Method for reducing surface defects in active thin film layer
By depositing aluminum nitride and molybdenum layers at high temperatures and deposition of scandium-doped aluminum nitride layers at low temperatures, the surface defects of the film layer in traditional processes are solved, the performance and crystallinity of the film layer are improved, and the high-performance film is satisfied. Industrial requirements.
Patent Information
- Application Number
- CN202280094706.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2022-04-21
- Publication Date
- 2024-12-03
AI Technical Summary
When traditional processes form scandium-doped aluminum nitride film layers, surface conical defects often occur, resulting in degradation of device and system performance.
The first crystal layer of aluminum nitride is deposited at a temperature of 350 degrees Celsius to 700 degrees Celsius, with a molybdenum layer in the middle, and then a scandium-doped aluminum nitride piezoelectric thin film layer is deposited at a temperature of less than 200 degrees Celsius, by controlling the deposition process Vacuum damage and film layer thickness to reduce surface defects.
The crystallinity and surface quality of scandium-doped aluminum nitride film layer is significantly improved, the surface conical defect count is reduced, and the requirements for high-performance films for MEMS and other applications are met.
Smart Images

Figure CN119073024A_ABST
Abstract
Description
[0001] field
[0002] Embodiments of the present principles generally relate to semiconductor processing of semiconductor substrates.
[0003] background
[0004] Piezoelectric devices and micro-electromechanical systems (MEMS) can incorporate scandium-doped aluminum nitride (ScAlN) thin film layers (active thin film layers) during the formation of the devices and systems. One of the limiting factors for using scandium-doped aluminum nitride is the ability to produce thin film layers without defects on the surface of the scandium-doped aluminum nitride. The defects degrade the performance of the devices and systems. However, the inventors have observed that conventional processes for forming scandium-doped aluminum nitride thin film layers result in a large number of surface cone defects, which significantly degrade the performance of the devices / systems.
[0005] Thus, the present inventors have provided a method for reducing surface defects in deposited active thin film layers, significantly improving the performance of structures using the thin film layers.
[0006] Overview
[0007] Provided herein are methods for reducing surface defects in deposited active thin film layers.
[0008] In some embodiments, a method for reducing surface defects of a thin film layer may include depositing a first seed crystal layer on a substrate, depositing an intermediate thin film layer on the first seed crystal layer at a first temperature of about 350 degrees Celsius to about 700 degrees Celsius, depositing a second seed crystal layer on the intermediate thin film layer, and depositing a piezoelectric thin film layer at a second temperature of less than 200 degrees Celsius.
[0009] In some embodiments, the method may further include, wherein depositing a first seed layer, an intermediate film layer, and a second seed layer without a vacuum break between depositions; wherein the intermediate film layer is a molybdenum layer, and the piezoelectric film layer is a scandium-doped aluminum nitride layer; wherein the scandium-doped aluminum nitride layer has a surface cone defect count of less than or equal to 2 per 100 square microns of the scandium-doped aluminum nitride layer surface area, at least in part due to an increase in crystallinity of the intermediate film layer and a reduction in the formation of surface cone defects on the piezoelectric film layer due to the second seed layer; wherein the first seed layer is aluminum nitride, and the second seed layer is aluminum nitride; wherein the scandium-doped aluminum nitride layer has approximately 20% scandium; wherein The thickness of the first seed crystal layer is about 10nm to about 200nm; wherein the thickness of the second seed crystal layer is about 5nm to about 55nm; wherein the first seed crystal layer has a thickness of about 150nm, the molybdenum layer has a thickness of about 20nm to 400nm, and the second seed crystal layer has a thickness of about 35nm; wherein the scandium-doped aluminum nitride layer has approximately 30% scandium; wherein the thickness of the first seed crystal layer is about 10nm to about 50nm; wherein the thickness of the second seed crystal layer is about 5nm to about 40nm; and / or wherein the first seed crystal layer has a thickness of about 30nm, the molybdenum layer has a thickness of about 25nm, and the second seed crystal layer has a thickness of about 10nm.
[0010] In some embodiments, a method for reducing surface defects of a thin film layer may include degassing a substrate, depositing a first seed layer of aluminum nitride on the substrate in a first deposition chamber after degassing, moving the substrate from the first deposition chamber to a second deposition chamber without breaking the vacuum, depositing a molybdenum layer on the first seed layer in the second deposition chamber at a first temperature of 350 degrees Celsius to approximately 700 degrees Celsius, moving the substrate from the second deposition chamber to the first deposition chamber without breaking the vacuum, depositing a second seed layer of aluminum nitride on the molybdenum layer after depositing the molybdenum layer, cooling the substrate and exposing the substrate to an ambient environment, degassing the substrate, and depositing a scandium-doped aluminum nitride layer in a third deposition chamber at a second temperature below 200 degrees Celsius, wherein the scandium-doped aluminum nitride layer has a surface cone defect count less than or equal to 2 per 100 square microns of the surface area of the scandium-doped aluminum nitride layer.
[0011] In some embodiments, the method may further include wherein the scandium-doped aluminum nitride layer is approximately 20% scandium; wherein the thickness of the first seed layer is approximately 10 nm to approximately 200 nm, and wherein the thickness of the second seed layer is approximately 5 nm to approximately 55 nm; wherein the scandium-doped aluminum nitride layer is approximately 30% scandium; and / or wherein the thickness of the first seed layer is approximately 10 nm to approximately 50 nm, and wherein the thickness of the second seed layer is approximately 5 nm to approximately 40 nm.
[0012] In some embodiments, a non-transitory computer-readable medium having instructions stored thereon, which when executed, result in execution of a method for reducing surface defects of a thin film layer, the method may include depositing a first seed layer on a substrate, depositing a molybdenum layer on the first seed layer at a first temperature of about 350 degrees Celsius to about 700 degrees Celsius, depositing a second seed layer on the molybdenum layer, and depositing a scandium-doped aluminum nitride layer at a second temperature of less than 200 degrees Celsius, wherein the scandium-doped aluminum nitride layer has a surface cone defect count less than or equal to 2 per 100 square microns of the surface area of the scandium-doped aluminum nitride layer.
[0013] In some embodiments, the method of non-transitory computer readable medium may further include, wherein the scandium-doped aluminum nitride layer is 20% or 30% scandium, wherein the first seed layer has a thickness of about 10nm to about 200nm for 20% scandium, wherein the first seed layer has a thickness of about 10nm to about 50nm for 30% scandium, wherein the molybdenum layer has a thickness of about 20nm to about 250nm for 20% scandium or 30% scandium, wherein the second seed layer has a thickness of about 5nm to about 55nm for 20% scandium, and wherein the second seed layer has a thickness of about 5nm to about 40nm for 30% scandium.
[0014] Other embodiments and further embodiments are disclosed below.
[0015] BRIEF DESCRIPTION OF THE DRAWINGS
[0016] The embodiments of the present principles are briefly summarized above and discussed in more detail below, which can be understood by referring to the illustrative embodiments of the principles described in the accompanying drawings. However, the drawings only illustrate typical embodiments of the present principles and are therefore not to be considered limiting of scope, as the present principles may allow other equally effective embodiments.
[0017] Figure 1 Methods of forming thin film stacks according to some embodiments of the present principles.
[0018] Figure 2 Depicted are cross-sectional views of substrates according to some embodiments of the present principles.
[0019] Figure 3 Depicted is a cross-sectional view of forming a first crystalline layer according to some embodiments of the present principles.
[0020] Figure 4 Depicted is a cross-sectional view of forming an intermediate thin film layer on a first seed layer, according to some embodiments of the present principles.
[0021] Figure 5 Depicted is a cross-sectional view of forming a second seed layer on an intermediate film layer according to some embodiments of the present principles.
[0022] Figure 6 Depicted is a cross-sectional view of forming an active thin film layer on a second seed layer according to some embodiments of the present principles.
[0023] Figure 7 Depicted is a top view of a surface showing pyramidal defects per unit area on an active film layer, according to some embodiments of the present principles.
[0024] Figure 8 An integrated tool according to some embodiments of the present principles is depicted.
[0025] For ease of understanding, the same reference numerals are used, where possible, to represent the same elements common to the drawings. These drawings are not drawn to scale and may be simplified for clarity. Elements and features of one embodiment may be beneficially incorporated into other embodiments without further elaboration.
[0026] Specific description
[0027] In some embodiments, the method provides a high-quality active film layer (e.g., a scandium-doped aluminum nitride film layer) with minimal surface cone defects. For example, the technology can provide a new process flow to improve the quality of a scandium-doped aluminum nitride active film layer grown on an intermediate molybdenum layer. The resulting scandium-doped aluminum nitride active film layer has a good crystal orientation, which results in a smaller full-width-half-maximum (FWHM) and loss tangent during the manufacture of, for example, piezoelectric materials and other materials. The method advantageously provides good active film surface quality and good crystal orientation of the intermediate film layer during plasma vapor deposition (PVD) sputtering of a scandium-doped aluminum nitride film stack.
[0028] The content of scandium-doped aluminum nitride is x=20% to 30% (ScxAl (1-x) N) and above are of great interest for MEMS sensing and actuation, ultrasonic generation and energy harvesting applications. The higher the scandium doping concentration, the stronger the electric field of the device / system. It is difficult to deposit scandium-doped aluminum nitride films from highly doped aluminum targets to meet industrial requirements for film properties. Some devices / systems have even more stringent requirements than integrated circuit applications, such as good crystallinity (FWHM: <1.5°) and good surface morphology. The method of the principles of the present invention enables scandium-doped aluminum nitride thin film layers to meet all requirements and even more. The method allows for higher control of the properties of the molybdenum and seed layers to improve surface cone defects and FWHM of scandium-doped aluminum nitride film stacks.
[0029] In short, a process for providing increased control over film orientation and reducing surface tapering defects may include depositing a first seed layer, an intermediate film layer (e.g., a molybdenum layer), a second seed layer, and then depositing an active film layer (e.g., a piezoelectric film layer, such as a scandium-doped aluminum nitride layer). The second seed layer and careful control of the film stacking process by eliminating vacuum breaks and a specific thickness combination of different film layers can produce, for example, a scandium-doped aluminum nitride active film surface with 1 or 2 surface tapering defects or less per 100 square microns for a 20% or 30% scandium-doped aluminum nitride layer composition. For reference, according to some embodiments, Figure 7 A top view 700 of an active film surface 720 is depicted showing one surface cone-shaped defect 728 per unit area 722 on an active film layer, such as a scandium-doped aluminum nitride layer 616. As used herein, the area 722 is defined as a 100 square micrometer area (e.g., width 724 = 10 micrometers, length 726 = 10 micrometers, etc.).
[0030] The technology provided herein provides similar benefits to any plasma vapor deposition (PVD) deposited film to improve crystallinity by high temperature deposition of an intermediate film layer on a first seed layer and to improve the high surface quality of the active film layer by using a second seed layer on the intermediate film layer before depositing the active film layer. In some film stacks, the intermediate film layer can be used as an electrode and can include, but is not limited to, films formed of tungsten, ruthenium, and molybdenum, etc. In some film stacks, the active layer can include a piezoelectric film active layer, which uses thin film materials such as, but not limited to, lead zirconate (PZT), lithium niobate (LiNbO3), lithium tantalate (LiTaO3), and scandium-doped aluminum nitride (ScAlN). The first and second seed layer materials can be adjusted based on compatibility with the intermediate layer material and the active layer material.
[0031] For the sake of simplicity and not meant to be limiting, the examples herein are based on a molybdenum intermediate thin film layer and a scandium-doped aluminum nitride active thin film layer with aluminum nitride first and second seed layers. Figure 1 According to some embodiments, a thin film stack having an active thin film layer such as a scandium-doped aluminum nitride layer is formed (see, for example, Figure 6 During the discussion of method 100, reference is made to Figures 2 to 8 .like Figure 2 The substrate 202 shown in the view 200 of FIG. 1 may be formed of, for example, silicon or silicon dioxide, etc., which is not meant to be limiting. If the substrate 202 has been exposed to the environment, the substrate 202 may be degassed before starting the thin film stack formation process. In block 102, as shown in FIG. Figure 3As shown in view 300 of FIG. 2 , a first seed layer 302 is deposited on substrate 202. In some embodiments, when a thin film stack of aluminum nitride doped with about 20% scandium is formed, a thickness 304 of the first seed layer 302 may be about 10 nm to about 200 nm. In some embodiments, when a thin film stack of aluminum nitride doped with about 30% scandium is formed, a thickness 304 of the first seed layer 302 may be about 10 nm to about 50 nm. The first seed layer 302 may include aluminum nitride, which may be deposited using a first deposition chamber, such as a PVD deposition chamber using an aluminum nitride sputtering target.
[0032] In block 104, if Figure 4 As shown in view 400 of , an intermediate thin film layer, such as a molybdenum layer 408, is deposited on the first seed layer 304. When the thin film stack is used in some devices / systems, the molybdenum layer 408 can be used as an electrode. In some embodiments, the thickness 410 of the molybdenum layer 408 can be from about 20 nm to about 400 nm. The inventors have found that a higher molybdenum thickness can help reduce surface cone defects on the scandium-doped aluminum nitride layer. The molybdenum layer 408 can be deposited using a second deposition chamber, such as a PVD deposition chamber using a molybdenum sputtering target. In some embodiments, in order to optimize the reduction of surface cone defects on the scandium-doped aluminum nitride layer, the molybdenum layer 408 can be deposited without a vacuum break between the deposition of the first seed layer 302 and the deposition of the molybdenum layer 408 to eliminate any possible contamination or particles on the first seed layer 302 before depositing the molybdenum layer 408. For example, the first deposition chamber and the second deposition chamber can be as follows Figure 8 A portion of an integrated tool 800 is shown that operates in a vacuum environment where substrates can be transferred between chambers without a vacuum break.
[0033] The temperature of the molybdenum deposition process can be used to control surface cone defects on the scandium-doped aluminum nitride layer. Higher molybdenum deposition temperatures produce higher quality molybdenum films (e.g., lower FWHM), resulting in a reduction in surface cone defects on subsequently deposited scandium-doped aluminum nitride layers. Higher quality molybdenum surfaces and crystal orientations produce higher quality scandium-doped aluminum nitride layer surfaces (lower surface cone defects). For example, the FWHM of a molybdenum film deposited at about 700°C is reduced from 2.5° of a molybdenum film deposited at about 350°C to less than about 1.2°. As the quality of the molybdenum film improves, the inventors have found that increasing the deposition temperature of the molybdenum to about 700 degrees Celsius can provide a surface cone defect count of less than or equal to 2 defects per 100 square microns for 20% and 30% scandium-doped aluminum nitride layers.
[0034] In block 106, if Figure 5As shown in view 500 of FIG. 5 , a second seed layer 512 is deposited on an intermediate thin film layer, such as molybdenum layer 408. The addition of the second seed layer 512 can reduce surface cone defects on a subsequently deposited scandium-doped aluminum nitride layer even when a lower molybdenum deposition temperature is used (e.g., 350 degrees Celsius for 20% Sc (ScAlN) and 500 degrees Celsius for 30% Sc (ScAlN)). In some cases, lower process temperatures may be required to meet thermal budget constraints for device manufacturing. The method of the present principles enables device manufacturers to now produce low thermal budget devices with low-defect scandium-doped aluminum nitride. In some embodiments, when an aluminum nitride thin film stack having about 20% scandium doping is formed, the thickness 514 of the second seed layer 512 can be about 5 nm to about 55 nm. In some embodiments, when an aluminum nitride thin film stack having about 30% scandium doping is formed, the thickness 514 of the second seed layer 512 can be about 5 nm to about 40 nm. The second seed layer 512 may be composed of aluminum nitride, which may be deposited using a first deposition chamber, such as a PVD deposition chamber using an aluminum nitride sputtering target.
[0035] In some embodiments, in order to optimize the reduction of surface cone defects on the active thin film layer (e.g., the scandium-doped aluminum nitride layer), the second seed layer 512 can be deposited without a vacuum break between the deposition of the molybdenum layer 408 and the deposition of the second seed layer 512 to eliminate any possible contamination or particles on the molybdenum layer 408 before depositing the second seed layer 512. For example, the first deposition chamber and the second deposition chamber can be operated in a vacuum environment such as Figure 8 A portion of an integrated tool 800 is shown in which a substrate can be transferred between chambers without vacuum breaking. The inventors believe that the immediate deposition of the second seed layer 512 retains residual heat from the deposition of the molybdenum layer 408 in the second deposition chamber, and the residual heat can further promote the reduction of surface cone defects in the scandium-doped aluminum nitride layer. The second seed layer 512 serves as a transition layer between the molybdenum layer 408 and the scandium-doped aluminum nitride layer 616 (described below) to promote the reduction of surface cone defect counts with respect to the scandium-doped aluminum nitride layer 616, even when a lower molybdenum deposition temperature (e.g., equal to or less than 500 degrees Celsius) is used.
[0036] In some embodiments, the substrate 202 may be cooled and exposed to the ambient environment. The substrate 202 may then be degassed before continuing to deposit the scandium-doped aluminum nitride layer. If the substrate 202 is cooled within the integrated tool 800, no degassing process is required before continuing to deposit the scandium-doped aluminum nitride layer. In block 108, as Figure 6As shown in view 600 of , an active thin film layer, such as a piezoelectric thin film layer including a scandium-doped aluminum nitride layer 616, is deposited on the second seed layer 512 at a substrate temperature of less than 200 degrees Celsius (without susceptor heating). In some embodiments, the substrate temperature can be less than about 100 degrees Celsius. The lower substrate temperature during deposition reduces surface defect formation. The inventors have found that the quality of the active thin film layer, especially the scandium-doped aluminum nitride film, is determined during the nucleation stage. In some embodiments, the susceptor temperature can be set to about 25 degrees Celsius so as not to add any further heating to the substrate (for example, after the second seed layer is deposited, it can be a temperature of about 60 degrees Celsius to about 70 degrees Celsius). Any heating of the substrate during PVD deposition of the active thin film layer is due to plasma deposition.
[0037] In some embodiments, the thickness 618 of the scandium-doped aluminum nitride layer 616 may be about 5 nm to about 100 nm. The scandium-doped aluminum nitride layer 616 is composed of scandium-doped aluminum nitride, which can be deposited using a third deposition chamber, which can be, for example, a PVD deposition chamber using a composite sputtering target of about 20% scandium-doped aluminum nitride or about 30% scandium-doped aluminum nitride. The third deposition chamber can be a separate or part of the integrated tool 800. As described above, the second seed layer 512 provides a transition layer between the molybdenum layer 408 and the scandium-doped aluminum nitride layer 616. Surface cone defects in the scandium-doped aluminum nitride layer 616 can be formed during the nucleation stage of the deposition process. The inventors have found that depositing scandium-doped aluminum nitride on aluminum nitride (the second seed layer 512) results in fewer surface cone defects than depositing scandium-doped aluminum nitride on molybdenum during the nucleation stage.
[0038] The inventors have discovered that in addition to temperature, vacuum break, and time between depositions, the combination of the thicknesses of the first seed layer 302, the molybdenum layer 408, and the second seed layer 512 can also affect the surface pyramidal defect count of the scandium-doped aluminum nitride layer. In some embodiments, to further reduce the surface pyramidal defect count of the scandium-doped aluminum nitride by about 20%, the first seed layer 304 has a thickness of about 150 nm, the molybdenum layer 408 has a thickness of about 200 nm, and the second seed layer 512 has a thickness of about 35 nm. In some embodiments, to further reduce the surface pyramidal defect count of the scandium-doped aluminum nitride by about 30%, the first seed layer 304 has a thickness of about 30 nm, the molybdenum layer 408 has a thickness of about 25 nm, and the second seed layer 512 has a thickness of about 10 nm.
[0039] The methods described herein may be performed in a separate process chamber, which may be provided in a standalone configuration or as part of a cluster tool, for example, as described below with respect to Figure 8An integrated tool 800 (i.e., a cluster tool) is described. An advantage of using the integrated tool 800 is that there is no vacuum break between chambers, and therefore, there is no need to degas and pre-clean the substrate prior to processing in the chamber. For example, in some embodiments, the methods of the present invention discussed above can be advantageously performed in an integrated tool so that there is limited or no vacuum break between processes, thereby limiting or preventing contamination of the substrate, such as oxidation, etc. The integrated tool 800 includes a vacuum sealed processing platform 801, a factory interface 804, and a system controller 802. The processing platform 801 includes a plurality of processing chambers, such as 814A, 813B, 814C, 814D, 814E, and 814F, which are operably coupled to vacuum substrate transfer chambers (transfer chambers 803A, 803B). The factory interface 804 consists of one or more load lock chambers (two load lock chambers, such as Figure 8 806A and 806B) shown in operably coupled to the transfer chamber 803A.
[0040] In some embodiments, the factory interface 804 includes at least one docking station 807 and at least one factory interface robot 838 to facilitate the transfer of semiconductor substrates. The docking station 807 is configured to receive one or more front opening unified pods (FOUPs). Figure 8 In the embodiment of FIG. 8 , four FOUPs are shown, such as 805A, 805B, 805C, and 805D. The factory interface robot 838 is configured to transfer substrates from the factory interface 804 to the processing platform 801 through the load lock chambers, such as 806A and 806B. Each of the load lock chambers 806A and 806B has a first port coupled to the factory interface 804 and a second port coupled to the transfer chamber 803A. The load lock chambers 806A and 806B are coupled to a pressure control system (not shown) that evacuates and vents the load lock chambers 806A and 806B to facilitate the passage of substrates between the vacuum environment of the transfer chamber 803A and the substantially ambient (e.g., atmospheric) environment of the factory interface 804. The transfer chambers 803A, 803B have vacuum robots 842A, 842B disposed in the respective transfer chambers 803A, 803B. The vacuum robot 842A can transfer the substrate 821 between the load lock chambers 806A, 806B, the process chambers 814A and 814F, and the cooling station 840 or the pre-cleaning station 842. The vacuum robot 842B can transfer the substrate 821 between the cooling station 840 or the pre-cleaning station 842 and the process chambers 814B, 814C, 814D, and 814E.
[0041] In some embodiments, processing chambers 814A, 814B, 814C, 814D, 814E, and 814F are coupled to transfer chambers 803A, 803B. Processing chambers 814A, 814B, 814C, 814D, 814E, and 814F may include, for example, atomic layer deposition (ALD) processing chambers, physical vapor deposition (PVD) processing chambers, chemical vapor deposition (CVD) chambers, annealing chambers, and the like. As described above, the chambers may include any chamber suitable for performing all or part of the methods described herein, such as a molybdenum deposition chamber, an aluminum nitride deposition chamber, a scandium-doped aluminum nitride deposition chamber, and the like. In some embodiments, one or more optional service chambers (shown as 816A and 816B) may be coupled to transfer chamber 803A. The service chambers 816A and 816B may be configured to perform other substrate processing such as degassing, orientation, substrate metrology, cooling, and the like.
[0042] The system controller 802 controls the operation of the tool 800 using direct control of the process chambers 814A, 814B, 814C, 814D, 814E, and 814F, or by controlling a computer (or controller) associated with the process chambers 814A, 814B, 814C, 814D, 814E, and 814F and the tool 800. In operation, the system controller 802 enables data to be collected and fed back from the corresponding chambers and systems to optimize the performance of the tool 800. The system controller 802 generally includes a central processing unit (CPU) 830, a memory 834, and support circuits 832. The CPU 830 can be any form of general-purpose computer processor that can be used in an industrial environment. The support circuits 832 are coupled to the CPU 830 in a conventional manner and can include caches, clock circuits, input / output subsystems, power supplies, etc. A software routine such as the method described above may be stored in memory 834 and, when executed by CPU 830, transforms CPU 830 into a special purpose computer (system controller) 802. The software routine may also be stored and / or executed by a second controller (not shown) located remotely from tool 800.
[0043] Embodiments according to the present principles may be implemented in hardware, firmware, software, or any combination thereof. Embodiments may also be implemented as instructions stored using one or more computer-readable media, which may be read and executed by one or more processors. Computer-readable media may include any mechanism for storing or transmitting information in a form readable by a machine (e.g., a computing platform or a "virtual machine" running on one or more computing platforms). For example, a computer-readable medium may include any suitable form of volatile or non-volatile memory. In some embodiments, a computer-readable medium may include a non-temporary computer-readable medium.
[0044] While the foregoing is directed to embodiments of the present principles, other and further embodiments of the present principles may be devised without departing from the basic scope thereof.
Claims
1. A method for reducing surface defects of a thin film layer, comprising the following steps: depositing a first crystalline layer on the substrate; depositing an intermediate thin film layer on the first seed layer at a first temperature of about 350 degrees Celsius to about 700 degrees Celsius; depositing a second seed layer on the intermediate thin film layer; and A piezoelectric thin film layer is deposited on the second seed layer at a second temperature less than 200 degrees Celsius.
2. The method of claim 1, wherein the first seed layer, the intermediate thin film layer, and the second seed layer are deposited without a vacuum break between depositions.
3. The method of claim 1, wherein the intermediate film layer is a molybdenum layer and the piezoelectric film layer is a scandium-doped aluminum nitride layer.
4. The method of claim 3, wherein the scandium-doped aluminum nitride layer has a surface pyramidal defect count less than or equal to 2 per 100 square microns of surface area of the scandium-doped aluminum nitride layer, at least in part due to the increased crystallinity of the intermediate film layer during deposition and the deposition of the second seed layer prior to depositing the piezoelectric film layer.
5. The method of claim 3, wherein the first seed layer is aluminum nitride and the second seed layer is aluminum nitride.
6. The method of claim 3 wherein the scandium doped aluminum nitride layer is approximately 20% scandium.
7. The method of claim 6, wherein the first crystalline layer has a thickness of about 10 nm to about 200 nm.
8. The method of claim 6, wherein the second seed layer has a thickness of about 5 nm to about 55 nm.
9. The method of claim 6, wherein the first seed layer has a thickness of about 150 nm, the molybdenum layer has a thickness of about 20 nm to 400 nm, and the second seed layer has a thickness of about 35 nm.
10. The method of claim 3, wherein the scandium doped aluminum nitride layer is approximately 30% scandium.
11. The method of claim 10, wherein the first crystalline layer has a thickness of about 10 nm to about 50 nm.
12. The method of claim 10, wherein the second seed layer has a thickness of about 5 nm to about 40 nm.
13. The method of claim 10, wherein the first seed layer has a thickness of approximately 30 nm, the molybdenum layer has a thickness of approximately 25 nm, and the second seed layer has a thickness of approximately 10 nm.
14. A method for reducing surface defects of a thin film layer, comprising the following steps: Degassing the substrate; After degassing, depositing a first seed layer of aluminum nitride on the substrate in a first deposition chamber; moving the substrate from the first deposition chamber to a second deposition chamber without breaking vacuum; depositing a molybdenum layer on the first seed layer in the second deposition chamber at a first temperature of 350 degrees Celsius to about 700 degrees Celsius; moving the substrate from the second deposition chamber to the first deposition chamber without breaking vacuum; After depositing the molybdenum layer, depositing a second seed layer of aluminum nitride on the molybdenum layer; cooling the substrate and exposing the substrate to an ambient environment; degassing the substrate; and A scandium-doped aluminum nitride layer is deposited in a third deposition chamber at a second temperature of less than 200 degrees Celsius, wherein the scandium-doped aluminum nitride layer has a surface pyramidal defect count less than or equal to 2 per 100 square microns of a surface area of the scandium-doped aluminum nitride layer.
15. The method of claim 14, wherein the scandium doped aluminum nitride layer is approximately 20% scandium.
16. The method of claim 15, wherein the first seed layer has a thickness of about 10 nm to about 200 nm, and wherein the second seed layer has a thickness of about 5 nm to about 55 nm.
17. The method of claim 14, wherein the scandium doped aluminum nitride layer is approximately 30% scandium.
18. The method of claim 17, wherein the first seed layer has a thickness of about 10 nm to about 50 nm, and wherein the second seed layer has a thickness of about 5 nm to about 40 nm.
19. A non-transitory computer readable medium having stored thereon instructions, which when executed cause a method of reducing surface defects of a thin film layer to be performed, the method comprising the steps of: depositing a first crystalline layer on the substrate; depositing a molybdenum layer on the first seed layer at a first temperature of about 350 degrees Celsius to about 700 degrees Celsius; depositing a second seed layer on the molybdenum layer; and A scandium-doped aluminum nitride layer is deposited at a second temperature of less than 200 degrees Celsius, wherein the scandium-doped aluminum nitride layer has a surface pyramidal defect count of less than or equal to 2 per 100 square microns of surface area of the scandium-doped aluminum nitride layer.
20. A non-transitory computer-readable medium as described in claim 19, wherein the scandium-doped aluminum nitride layer is 20% or 30% scandium, wherein the first seed layer has a thickness of about 10nm to about 200nm for 20% scandium, wherein for 30% scandium, the first seed layer has a thickness of about 10nm to about 50nm, wherein for 20% scandium or 30% scandium, the molybdenum layer has a thickness of about 20nm to about 250nm, wherein for 20% scandium, the second seed layer has a thickness of 5nm to about 55nm, and wherein for 30% scandium, the second seed layer has a thickness of about 5nm to about 40nm.