Oyster shell-lanthanum hydroxide composite material, preparation method thereof and application of oyster shell-lanthanum hydroxide composite material in phosphorus removal of water body

Through the use of oyster shell-lanthanum hydroxide composite materials, the existing adsorbents have been solved in poor phosphorus removal, difficult separation and high cost, and efficient and low-cost removal of phosphorus pollution in water bodies is achieved, suitable for natural water bodies and Treatment of industrial wastewater.

CN119075896APending Publication Date: 2024-12-06HENAN UNIVERSITY +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411198015.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing hydroxide and oxide adsorbents have incomplete phosphorus removal effect in water bodies, are difficult to separate after adsorption and are costly, making it difficult to effectively solve the problem of phosphorus chemical pollution.

Method used

The oyster shell-lanthanum hydroxide composite material is used to load the lanthanum hydroxide particles on the oyster shell powder to form a composite material. Its efficient adsorption mechanism of lanthanum phosphate is used to achieve efficient phosphorus removal, and due to the amorphous and irregular structure of the material , easy to separate after adsorption and low cost.

Benefits of technology

It has achieved efficient removal of phosphorus in water, with an adsorption amount of 112.42 mg/g, a removal rate of nearly 100%, and the material is easy to separate and has low cost. It is suitable for phosphorus pollution removal of groundwater, surface water and industrial wastewater.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119075896A_ABST
    Figure CN119075896A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of adsorption materials, and provides an oyster shell-lanthanum hydroxide composite material, a preparation method thereof and application of the oyster shell-lanthanum hydroxide composite material in phosphorus removal of a water body. The oyster shell-lanthanum hydroxide composite material provided by the invention comprises oyster shell powder and lanthanum hydroxide particles loaded on the oyster shell powder, the surface of the composite material has a large number of adsorption sites, the composite material has relatively strong affinity to phosphorus, and a product after phosphorus adsorption has good stability and high phosphorus removal efficiency, and is easy to separate after adsorption; meanwhile, the oyster shell powder is adopted as the raw material, the raw material is low in price, easy to obtain, green, environmentally friendly and free of pollution, and waste of oyster shells can be slowed down to a certain extent; in addition, the preparation method of the composite material is simple, and large-scale batch synthesis can be achieved. In conclusion, the oyster shell-lanthanum hydroxide composite material provided by the invention has potential application value and prospect in the aspect of removing phosphorus pollution in natural water bodies such as underground water and surface water or industrial wastewater.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of adsorption materials, and in particular to an oyster shell-lanthanum hydroxide composite material and a preparation method thereof and application thereof in water body phosphorus removal. Background Art

[0002] With the development of phosphorus chemical industry, the environmental pollution is becoming more and more serious. Therefore, preventing and controlling phosphorus chemical pollution, protecting the ecological environment, and rationally utilizing non-renewable limited resources are urgent tasks and important topics facing the healthy development of my country's phosphorus chemical industry. It is of great practical significance to recognize the hazards of phosphorus pollution and study the methods of phosphorus removal.

[0003] At present, researchers have explored a variety of ways to purify phosphorus in water systems, including chemical precipitation, ion exchange, adsorption, biological methods and membrane separation. Among these methods, adsorption has the advantages of low cost, easy operation and high removal efficiency, and is widely regarded as a promising technology. Therefore, in recent years, researchers have invested a lot of energy in adsorbents. Common phosphorus removal adsorbents include hydroxides and oxides. However, the commonly used hydroxide and oxide adsorbents generally have problems such as incomplete phosphorus removal, difficult separation process after adsorption, and high cost. Summary of the invention

[0004] In view of this, the present invention provides an oyster shell-lanthanum hydroxide composite material and a preparation method thereof and application thereof in water phosphorus removal. The oyster shell-lanthanum hydroxide composite material provided by the present invention has good phosphorus removal effect, is easy to separate after adsorption, and has low cost, and has potential application value and prospects in water phosphorus removal.

[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0006] An oyster shell-lanthanum hydroxide composite material comprises oyster shell powder and lanthanum hydroxide particles loaded on the oyster shell powder.

[0007] Preferably, the mass fraction of lanthanum hydroxide particles in the oyster shell-lanthanum hydroxide composite material is 10 to 80%.

[0008] The present invention also provides a method for preparing the oyster shell-lanthanum hydroxide composite material described in the above scheme, comprising the following steps:

[0009] The lanthanum salt solution and the oyster shell powder suspension are mixed to obtain a mixed solution;

[0010] The alkaline solution and the mixed solution are mixed, aged and centrifuged to obtain the oyster shell-lanthanum hydroxide composite material.

[0011] Preferably, the lanthanum salt in the lanthanum salt solution comprises one or more of lanthanum nitrate, lanthanum chloride and lanthanum sulfate; 3+ The concentration is 0.05~1.2mol / L.

[0012] Preferably, the concentration of the oyster shell powder suspension is 5 to 30 g / L; the lanthanum salt solution contains La 3+ The mass ratio of oyster shell powder to the oyster shell powder suspension is 1:(0.2~3.5).

[0013] Preferably, the lanthanum salt solution and the oyster shell powder suspension are mixed in the following manner: under stirring conditions, the lanthanum salt solution is added to the oyster shell powder suspension, and stirring is continued for 0.2 to 12 hours after the addition is completed.

[0014] Preferably, the alkaline solution is an inorganic strong alkali solution or aqueous ammonia; the solvent of the inorganic strong alkali solution is water, ethanol or an ethanol-water mixed solvent; the concentration of the alkaline solution is 0.2 to 5 mol / L.

[0015] Preferably, the inorganic strong alkali solution and the mixed solution are mixed in a manner of: adding the alkaline solution to the mixed solution under stirring conditions.

[0016] Preferably, the alkaline solution is added by dripping, injection or pouring; when the addition method is dripping, the pH value of the system is controlled to be 9 to 12 during the dripping process, and then stirring is continued for 0.2 to 5 hours.

[0017] Preferably, the aging time is 1 to 24 hours.

[0018] The present invention also provides the use of the oyster shell-lanthanum hydroxide composite material described in the above scheme or the oyster shell-lanthanum hydroxide composite material prepared by the preparation method described in the above scheme in phosphorus removal from water.

[0019] The present invention provides an oyster shell-lanthanum hydroxide composite material (oyster shell @ La (OH) 3 composite material), comprising oyster shell powder and lanthanum hydroxide particles loaded on the oyster shell powder. The present invention loads lanthanum hydroxide particles on the surface of the oyster shell powder, and its phosphorus removal mechanism is: lanthanum hydroxide can form lanthanum phosphate after adsorbing phosphorus, thereby achieving phosphorus removal; the composite material surface provided by the present invention has a large number of adsorption sites, has a strong affinity for phosphorus, and the product after adsorbing phosphorus has good stability and high phosphorus removal efficiency, which overcomes the disadvantage of poor phosphorus removal effect of traditional La (lanthanum) based materials. The results of the embodiment show that when the pH is 7.0 and the dosage of the oyster shell-lanthanum hydroxide composite material is 0.5g / L, the phosphorus adsorption amount of the composite material can reach 112.42mg / g, and under the conditions of a phosphorus concentration of 30mg / L and a pH value of 3 to 9, the phosphorus removal rate of the composite material of the present invention is close to 100%.

[0020] In addition, the oyster shell-lanthanum hydroxide composite material provided by the present invention is an amorphous, irregular particle aggregate, which is easy to separate after adsorption. In addition, the present invention uses oyster shell powder as a raw material, the raw material is cheap and easy to obtain, green and pollution-free, and can also slow down the waste of oyster shells to a certain extent.

[0021] In summary, the oyster shell-lanthanum hydroxide composite material provided by the present invention has high phosphorus removal efficiency, is easy to separate, and has low cost, and has potential application value and prospects in the removal of phosphorus pollution in natural water bodies such as groundwater and surface water or industrial wastewater.

[0022] The present invention also provides a method for preparing the oyster shell-lanthanum hydroxide composite material described in the above scheme. The preparation method provided by the present invention is simple to operate and can be synthesized in large quantities. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 It is a schematic diagram of the preparation process and phosphorus removal process of the oyster shell-lanthanum hydroxide composite material of the present invention;

[0024] Figure 2 This is the XRD pattern of the oyster shell@La(OH)3 composite material prepared in Example 1;

[0025] Figure 3 This is a SEM image of the oyster shell@La(OH)3 composite material prepared in Example 1;

[0026] Figure 4 The adsorption amount and removal efficiency of phosphorus by oyster shell@La(OH)3 composite material under different initial concentrations of phosphorus solution;

[0027] Figure 5 The effect of interference of different coexisting ions on phosphorus removal by oyster shell@La(OH)3 composites;

[0028] Figure 6 is the phosphorus removal efficiency of oyster shell@La(OH)3 composite material after five cycles at pH 7;

[0029] Figure 7 This is a comparison chart of the phosphorus removal effects of oyster shell@La(OH)3 composite material and oyster shell powder under pH values ​​of 3 to 11. DETAILED DESCRIPTION

[0030] The invention provides an oyster shell-lanthanum hydroxide composite material, comprising oyster shell powder and lanthanum hydroxide particles loaded on the oyster shell powder.

[0031] In the present invention, the mass fraction of lanthanum hydroxide particles in the oyster shell-lanthanum hydroxide composite material is preferably 10 to 80%, and more preferably 20 to 60%.

[0032] The present invention also provides a method for preparing the oyster shell-lanthanum hydroxide composite material described in the above scheme, comprising the following steps:

[0033] The lanthanum salt solution and the oyster shell powder suspension are mixed to obtain a mixed solution;

[0034] The alkaline solution and the mixed solution are mixed, aged and centrifuged to obtain the oyster shell-lanthanum hydroxide composite material.

[0035] The present invention mixes a lanthanum salt solution and an oyster shell powder suspension to obtain a mixed solution. In the present invention, the lanthanum salt in the lanthanum salt solution preferably includes one or more of lanthanum nitrate, lanthanum chloride and lanthanum sulfate, and more preferably La(NO3)3·6H2O, LaCl3·7H2O or La2(SO4)3·9H2O; La in the lanthanum salt solution 3+ The concentration of the oyster shell powder suspension is preferably 0.05-1.2 mol / L, more preferably 0.1-0.6 mol / L, and further preferably 0.3-0.5 mol / L; the concentration of the oyster shell powder suspension is preferably 5-30 g / L, more preferably 10-20 g / L; in a specific embodiment of the present invention, the oyster shell powder is preferably passed through a 100-mesh sieve, and the sieve under is used; the solvent of the lanthanum salt solution and the oyster shell powder suspension is preferably water, and the present invention has no special requirements for the water, and tap water or distilled water can be used; La in the lanthanum salt solution 3+ The mass ratio of oyster shell powder to the oyster shell powder in the oyster shell powder suspension is preferably 1:(0.2-3.5), and more preferably 1:(1.4-1.5).

[0036] In the present invention, the lanthanum salt solution and the oyster shell powder suspension are preferably mixed in the following manner: under stirring conditions, the lanthanum salt solution is added to the oyster shell powder suspension, and stirring is continued for 0.2 to 12 hours after the addition is completed, preferably stirring is continued for 0.2 to 3 hours, and more preferably stirring is continued for 0.5 to 2.5 hours; the lanthanum salt solution is preferably slowly added to the oyster shell powder solution; the present invention has no special requirements for the stirring speed, as long as the lanthanum salt solution and the oyster shell powder suspension can be fully mixed.

[0037] After obtaining the mixed solution, the present invention mixes the alkaline solution with the mixed solution, and then ages and centrifuges to obtain the oyster shell-lanthanum hydroxide composite material. In the present invention, the alkaline is preferably an inorganic strong base solution or ammonia water; the inorganic strong base is preferably an alkali metal hydroxide, more preferably KOH or NaOH; the solvent of the inorganic strong base solution is preferably water, ethanol or an ethanol-water mixed solvent; the volume fraction of ethanol in the ethanol-water mixed solvent is preferably 20-80%, more preferably 40-60%, more preferably 46%; the concentration of the alkaline solution is preferably 0.2-5 mol / L, more preferably 2-3 mol / L.

[0038] In the present invention, the alkaline solution and the mixed liquid are preferably mixed in a manner of: adding the alkaline solution to the mixed liquid under stirring; in a specific embodiment of the present invention, the adding method is preferably dripping, injecting or pouring, more preferably dripping; when the dripping method is adopted, the pH value of the system is preferably controlled to be 9-12, preferably 10-11 during the dripping process, and stirring is continued for 0.2-5h after the dripping is completed, more preferably stirring is continued for 0.5-2.5h; in a specific embodiment of the present invention, as the reaction proceeds, the pH value of the system will decrease, and the present invention preferably maintains the pH value of the mixed system at 10-11 by dripping the alkaline solution.

[0039] In the present invention, the aging time is preferably 1 to 24 hours, more preferably 1 to 8 hours, and further preferably 2 to 6 hours; the aging temperature is preferably room temperature; the present invention has no special requirements for the specific operation method of the centrifugation, and the method familiar to those skilled in the art can be used.

[0040] After the centrifugation is completed, the present invention preferably further comprises washing and drying the obtained solid product; the present invention has no special requirements for the washing, and the washing can be carried out by methods well known to those skilled in the art; the drying is preferably vacuum drying, freeze drying or oven drying.

[0041] The present invention also provides the use of the oyster shell-lanthanum hydroxide composite material described in the above scheme or the oyster shell-lanthanum hydroxide composite material prepared by the preparation method described in the above scheme in phosphorus removal from water bodies; the present invention has no special requirements for the specific method of the application, and any method familiar to those skilled in the art can be used; the water body is preferably a natural water body or industrial wastewater, and the natural water body is specifically groundwater, surface water, etc.; the pH value of the water body is preferably 3 to 11, more preferably 3 to 9, and further preferably 7; the phosphorus content in the water body is preferably 0.1 to 80 mg / L.

[0042] In a specific embodiment of the present invention, when removing phosphorus from water, the oyster shell-lanthanum hydroxide composite material of the present invention is preferably added to the raw water, mixed and adsorbed, so as to efficiently remove phosphorus in the water; the amount of the oyster shell-lanthanum hydroxide composite material can be determined according to the quality of the raw water; the adsorption time is preferably 2 to 24 hours, preferably 6 to 18 hours; after the adsorption is completed, the adsorbed composite material is preferably separated from the water by solid-liquid separation.

[0043] In a specific embodiment of the present invention, the adsorbed composite material is preferably regenerated and reused, and the regeneration method preferably includes: mixing the adsorbed composite material and an alkaline solution for shaking treatment; the alkaline solution is preferably an inorganic strong base solution or ammonia water; the inorganic strong base is preferably an alkali metal hydroxide, more preferably sodium hydroxide or potassium hydroxide; the concentration of the alkaline solution is preferably 0.05-0.2 mol / L, more preferably 0.1 mol / L; the temperature of the shaking treatment is preferably 25-35°C, and the time is preferably 5-7h, more preferably 6h.

[0044] Figure 1 The present invention is a schematic diagram of the preparation process and phosphorus removal process of the oyster shell-lanthanum hydroxide composite material. The present invention uses oyster shell powder to load lanthanum hydroxide particles, and uses the obtained composite material to remove phosphorus from water. The composite material has strong adsorption capacity, is green and economical, and has good application prospects and promotion value.

[0045] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0046] Example 1

[0047] Preparation of oyster shell-lanthanum hydroxide composite material:

[0048] (1) Dissolve 6.5 g La(NO3)3·6H2O in 50 mL of double distilled water to obtain a lanthanum salt solution, in which La 3+ The concentration is 0.3 mol / L;

[0049] (2) dissolving 3 g of oyster shell powder in 200 mL of water to obtain an oyster shell powder suspension;

[0050] (3) under stirring conditions, slowly adding the lanthanum salt solution obtained in step (1) to the oyster shell powder suspension obtained in step (2);

[0051] (4) Dissolve 16.8 g of KOH in 100 mL of an ethanol-water mixed solvent (the volume fraction of ethanol is 46%) to obtain a KOH solution in which the concentration of KOH is 3 mol / L:

[0052] (5) continuing to stir the milky white precipitate obtained in step (3), and then adding the KOH solution prepared in step (4) dropwise into the milky white suspension to maintain pH = 11;

[0053] (6) The mixed liquid obtained in step (5) is stirred for 2 hours, aged for 3 hours, and then centrifuged, washed and dried to obtain an oyster shell@La(OH)3 composite material.

[0054] Example 2

[0055] Preparation of oyster shell-lanthanum hydroxide composite material:

[0056] (1) Dissolve 5.57 g LaCl3·7H2O in 50 mL tap water to obtain a lanthanum salt solution, in which La 3+ The concentration is 0.3 mol / L;

[0057] (2) dissolving 3 g of oyster shell powder in 200 mL of water to obtain an oyster shell powder suspension;

[0058] (3) under stirring conditions, slowly adding the lanthanum salt solution obtained in step (1) to the oyster shell powder suspension obtained in step (2);

[0059] (4) Dissolve 4.2 g of KOH in 25 mL of an ethanol-water mixed solvent (the volume fraction of ethanol is 46%) to obtain a KOH solution in which the concentration of KOH is 3 mol / L:

[0060] (5) continuing to stir the milky white precipitate obtained in step (3), and then pouring the KOH solution prepared in step (4) into the milky white suspension;

[0061] (6) The mixed liquid obtained in step (5) is stirred for 2 hours, aged for 3 hours, and then centrifuged, washed and dried to obtain an oyster shell@La(OH)3 composite material.

[0062] Example 3

[0063] Preparation of oyster shell-lanthanum hydroxide composite material:

[0064] (1) Dissolve 5.46 g La2(SO4)3·9H2O in 50 mL of double distilled water to obtain a lanthanum salt solution, in which La 3+ The concentration is 0.3 mol / L;

[0065] (2) dissolving 3 g of oyster shell powder in 200 mL of water to obtain an oyster shell powder suspension;

[0066] (3) under stirring conditions, slowly adding the lanthanum salt solution obtained in step (1) to the oyster shell powder suspension obtained in step (2);

[0067] (4) Dissolve 16.8 g of KOH in 100 mL of an ethanol-water mixed solvent (the volume fraction of ethanol is 46%) to obtain a KOH solution in which the concentration of KOH is 3 mol / L:

[0068] (5) The milky white precipitate obtained in step (3) is continuously stirred, and then the KOH solution prepared in step (4) is added dropwise to the milky white suspension to maintain pH = 11;

[0069] (6) The mixed liquid obtained in step (5) is stirred for 2 hours, aged for 3 hours, and then centrifuged, washed and dried to obtain an oyster shell@La(OH)3 composite material.

[0070] Comparative Example 1

[0071] A three-dimensional structured rush loaded with La(OH)3 was used as comparative example 1. The preparation method of the three-dimensional structured rush loaded with La(OH)3 is referred to Yuhang Xu. Desalination and Water Treatment. Volume. 311, November 2023, Pages 228-236.

[0072] Test Case

[0073] The structure and adsorption performance of the composite material synthesized in Example 1 were studied.

[0074] (1) Structural study

[0075] Figure 2 The XRD pattern of the oyster shell @ La (OH) 3 composite material prepared in Example 1, wherein OS represents oyster shell powder, and OS-La represents oyster shell @ La (OH) 3 composite material; Figure 2 It can be seen that the main component of oyster shell is CaCO3, and La(OH)3 is successfully loaded onto the oyster shell.

[0076] Figure 3 This is a SEM image of the oyster shell@La(OH)3 composite material prepared in Example 1. Figure 3 It can be seen that a large number of nanosheet lamellar agglomerates are gathered on the surface of the composite material with a relatively large attachment area, which provides abundant attachment points for phosphorus adsorption active sites and helps to improve the phosphorus adsorption capacity of the composite material.

[0077] (2) Adsorption performance study

[0078] Sodium dihydrogen phosphate was used to prepare phosphorus-containing solutions with initial phosphorus concentrations of 40 mg / L, 45 mg / L, 50 mg / L, 55 mg / L, 60 mg / L, 65 mg / L, 70 mg / L, 75 mg / L, and 80 mg / L, respectively. 100 mL of the phosphorus-containing solution was placed in a conical flask, the pH of the solution was adjusted to about 7, and then 0.5 g / L of the adsorption material (i.e., the oyster shell@La(OH)3 composite material prepared in Example 1) was added. The pH value of the system was maintained stable at 7 with 1 mol / L or 0.1 mol / L NaOH solution or HCl solution. The conical flask was sealed with plastic wrap to prevent the solution from splashing during the shaking process. The conical flask was placed in a desktop constant temperature oscillator and shaken at 200 rpm. After balancing for 24 hours, a syringe filter was used to sample and analyze the phosphorus concentration in the solution.

[0079] The test results are as follows Figure 4 As shown, according to Figure 4 It can be seen that the equilibrium adsorption capacity of phosphorus by the oyster shell @ La (OH) 3 composite material under different initial concentrations of phosphorus solution is 76.87 mg / g, 86.93 mg / g, 95.42 mg / g, 106.67 mg / g, 107.43 mg / g, 107.57 mg / g, 107.76 mg / g, 108.19 mg / g, and 112.42 mg / g, respectively. This indicates that the oyster shell @ La (OH) 3 composite material prepared by the present invention has good adsorption performance for phosphorus, and the adsorption capacity can reach 112.42 mg / g.

[0080] (3) Study on the influence of coexisting ions

[0081] Sodium dihydrogen phosphate was used to prepare 100 mL of a phosphorus solution with an initial concentration of 50 mg / L. The solution was placed in a conical flask and the pH was adjusted to 7. Then, five interfering ions (HCO3 - 、C5H7O5COO - ,Ac - 、SO4 - 、NO3 - ), add 0.5 g / L of adsorption material (i.e., the oyster shell@La(OH)3 composite material prepared in Example 1), maintain the pH value stable at 7 with 1 mol / L or 0.1 mol / L NaOH solution or HCl solution, seal the conical flask with plastic wrap to prevent the solution from splashing during the shaking process, place the conical flask in a desktop constant temperature oscillator, shake at 200 rpm, and after balancing for 24 hours, use a syringe filter to sample and analyze the phosphorus concentration in the solution.

[0082] The test results are as follows Figure 5 shown; according to Figure 5 It can be seen that: at different concentrations of HCO3 - 、SO4 - 、NO3 - In the solution, the amount of phosphorus adsorbed by the adsorbent material and the removal efficiency do not change much. This is because these anions will not occupy the adsorption sites of phosphorus, or their affinity for the adsorption sites is weaker than that of phosphorus. The removal efficiency of phosphorus can still be maintained above 80%. Organic compounds in water, such as C5H7O5COO - ,Ac - , can be used with La 3+ The reaction forms La-C5H7O5COO and La-Ac, thus reducing the phosphate removal efficiency.

[0083] (4) Recycling of adsorption materials

[0084] The adsorbent material (i.e., the oyster shell@La(OH)3 composite material prepared in Example 1) was added to 100 mL of a phosphorus solution with an initial concentration of 1 mg / L and a pH value of 7.0. The amount of adsorbent material added was controlled to be 0.5 g / L, and the solution was shaken in a constant temperature shaker at 25°C for 24 hours. During this period, the pH of the solution was adjusted with HCl to make the final pH of the solution = 7, and the solid-liquid separation was performed. The residual concentration of phosphorus in the solution was measured. The adsorbent material after adsorption was added to 100 mL of 1.0 mol / L NaOH solution, shaken in a constant temperature shaker for 6 hours, centrifuged, and washed with tap water. The adsorption experiment was carried out again, and the adsorption-desorption cycle was repeated 5 times to calculate the phosphorus removal efficiency.

[0085] The test results are as follows Figure 6 As shown. Figure 6 It can be seen that the phosphorus removal efficiency in the five cycle experiments reached more than 90%. The results show that the oyster shell@La(OH)3 composite material prepared by the present invention is an economical and easy-to-operate material for removing phosphorus-contaminated water.

[0086] (5) Comparison between the adsorption material of the present invention and oyster shell powder

[0087] Sodium dihydrogen phosphate was used to prepare 100 mL of a solution with an initial phosphorus concentration of 30 mg / L, and the pH value of the solution was adjusted to 3-11. The solution was then divided into two groups, and 0.05 g of the oyster shell@La(OH)3 composite material and oyster shell powder prepared in Example 1 were added respectively. The pH value was maintained stable with 1 mol / L NaOH solution or HCl solution. After equilibration for 24 hours, the phosphorus concentration in the solution was sampled and analyzed using a syringe and a 0.22 μm filter.

[0088] The test results are as follows Figure 7 As shown. Figure 7It can be seen that oyster shell powder has a high phosphorus removal rate only when the solution pH value is 7-9, but the highest phosphorus removal rate is only about 78%, while the oyster shell@La(OH)3 composite material provided by the present invention has a high phosphorus removal rate under the condition of solution pH value of 3-11, especially in the range of pH value of 3-9, the phosphorus removal rate is close to 100%. The above results show that the present invention uses lanthanum hydroxide particles and oyster shell powder to composite, which can significantly improve the phosphorus removal ability.

[0089] (6) Comparison of the adsorption material of the present invention with other lanthanum modified materials

[0090] The maximum adsorption capacity of the material in Comparative Example 1 at 25°C is 22.75 mg / g, while the adsorption capacity of the oyster shell@La(OH)3 composite material provided by the present invention is 112.42 mg / g under the conditions of pH 7 and initial phosphorus concentration of 80 mg / L. The above results show that the composite of lanthanum hydroxide particles and oyster shell powder in the present invention can significantly improve the phosphorus removal capacity and is an excellent phosphorus adsorption material.

[0091] (7) Practical application of the adsorbent material of the present invention 1

[0092] This experiment is to remove phosphorus from a chemical wastewater in Henan Province using this adsorbent material. The chemical wastewater contains a large amount of inorganic coexisting ions (such as Cl - 、NO3 - 、Na + , K + etc.), the phosphorus concentration was 12.43 mg / L, and the pH was 6.49; 1L of the chemical wastewater was taken, 1g of the oyster shell @La(OH)3 adsorbent prepared in Example 1 was added, and the mixture was stirred for 6 hours (during which the pH of the solution was adjusted with dilute HCl so that the final pH of the solution was less than 7), solid-liquid separation was performed, and the residual phosphorus concentration was tested. The results showed that the phosphorus concentration in the solution was 0.19 mg / L, and the removal efficiency reached 98.47%, which met the wastewater discharge needs.

[0093] (8) Practical application of the adsorbent material of the present invention 2

[0094] This experiment is to remove phosphorus from phosphorus-containing industrial wastewater in Henan Province using the adsorbent material. The phosphorus concentration of the phosphorus-containing industrial wastewater is 5 mg / L and the pH is 3.65. Take 1L of the phosphorus-containing industrial wastewater, add 2.0g of the oyster shell@La(OH)3 composite material prepared in Example 1, and shake it in a constant temperature shaker for 6 hours. During this period, the pH of the solution is adjusted with dilute HCl to make the final pH of the solution about 7. The solid-liquid separation is performed, and the phosphorus concentration in the water is measured. The phosphorus concentration in the water is measured to be 0.01 mg / L, which meets the wastewater discharge requirements.

[0095] (9) Practical application of the adsorbent material of the present invention 3

[0096] This experiment is the application of the adsorption material in phosphorus-containing groundwater: a certain phosphorus-containing groundwater, the phosphorus concentration is 0.63 mg / L, pH is 6.8; take 250mL of the water, add 1g of the oyster shell @ La (OH) 3 composite material prepared in Example 1, and shake it in a constant temperature shaker for 3h. During this period, the pH of the solution is adjusted with dilute HCl so that the final pH of the solution is about 7. The solid-liquid separation is carried out, and the phosphorus concentration in the water is measured. The measured phosphorus concentration in the water is 0.025mg / L, which meets the drinking water standard.

[0097] The oyster shell @La(OH)3 adsorbent prepared in Examples 2 to 3 was tested according to the methods shown in (2) to (9) in the test examples. The test results were similar to those of the oyster shell @La(OH)3 adsorbent prepared in Example 1, and both showed good adsorption performance for phosphorus, fast adsorption rate, good cycle performance, high phosphorus removal rate and good stability.

[0098] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. An oyster shell-lanthanum hydroxide composite material, characterized in that The invention comprises oyster shell powder and lanthanum hydroxide particles loaded on the oyster shell powder.

2. The oyster shell-lanthanum hydroxide composite material according to claim 1, characterized in that The mass fraction of lanthanum hydroxide particles in the oyster shell-lanthanum hydroxide composite material is 10-80%.

3. The method for preparing the oyster shell-lanthanum hydroxide composite material according to claim 1 or 2, characterized in that: The following steps are involved: The lanthanum salt solution and the oyster shell powder suspension are mixed to obtain a mixed solution; The alkaline solution and the mixed solution are mixed, aged and centrifuged to obtain the oyster shell-lanthanum hydroxide composite material.

4. The preparation method according to claim 3, characterized in that: The lanthanum salt in the lanthanum salt solution includes one or more of lanthanum nitrate, lanthanum chloride and lanthanum sulfate; the lanthanum salt solution contains lanthanum nitrate, lanthanum chloride and lanthanum sulfate. 3+ The concentration is 0.05~1.2mol / L; The concentration of the oyster shell powder suspension is 5 to 30 g / L; the lanthanum salt solution contains La 3+ The mass ratio of oyster shell powder to the oyster shell powder suspension is 1:(0.2~3.5).

5. The preparation method according to claim 3, characterized in that: The lanthanum salt solution and the oyster shell powder suspension are mixed in the following manner: under stirring conditions, the lanthanum salt solution is added to the oyster shell powder suspension, and stirring is continued for 0.2 to 12 hours after the addition is completed.

6. The preparation method according to claim 3, characterized in that: The alkali in the alkaline solution is an inorganic strong alkali solution or ammonia water; the solvent of the inorganic strong alkali solution is water, ethanol or an ethanol-water mixed solvent; the concentration of the alkaline solution is 0.2-5 mol / L.

7. The preparation method according to claim 3, characterized in that: The alkaline solution and the mixed solution are mixed in a manner of: adding the alkaline solution into the mixed solution under stirring conditions.

8. The preparation method according to claim 7, characterized in that: The alkaline solution is added by dripping, injecting or pouring. When the addition method is dripping, the pH value of the system is controlled to be 9-12 during the dripping process, and stirring is continued for 0.2-5h after the dripping is completed.

9. The preparation method according to claim 3, characterized in that: The aging time is 1 to 24 hours.

10. Use of the oyster shell-lanthanum hydroxide composite material according to claim 1 or 2 or the oyster shell-lanthanum hydroxide composite material prepared by the preparation method according to any one of claims 3 to 9 in phosphorus removal from water.