Light energy adsorption material with broad-spectrum absorption, preparation method and application
By combining nano-scale Ti2O3 and carbon particles with agate vines, a photoenergy adsorption material with broad spectrum absorption is formed, which solves the problems of resource loss and environmental pollution in traditional seawater desalination methods, and improves the absorbance and photothermal conversion of the evaporator Efficiency, achieving efficient seawater desalination effect.
Patent Information
- Application Number
- CN202411193140.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-08-28
AI Technical Summary
Traditional seawater desalination methods have problems such as large resource loss, serious environmental pollution, high maintenance costs and low absorbance. In particular, evaporators using semiconductor materials have low absorbance and low photothermal conversion efficiency of carbon-based materials.
Using a light energy adsorption material with broad spectrum absorption, it is coated on agate vine by grinding commercial Ti2O3 powder into nano-scale particles and mixing with nano-scale carbon particles, combining polyvinyl alcohol and polydimethylsiloxane. On the surface, a hydrophobic layer is formed to improve the light absorption performance and photothermal conversion efficiency of photothermal materials.
It significantly improves the photothermal conversion efficiency and absorbance, reduces heat energy loss, enhances the evaporation performance and salt resistance of the evaporator, and achieves efficient seawater desalination.
Smart Images

Figure CN119081480A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of light energy absorption materials, and in particular relates to a light energy absorption material with broad-spectrum absorption, a preparation method and an application thereof. Background Art
[0002] Water is one of the most abundant resources on Earth, covering three-quarters of the Earth's surface, but about 97% of it is salt water and only 3% is fresh water, suitable for humans, plants and animals. In recent decades, the excessive population growth, industrial development and improved living standards have brought the world's demand for fresh water to an unprecedented level. Seawater desalination is one of the important ways to solve the current shortage of freshwater resources. The fresh water produced by this technology can not only be used for urban water, but also for a variety of industrial water. At present, traditional seawater desalination methods include: reverse osmosis, low multi-effect, multi-stage flash evaporation, electrodialysis, compressed steam distillation, dew point evaporation, water and power cogeneration, etc. These methods can be roughly divided into two categories: distillation and membrane. Among them, reverse osmosis (RO), multi-stage flash evaporation (MSF) and multi-effect distillation (MED) are the mainstream methods in the world and have been commercialized. In the distillation method, the heating method can be divided into bottom heating, volume heating and interface heating. Compared with the first two, interface heating concentrates the heat on the surface of the water body, reducing heat loss and the use of photothermal materials. For interfacial heating, the selection of water transport materials and photothermal materials is particularly important. The water transport material should have the ability to quickly transfer the bottom water to the upper surface of the evaporator. In addition to preparing other pore structures such as hydrogels with many vertical pores, some biomass materials can also be selected. Wood, bamboo, and rattan also have a large number of tiny vertical channels with large capillary pressure, which can effectively transport water vertically. Photothermal materials can effectively absorb solar energy and convert it into heat energy. When sunlight shines on the surface of the material, part of the sunlight is absorbed by it, and the other part is re-reflected to the environment. The absorbed solar energy is stimulated to generate heat energy. Part of this heat energy is used to evaporate surface water, and the other part will be lost in various forms. Excellent photothermal materials will minimize the loss of heat energy and use most of it for water evaporation. At the same time, they have a relatively wide range of absorption of the solar spectrum. Photothermal materials usually include carbon-based materials, metal materials, polymer materials, semiconductor materials, etc. The selection of different photothermal materials will also make the light absorption performance of the evaporator different.
[0003] At present, desalination technology often requires a large amount of electrical energy or chemical energy. At the same time, the maintenance, installation and operation costs of the equipment are high, and there are problems such as large resource loss, serious environmental pollution and high maintenance costs. At the same time, the traditional evaporator made of semiconductor as the light-absorbing layer has the problem of low absorbance, while the evaporator made of carbon-based materials has the problem of low light-to-heat conversion efficiency. Summary of the invention
[0004] In view of the deficiencies in the prior art, the present invention provides a light energy absorption material with broad-spectrum absorption, a preparation method and an application thereof.
[0005] The purpose of the present invention can be achieved through the following technical solutions:
[0006] A method for preparing a light energy absorption material with broad spectrum absorption, the preparation method comprising the following steps:
[0007] S1, placing commercial Ti2O3 powder into a ball mill for ball milling to obtain nano-sized Ti2O3 particles;
[0008] S2, mixing nano-sized Ti2O3 particles and nano-sized carbon particles, adding anhydrous ethanol, stirring evenly and then drying in an oven to obtain mixed particles;
[0009] S3, adding polyvinyl alcohol to deionized water, heating to completely dissolve it, and then cooling it to room temperature to obtain a polyvinyl alcohol solution, and evenly coating the polyvinyl alcohol solution on the surface of the treated agate vine block; and then spraying the mixed particles on the surface of the agate vine block;
[0010] S4. Coat polydimethylsiloxane on the surface of the agate vine block sprayed with the mixed particles, irradiate it with a UV lamp, and then take it out and place it in a drying oven to dry it to obtain a hydrophobic surface.
[0011] Furthermore, in step S1, the particle size of the steel balls in the ball mill is 5-10 mm, the ball milling time is 24 h, the rotation speed is 400 r / min, and the rest time is 10 min.
[0012] Furthermore, in step S2, the mass ratio of the nano-sized Ti2O3 particles to the nano-sized carbon particles is 3 to 5:1.
[0013] Furthermore, the concentration of the polyvinyl alcohol solution prepared in step S3 is 0.8-1.5 g / ml.
[0014] Furthermore, the diameter of the agate vine block processed in step S3 is 20 mm, and the thickness is 10 mm; the agate vine block needs to be polished with sandpaper before being coated with the polyvinyl alcohol solution.
[0015] Furthermore, in step S3, the coating amount of the polyvinyl alcohol solution is 0.05-0.1 g; the spraying amount of the mixed particles is 0.3-0.5 g; when spraying the mixed particles, the fixed spraying time is 7-10 s, the spraying distance is 5-6 mm, and the voltage is 15-20 KV.
[0016] Furthermore, in step S4, the coating amount of polydimethylsiloxane is 0.05 to 0.1 g.
[0017] Furthermore, in step S4, the wavelength of the UV lamp is 365 nm and the intensity is 2.6 mW·cm -2 The irradiation time is 2 to 3 hours.
[0018] A light energy absorption material with broad spectrum absorption is prepared by the above-mentioned method for preparing a light energy absorption material with broad spectrum absorption.
[0019] The above-mentioned light energy absorption material with broad spectrum absorption is used as a substrate to manufacture a solar evaporator. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0021] Figure 1 The middle part is the preparation process of nano-sized Ti2O3 particles and mixed particles;
[0022] Figure 2 (a) is an X-ray diffraction pattern of the prepared Ti2O3 nanoparticles; (b) is a SEM image of the prepared Ti2O3 nanoparticles;
[0023] Figure 3 The morphology and microstructure of natural agate vine;
[0024] Figure 4 (a) shows the microscopic and macroscopic structures of the surface of rattan material loaded with C nanoparticles; (b) shows the microscopic and macroscopic structures of the surface of rattan material loaded with Ti2O3 nanoparticles; (c) shows the microscopic and macroscopic structures of the surface of rattan material loaded with mixed nanoparticles; (d) shows the side view of the array structure and the micro-nanostructure on it;
[0025] Figure 5 (a) is the absorbance and solar spectrum irradiance of the surface of Rr, Tr, Cr and TC-r rattan materials; (b) is the XPS measurement spectrum of Rr, TC-r and TCP-r; (c) is the FTIR spectrum of TC-r and TCP-r; (d) is the thermal conductivity of different biomass materials; (e) is the water contact angle of the original rattan material and the rattan material loaded with photothermal materials; (f) is the capillary performance of the natural agate rattan slice along the growth direction;
[0026] Figure 6is the evaporation performance of the solar evaporator; (a) is the mass change of Rr, Cr, Tr, TC-r, TCP-r and the mass change of pure water over time when working under one sun; (b) is the evaporation enthalpy of pure water and water in the evaporator in the dark; (c) is the evaporation enthalpy of pure water and water in the evaporator under one sun; (d) is the comparison of the evaporation rate and photothermal conversion efficiency of the evaporator and other carbon-based materials or biomass material evaporators under one sun; (e) is the surface temperature of Rr, Cr, Tr, TC-r and TCP-r under one sun and the corresponding infrared images, showing the temperature distribution when the irradiation time is 0, 180, 360 and 540s respectively;
[0027] Figure 7 (a) is the ambient humidity, temperature and solar power during the outdoor solar evaporation experiment; (b) is the evaporation rate of Tr, Cr and TCP-r at different time of day; (c) is the evaporation rate of TCp-r in pure water for 10 cycles under 1 sun illumination, and the inset shows the change of the mass of the system with time during the 1st and 10th cycles;
[0028] Figure 8 is the salt tolerance of the solar evaporator; (a) is the evaporation rate of TCP-r in NaCl solutions of different salinities; the inset shows the top surface of the evaporator after 10 hours; (b) is the evaporation rate of TCP-r in 10.0wt% different salt solutions and simulated seawater; (c) is the concentration of the four main ions in the solutions collected before and after evaporation of 10.0wt% different salt solutions and simulated seawater by TCP-r; (d) is the desalination performance of TC-r and TCP-r after 0, 3, and 5 days of desalination in simulated seawater. DETAILED DESCRIPTION
[0029] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0030] Example 1
[0031] A method for preparing a light energy absorption material with broad spectrum absorption, the preparation method comprising the following steps:
[0032] S1. Commercial Ti2O3 powder is placed in a ball mill for ball milling to obtain nano-sized Ti2O3 particles; the particle size of the steel balls in the ball mill is 5 mm, the ball milling time is 24 h, the rotation speed is 400 r / min, and the rest time is 10 min.
[0033] S2. Mix nano-sized Ti2O3 particles and nano-sized carbon particles, add anhydrous ethanol, stir evenly and then put into an oven to dry to obtain mixed particles; the mass ratio of nano-sized Ti2O3 particles to nano-sized carbon particles is 3:1.
[0034] S3. Add polyvinyl alcohol to deionized water, heat it to completely dissolve it, and then cool it to room temperature to obtain a polyvinyl alcohol solution, and evenly apply the polyvinyl alcohol solution on the surface of the treated agate vine block; then spray the mixed particles on the surface of the agate vine block; the concentration of the prepared polyvinyl alcohol solution is 0.8g / ml; the diameter of the treated agate vine block is 20mm; the thickness is 10mm; the agate vine block needs to be polished with sandpaper before coating with the polyvinyl alcohol solution; the coating amount of the polyvinyl alcohol solution is 0.05g; the spraying amount of the mixed particles is 0.3g; when spraying the mixed particles, the fixed spraying time is 7s, the spraying distance is 5mm, and the voltage is 15KV.
[0035] S4, coating polydimethylsiloxane on the surface of the agate vine block sprayed with the mixed particles, irradiating it with a UV lamp, and then taking it out and drying it in a drying oven to obtain a hydrophobic surface; a light energy absorption material with broad spectrum absorption is prepared. The coating amount of polydimethylsiloxane is 0.05g; the wavelength of the UV lamp is 365nm and the intensity is 2.6mW·cm -2 , the irradiation time is 2h.
[0036] Comparative Example 1
[0037] Compared with Example 1, Comparative Example 1 uses ordinary commercial Ti2O3 powder, and the commercial Ti2O3 powder is not ball-milled; the other steps are the same as Example 1, and a light energy absorption material with broad-spectrum absorption is prepared.
[0038] Comparative Example 2
[0039] Compared with Example 1, in Comparative Example 2, nano-scale carbon particles and nano-scale Ti2O3 particles are not mixed in step S2, that is, nano-scale carbon particles are missing in step S2; other steps are the same as Example 1, and a light energy absorption material with broad-spectrum absorption is prepared.
[0040] The X-ray diffraction pattern of commercial Ti2O3 powder after ball milling can well indicate the corundum phase ( Figure 2 a). Representative scanning electron microscopy (SEM) images of the prepared Ti2O3 nanoparticles show that the average diameter is about 450nm ( Figure 2 b);
[0041] The pore size of rattan wood is very important for water transport. It can be seen in the figure that rattan wood has a large number of longitudinal tiny vertical channels. The diameter of the metaxylem vessels is about 300-350μm. The wider diameter of the vessels allows for adequate water supply. The slender protoxylem vessels and sieve tubes surround the metaxylem vessels. Compared with the metaxylem vessels, they are narrower in structure and smaller in size, with a diameter of 50-70μm. This slender vertical channel is arranged axially, which helps the vertical transport of water. In addition, the numerous pits arranged on the cell wall can serve as horizontal channels for salt exchange, with a height of usually 0.5-1.5μm and a width of usually 3-5μm.
[0042] Ti2O3 nanoparticles have high hydrophilicity and are more easily dispersed in PVA when sprayed on the surface of rattan materials. Therefore, they can be more evenly dispersed on the surface of rattan materials. Nanocarbon has weaker hydrophilicity than Ti2O3 and is usually less dispersed than Ti2O3 nanoparticles on the surface of rattan materials coated with PVA. Figure 4 As shown in Figure b, the surface formed by Ti2O3 nanoparticles is relatively smooth under the microscopic view. The addition of nanocarbon reduces the dispersion of Ti2O3 powder to a certain extent, making the coating surface rough. During the cutting process, there is still a trace amount of tissue remaining around the vascular bundle, so that after the mixed powder is sprayed, a uniform and dense array structure with a diameter of about 200μm and a height of about 200μm is formed on the periphery of the catheter. Due to the increase in roughness, the array surface appears in the shape of many micro-nano clusters. This micro-nano structure increases the light absorption area, reduces the surface reflectivity, and prolongs the residence time of sunlight inside the material, thereby enhancing the interaction between light and material and improving the photothermal conversion efficiency and absorbance ( Figure 4 ).
[0043] As a semiconductor with an extremely narrow band gap, Ti2O3 has a high light-to-heat conversion efficiency and shows higher absorbance than carbon in the ultraviolet and visible light bands. The absorbance of Tr in the wavelength range of 500-2500nm reaches 90.03%, but its absorbance in the near-infrared band shows a relatively obvious downward trend, and is also much smaller than the absorbance of Cr in the near-infrared band. The absorbance of Cr reaches 93.12%. The synergistic effect produced by the uniform mixing of the two makes up for their respective defects in different bands. There is no obvious downward trend in its light absorption capacity in the near-infrared band. The absorbance of TC-r reaches 95.92% ( Figure 5 a). In addition, we used XPS to characterize the chemical composition of unprocessed rattan, rattan with mixed particles attached, and rattan with a hydrophobic layer attached. The Ti content of rattan increased significantly after the Ti2O3 nanoparticles were attached. The attachment of the hydrophobic layer made the Si content reach 10.15%, while the Ti content decreased to 5.82% ( Figure 5b). FTIR was used to characterize the functional group changes of the original rattan material before and after the attachment of Ti2O3 nanoparticles and hydrophobic layer. Ti-O-Ti bonds appeared in both TC-r and TCP-r, and a large number of silicon-based functional groups appeared in TCP-r ( Figure 5 c). During the operation of the evaporator, the thermal conductivity of agate vine is relatively low, only 0.23 W·m -2 ·K -1 This reduces the heat loss to the surrounding water during evaporation, and the thermal conductivity of the treated rattan material is only slightly increased, which is 0.26 W·m -2 ·K -1 and 0.28W·m -2 ·K -1 , which is lower than the thermal conductivity of other biomass materials ( Figure 5 d). After the hydrophobic treatment of TC-r, its water contact angle increased from 73.9° to 131.2°, which laid the foundation for its salt resistance. The hydrophobic angle of Tr was only 54.8°, slightly higher than that of Rr. Due to the partial hydrophobicity of carbon particles, the hydrophobic angle of Cr reached 70.9° ( Figure 5 e). The rapid water transfer of agate vine is due to its large capillary force. In the dyeing experiment, the red dye rose to the top of the semicircular vine with a thickness of 1 mm in only 3 seconds, and the flow rate was about 3.4 mm·s -1 , while the non-porous fir is only 0.5mm·s -1 ( Figure 5 f).
[0044] The change in mass over time during the operation of the evaporator often reflects the performance of the evaporator. The evaporation rate can be calculated by fitting the slope of the mass-time curve. In general, the evaporation rate of Rr is 0.55 Kg·m -2 ·h -1 The evaporation rates of Tr and Cr increased significantly, reaching 2.02 Kg·m -2 ·h -1 and 1.97Kg·m -2 ·h -1 The evaporation rate of TC-r obtained by mixing the two powders in a certain proportion increased significantly on this basis, reaching 2.35Kg·m -2 ·h -1 The evaporation rate of TCP-r obtained by hydrophobic treatment of TC-r was slightly increased to 2.39 Kg·m -2 ·h -1 ( Figure 6 a). Figure 6 b and Figure 6c shows the evaporation enthalpy of pure water and the system consisting of evaporator and water under dark conditions and one sun illumination conditions respectively (the name of the system consisting of evaporator and water is replaced by the abbreviation of the treatment of Houtou material). At room temperature, the evaporation enthalpy of pure water is 2.44 MJ·kg -1 , Rr is 1.90MJ·kg -1 The evaporation enthalpy of the treated rattan material decreased to 1.39 and 1.42 MJ·kg-1 for Tr and Cr respectively, and the evaporation enthalpy of TC-r decreased slightly to 1.30 MJ·kg -1 After the hydrophobic layer was applied, the evaporation enthalpy did not change significantly, and TCP-r was 1.32 MJ·kg -1 Under one sun, as the temperature increases, the evaporation enthalpy decreases further, and the evaporation enthalpy of Tr and Cr decreases to 1.37 and 1.39 MJ·kg -1 , the evaporation enthalpy of TC-r dropped to 1.27 MJ·kg -1 , the evaporation enthalpy of TCP-r dropped to 1.29 MJ·kg -1 , the evaporation enthalpy is closely related to the photothermal conversion efficiency, and they can usually be related by the following equation:
[0045]
[0046] in is the net evaporation rate, which can be calculated based on the evaporation rate under one sun and the evaporation rate in darkness, h LV is the phase change enthalpy of liquid to vapor, including sensible heat (h sh ) and enthalpy of evaporation (h ee ),C opt is the optical concentration, and P0 is the solar radiation of one sun. Figure 6 As shown in Figure d, the final product TCP-r showed a photothermal conversion efficiency of 93.5%, which is comparable to the photothermal conversion efficiency of other carbon-based materials or biomass material evaporators reported by other researchers, and its evaporation rate is also among the best. In addition, under the irradiation of one sun, the temperature of Rr slowly rose to 34.2°C within 600s. Due to the presence of semiconductor Ti2O3, the temperature of Tr, TC-r, and TCP-r rose rapidly, reaching quasi-steady states of about 43.8°C, 43.7°C, and 44.9°C at 540s, respectively. Cr stabilized at about 40.8°C at 540s.
[0047] In practical applications, sunlight is not always perpendicular to the upper surface of the evaporator. As time goes by, the incident light changes from 0° at sunrise to 90° at noon and then to 0° at sunset. Most of the time, the angle between the incident light and the evaporator is less than 90°. Here, we conducted an outdoor evaporation experiment to study the evaporation performance of the evaporator in practical applications. The experiment was conducted on a typical sunny day in Nanjing, Jiangsu Province (24°32′N, 117°22′E). The ambient humidity, temperature and solar power ( Figure 7 a) The average solar flux measured outdoors is 0.62 kW·m -2 The evaporation rate measured during this period was lower than that measured under ideal conditions in the laboratory. The evaporation rate of TCP-r was 0.92 kg·m at 6 am. -2 ·h -1 , 1.72Kg·m at 12 noon -2 ·h -1 From 12:00 noon to 15:00 p.m., the evaporation rate was maintained at 1.70 kg·m -2 ·h -1 above, and gradually decreased to 1.43Kg·m at 18:00 -2 ·h -1 The evaporation rate of Tr and Cr can only be maintained at 1.3 kg·m from 12:00 to 15:00 in the afternoon. -2 ·h -1 The evaporation rate of Tr at 12 o'clock reached 1.35 Kg·m -2 ·h -1 The evaporation rate of Cr is only 1.3 Kg·m at 12 noon. -2 ·h -1 ( Figure 7 b). In addition, the average evaporation rate of TCP-r reached 1.53 Kg·m -2 ·h -1 The average evaporation rate of Tr is 1.15 Kg·m -2 ·h -1 The average evaporation rate of Cr is only 1.13 Kg·m -2 ·h -1 The synergistic effect of the mixed particles makes TCP-r still have a relatively stable and high evaporation rate in practical applications. Figure 7 c shows the change in evaporation rate of the final product TCP-r during 10 cycles of evaporation experiments (each cycle includes 12 hours in the dark and 12 hours in the sun), and the inset shows the change in mass over time between the 1st and 10th cycles, where the maximum evaporation rate difference between single cycles is only 3%, ensuring the stability of the evaporator under long-term operation.
[0048] In practical applications, ensuring the long-term salt resistance of the evaporator plays a vital role in continuous solar desalination. Excessive salt deposition significantly reduces the light absorption capacity of the evaporator's light-absorbing layer. In addition, it will block the conduit, making it difficult to replenish water, resulting in a serious decrease in the evaporation rate. The introduction of the hydrophobic layer significantly reduces the hydrophilicity of the surface of the light-absorbing layer. After the salt is enriched on the surface of the hydrophobic layer, it is sent back to the bulk solution due to the concentration gradient. Since the surface temperature of the evaporator is much higher than that of the bulk solution, the redissolution of the salt is accelerated. Figure 8 a shows the evaporation rate of TCP-r in NaCl solutions with different salinities. The evaporation rate of TCP-r in 3.5wt% and 10wt% NaCl solutions is stable at 2.02Kg·m -2 ·h -1 and 1.91Kg·m -2 ·h -1 When the concentration increased to 15wt%, the evaporation rate of TCP-r did not decrease significantly and could still be maintained at 1.70Kg·m -2 ·h -1 When the concentration further increased to 20wt%, the evaporator performance did not decrease significantly in the first four hours and remained at 1.40Kg·m -2 ·h -1 In the fourth hour, salt began to deposit. Due to the high concentration of the salt solution, the deposition rate began to exceed the dissolution rate. As the deposition area increased, the evaporation rate gradually decreased. By the tenth hour, the evaporation rate was only 0.78 kg·m -2 ·h -1 , the illustration shows that the light-absorbing surface of the evaporator is almost covered by salt. After evaporation tests of various types of 10wt% salt solutions, TCP-r can stably exert its evaporation performance without obvious salt deposition. For 10wt% KCl solution, the evaporation rate of TCP-r can be stabilized at 1.80Kg·m -2 ·h -1 For 10.0wt% Na2SO4, it can also be stabilized at 1.72Kg·m -2 ·h -1 However, its evaporation rate in MgSO4 and CaCl2 is lower, about 1.66 and 1.58 Kg·m -2 ·h -1 In simulated seawater, the evaporation rate of TCP-r is about 1.98 Kg·m -2 ·h -1 ( Figure 8 b). In addition, we measured the ion concentrations of the solutions collected before and after evaporation of various 10 wt% salt solutions from TCP-r ( Figure 8c), the ion concentration of the distilled water collected was greatly reduced, which is far below the drinking water limit of the World Health Organization (WHO), China National Standard (GBT) and the US Environmental Protection Agency (EPA), and the desalination rate exceeded 99%. In addition, in a comparative experiment, we evaporated TC-r and TCP-r in simulated seawater for 5 days ( Figure 8 d), On the third day, more salt deposits appeared in TC-r, and on the fifth day, the salt almost covered the surface of the light-absorbing layer, while TCP-r still had no obvious crystallization phenomenon on the fifth day.
[0049] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0050] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, and these changes and improvements all fall within the scope of the present invention to be protected.
Claims
1. A method for preparing a light energy absorption material with broad spectrum absorption, characterized in that: The preparation method comprises the following steps: S1, placing commercial Ti2O3 powder into a ball mill for ball milling to obtain nano-sized Ti2O3 particles; S2, mixing nano-sized Ti2O3 particles and nano-sized carbon particles, adding anhydrous ethanol, stirring evenly and then drying in an oven to obtain mixed particles; S3, adding polyvinyl alcohol to deionized water, heating to completely dissolve it, and then cooling it to room temperature to obtain a polyvinyl alcohol solution, and evenly coating the polyvinyl alcohol solution on the surface of the treated agate vine block; and then spraying the mixed particles on the surface of the agate vine block; S4. Coat polydimethylsiloxane on the surface of the agate vine block sprayed with the mixed particles, irradiate it with a UV lamp, and then take it out and place it in a drying oven to dry it to obtain a hydrophobic surface.
2. The method for preparing a light energy absorption material with broad spectrum absorption according to claim 1, characterized in that: In step S1, the particle size of the steel balls in the ball mill is 5-10 mm, the ball milling time is 24 h, the rotation speed is 400 r / min, and the rest time is 10 min.
3. The method for preparing a light energy absorption material with broad spectrum absorption according to claim 1, characterized in that: In step S2, the mass ratio of nano-sized Ti2O3 particles to nano-sized carbon particles is 3-5:
1.
4. The method for preparing a light energy absorption material with broad spectrum absorption according to claim 1, characterized in that: The concentration of the polyvinyl alcohol solution prepared in step S3 is 0.8-1.5 g / ml.
5. The method for preparing a light energy absorption material with broad spectrum absorption according to claim 1, characterized in that: The diameter of the agate vine block processed in step S3 is 20 mm, and the thickness is 10 mm. The agate vine block needs to be polished with sandpaper before being coated with the polyvinyl alcohol solution.
6. The method for preparing a light energy absorption material with broad spectrum absorption according to claim 1, characterized in that: In step S3, the coating amount of the polyvinyl alcohol solution is 0.05-0.1 g; the spraying amount of the mixed particles is 0.3-0.5 g; when spraying the mixed particles, the fixed spraying time is 7-10 s, the spraying distance is 5-6 mm, and the voltage is 15-20 KV.
7. The method for preparing a light energy absorption material with broad spectrum absorption according to claim 1, characterized in that: The coating amount of polydimethylsiloxane in step S4 is 0.05-0.1 g.
8. The method for preparing a light energy absorption material with broad spectrum absorption according to claim 1, characterized in that: The wavelength of the UV lamp in step S4 is 365nm and the intensity is 2.6mW·cm -2 The irradiation time is 2 to 3 hours.
9. A light energy absorption material with broad spectrum absorption prepared by the preparation method of a light energy absorption material with broad spectrum absorption according to any one of claims 1 to 8.
10. The light energy absorption material with broad spectrum absorption as claimed in claim 9 is used as a substrate for manufacturing a solar evaporator.
Citation Information
Patent Citations
Super-hydrophobic low-adhesion material with photo-thermal and photocatalytic synergistic effect as well as preparation method and application of super-hydrophobic low-adhesion material
CN115748232A
Multifunctional particulate material, fluid, and composition
US20040105980A1
Polymeric composites with functional surfaces
US20190091950A1
Omniphobic antimicrobial microparticles and compositions thereof
WO2024077382A1