8. The thermoplastic composition according to aspect 7, wherein the rectangular sample exhibits a shrinkage of less than 0.45% in length and less than 0.45% in width.

[0062] Aspect 9. The thermoplastic composition of aspect 7, wherein the rectangular sample exhibits a shrinkage of about 0.35% in length and about 0.4% in width.

[0063] Aspect 10. The thermoplastic composition according to any one of aspects 7 to 9, wherein the rectangular sample exhibits a total warpage of less than 1.0 mm, wherein the total warpage is determined by measuring the warpage at each of the four corners of the rectangular sample and adding the warpage at the four corners.

[0064] Aspect 11. A thermoplastic composition according to any one of Aspects 7 to 10, wherein the rectangular sample exhibits at least 50% less total warpage than a comparative sample not including a PEI component, wherein the total warpage is determined by measuring the warpage at each of the four corners of the rectangular sample and adding the warpage at the four corners.

[0065] Aspect 12. A method of forming a molded article comprising, consisting of, or consisting essentially of:

[0066] combining (a) about 50 wt % to about 70 wt % of a PEEK (polyetheretherketone) component, (b) about 5 wt % to about 20 wt % of a PEI (polyetherimide) component, and (c) about 20 wt % to about 40 wt % of a glass fiber component to form a mixture; and

[0067] molding the mixture to form a molded article,

[0068] The combined weight percentage values ​​of all components do not exceed 100 wt %, and all weight percentage values ​​are based on the total weight of the product.

[0069] Aspect 13. The method according to aspect 12, wherein molding comprises injection molding, extrusion, rotational molding, blow molding, thermoforming, or a combination thereof.

[0070] Aspect 14. The method according to aspect 12 or 13, wherein the article comprises about 55 wt% to about 65 wt% of a PEEK component, about 5 wt% to about 15 wt% of a PEI component, and about 25 wt% to about 35 wt% of a glass fiber component.

[0071] Aspect 15. The method according to any one of aspects 12 to 14, wherein the article comprises about 58 wt% to about 60 wt% of a PEEK component, about 10 wt% of a PEI component, and about 30 wt% to about 32 wt% of a glass fiber component.

[0072] Aspect 16. The method according to any one of aspects 12 to 15, wherein the glass fiber component comprises chopped glass fibers, flat glass fibers, or a combination thereof.

[0073] Aspect 17. The method of aspect 16, wherein the glass fiber component comprises glass fibers having a length of about 3 mm (millimeter).

[0074] Aspect 18. The method according to any one of aspects 12 to 17, wherein the PEEK component has a melt viscosity of 120 to 180 Pascal-seconds (Pa-s) at 400°C, determined according to ISO 11443.

[0075] Aspect 19. The method according to any one of aspects 12 to 17, wherein a rectangular sample of the composition injection molded into a mold having a length of 8 in (inches), a width of 6 in and a thickness of 3.2 mm (millimeters) exhibits a shrinkage of less than 0.5% in length and less than 0.5% in width at 23°C.

[0076] Aspect 20. The method of aspect 19, wherein the rectangular sample exhibits a shrinkage of less than 0.45% in length and less than 0.45% in width.

[0077] Aspect 21. The method of aspect 19, wherein the rectangular sample has a shrinkage of about 0.35% in length and about 0.4% in width.

[0078] Aspect 22. The method according to any one of Aspects 19 to 21, wherein the rectangular sample exhibits a total warpage of less than 1.0 mm, wherein the total warpage is determined by measuring the warpage at each of the four corners of the rectangular sample and adding the warpage at the four corners.

[0079] Aspect 23. A method according to any one of Aspects 19 to 22, wherein the rectangular sample exhibits at least 50% less total warpage than a comparative sample not including a PEI component, wherein the total warpage is determined by measuring the warpage at each of the four corners of the rectangular sample and adding the warpage at the four corners.

[0080] Aspect 24. An article comprising the thermoplastic composition according to any one of aspects 1 to 10, wherein the article is a compressor plate, a housing for a telecommunication device, or a bracket for an automotive sensor.

[0081] Example

[0082] The following examples are presented to provide a person of ordinary skill in the art with a complete disclosure and description of how to make and evaluate the compounds, compositions, articles, devices and / or methods claimed herein, and are intended to be purely exemplary and are not intended to limit the present disclosure. Every effort has been made to ensure the accuracy of the values ​​(e.g., amounts, temperatures, etc.), but some errors and deviations should be considered. Unless otherwise stated, parts are parts by weight, temperatures are in ° C or ambient temperature, and pressures are at or near atmospheric pressure. Unless otherwise stated, percentages related to compositions are wt%.

[0083] There are many variations and combinations of reaction conditions (e.g., component concentrations, desired solvents, solvent mixtures, temperature, pressure, and other reaction ranges and conditions) that can be used to optimize the product purity and yield obtained by the process. Such process conditions can be optimized with only reasonable and routine experimentation.

[0084] Compositions were formed and various properties were tested as shown in Table 1:

[0085] Table 1 - Composition and properties

[0086]

[0087]

[0088] The following units are abbreviated in Table 1: Celsius (°C); Megapascal (MPa); Joule / meter (J / m); Micrometer / meter-°C (pm / m-°C); Joule / gram (J / g); Gigapascal (GPa).

[0089] The specific gravity is determined according to ASTM D792. The heat deformation temperature (HDT) is determined according to ASTM D648 at 0.45 megapascals (MPa). The tensile properties (modulus, strength and elongation at break) are determined according to ASTM D638. The flexural properties (modulus and strength) are determined according to ASTM D790. The unnotched Izod impact strength (UNII) is determined according to ASTM D4812 at room temperature (23°C). The notched Izod impact strength (NII) is determined according to ASTM D256 at room temperature. The coefficient of thermal expansion (CTE) is determined according to ASTM E831 in the flow and cross flow (x flow) directions. The crystallization properties (crystallization temperature Tc (onset and peak), enthalpy change (ΔH), crystallinity, melting temperature Tm (peak) and glass transition temperature Tg) are determined by differential scanning calorimetry (DSC) and the SABIC method. The SABIC method uses DSC to study the behavior of materials under heating and cooling cycles. Pelletized samples of the thermoplastic composition were placed in an aluminum pan and the endothermic and exothermic behavior was recorded under DSC heating at a rate of 20°C / min from room temperature to 400°C and then cooling at a rate of 20°C / min to room temperature. Shear strength was determined in accordance with ASTM D732. Compressive properties (strength in flow and x-flow (direction), modulus in flow and x-flow (direction)) were determined in accordance with ASTM D695.

[0090] Composition C1 is a 70:30 blend of PEEK-glass fiber (GF1); Composition C2 is a 70:30 blend of PEEK-glass fiber (GF2); Composition C3 is a 60:10:30 blend of PEEK, ULTEM, and glass fiber (GF2). Both GF1 and GF2 are flat glass fibers available from Nittobo. PEEK is a conventional high flow grade of polyetheretherketone. PEI is ULTEM from SABIC TM .

[0091] From the results in Table 1, it is observed that the three different blends have similar physical and mechanical properties. Blending amorphous (PEI) and crystalline (PEEK) polymers results in changes in crystallization behavior, including slower crystallization rates and lower crystallinity. In some cases, the addition of an amorphous polymer completely disrupts the crystallization formation of the other phases, which can negatively affect chemical resistance and long-term creep properties. Referring to the DSC cooling data, it can be seen that the three blends begin to crystallize at similar temperatures (around 295°C) and reach a peak at about 290°C. In addition, the crystallinity of each composition is comparable (slightly over 23%). From this data, it can be concluded that the three compositions have very similar crystallization behaviors (rates and crystallinity). One observable difference is that the Tg of the composition containing PEI increases by about 10°C.

[0092] Shrinkage and warpage were evaluated by injection molding the compositions into a mold that was 8 inches long, 6 inches wide, and 3.2 mm (millimeter) thick. The shrinkage of the molded parts was evaluated at room temperature (23°C) by measuring the length and width of the molded parts and comparing them to the tool dimensions (8" (inches or in) x 6"). The shrinkage of composition C3 was the lowest in both the width and height directions. Refer to Table 2 and Figure 1 The warpage of each corner of the panel is measured, and the total warpage is the sum of the four warpage numbers. The reduction in warpage observed in composition C3 is significant even in small and simple panel parts. The total warpage of composition C3 is only 0.65 mm, which is about one-third of the warpage of composition C1 and about one-fifth of the warpage of composition C2.

[0093] Table 2 - Shrinkage and Warpage Properties

[0094] C1 C2 C3 Width(in) 5.970 5.970 5.976 Height(in) 7.968 7.960 7.972 Width shrinkage (%) 0.50 0.50 0.40 Height shrinkage (%) 0.40 0.50 0.35 ①Warp amount (mm) 0.92 1.71 0.06 ②Warp amount (mm) 0.05 0.08 0.25 ③Warp amount (mm) 0.86 1.71 0.13 ④Warp amount (mm) 0.08 0.07 0.21 Total warpage (mm) 1.91 3.57 0.65

[0095] The above description is intended to be exemplary, not restrictive. For example, the above examples (or one or more aspects thereof) can be used in combination with each other. Other aspects may be adopted, such as by a person of ordinary skill in the art after reading the above description. The abstract is provided to comply with the provisions of 37C.FR§1.72(b) so that the reader can quickly determine the nature of the present technology disclosure. It is submitted and understood that it will not be used to interpret or limit the scope or meaning of the claims. In addition, in the above detailed description, various features can be grouped together to simplify the disclosure. This should not be interpreted as an intention that the disclosed features that are not limited by the claims are necessary for any claim. Instead, the subject matter of the invention may be present in less than all the features of the specific disclosure aspects. Therefore, the attached claims are hereby incorporated into the detailed description as examples or aspects, wherein each claim itself is a separate aspect, and it is considered that such aspects can be combined with each other in various combinations or arrangements. The scope of the present disclosure should be determined with reference to the attached claims and the equivalent form of the full range enjoyed by such claims.

Claims

1. A thermoplastic composition comprising: about 50 wt % to about 70 wt % of a PEEK (polyetheretherketone) component; about 5 wt % to about 20 wt % of a PEI (polyetherimide) component; and about 20 wt % to about 40 wt % of a glass fiber component, The combined weight percentage values ​​of all components do not exceed 100 wt %, and all weight percentage values ​​are based on the total weight of the composition.

2. The thermoplastic composition of claim 1, wherein the composition comprises about 55 wt% to about 65 wt% of the PEEK component, about 5 wt% to about 15 wt% of the PEI component, and about 25 wt% to about 35 wt% of the glass fiber component.

3. The thermoplastic composition of claim 1 or 2, wherein the composition comprises about 58 wt% to about 60 wt% of the PEEK component, about 10 wt% of the PEI component, and about 30 wt% to about 32 wt% of the glass fiber component.

4. The thermoplastic composition of any one of claims 1 to 3, wherein the glass fiber component comprises chopped glass fibers, flat glass fibers, or a combination thereof.

5. The thermoplastic composition of claim 4, wherein the glass fiber component comprises glass fibers having a length of about 3 mm (millimeter).

6. The thermoplastic composition according to any one of claims 1 to 5, wherein the PEEK component has a melt viscosity of 120 to 180 Pascal-seconds (Pa-s) at 400°C determined according to ISO 11443.

7. The thermoplastic composition of any one of claims 1 to 6, wherein a rectangular sample of the composition injection molded into a mold having a length of 8 in (inches), a width of 6 in and a thickness of 3.2 mm (millimeters) exhibits a shrinkage of less than 0.5% in length and less than 0.5% in width at 23°C.

8. The thermoplastic composition of claim 7, wherein the rectangular sample exhibits a shrinkage of less than 0.45% in length and less than 0.45% in width.

9. The thermoplastic composition of claim 7, wherein the rectangular sample exhibits a shrinkage of about 0.35% in length and about 0.4% in width.

10. The thermoplastic composition according to any one of claims 7 to 9, wherein the rectangular sample exhibits a total warpage of less than 1.0 mm, wherein the total warpage is determined by measuring the warpage at each of the four corners of the rectangular sample and adding the warpage at the four corners.

11. The thermoplastic composition of any one of claims 7 to 10, wherein the rectangular sample exhibits at least 50% less total warpage than a comparative sample not including the PEI component, wherein the total warpage is determined by measuring the warpage at each of the four corners of the rectangular sample and adding the warpage at the four corners.

12. A method of forming a molded article, comprising: combining (a) about 50 wt % to about 70 wt % of a PEEK (polyetheretherketone) component, (b) about 5 wt % to about 20 wt % of a PEI (polyetherimide) component, and (c) about 20 wt % to about 40 wt % of a glass fiber component to form a mixture; and molding the mixture to form the molded article, The combined weight percentage value of all components does not exceed 100 wt %, and all weight percentage values ​​are based on the total weight of the article.

13. The method of claim 12, wherein the molding comprises injection molding, extrusion, rotational molding, blow molding, thermoforming, or a combination thereof.

14. The method of claim 12 or 13, wherein the article comprises about 55 wt% to about 65 wt% of the PEEK component, about 5 wt% to about 15 wt% of the PEI component, and about 25 wt% to about 35 wt% of the glass fiber component.

15. An article comprising the thermoplastic composition according to any one of claims 1 to 11, wherein the article is a compressor plate, a housing for a telecommunication device or a bracket for an automotive sensor.

Citation Information

Patent Citations

  • Resin composition used for metal bonding, resin composition-metal bonded finished product, and manufacturing method

    CN108250668A

  • Polyether-ether-ketone based transformer skeleton and preparation method thereof

    CN109517332A

  • Fiber reinforced polyaryletherketone resin compositions

    US20150087767A1

  • Polyimide resin composition

    US5580918A

  • Improved poly aryl ether ketone polymer blends

    WO2007035402A2