Preparation method of DNA origami crystal for regulating and controlling morphology of loaded nanoparticles
By regulating the morphology of nanoparticles in the octahedral of DNA origami, the problem of loading of large-size or anisotropic nanoparticles is solved, and the diversified morphology transformation and environmental responsiveness of nanoparticles are achieved, which promotes DNA origami technology in micro-nano Applications in the field of devices.
Patent Information
- Application Number
- CN202411194337.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-12-06
AI Technical Summary
The existing DNA origami technology is difficult to load large-sized or anisotropic nanoparticles in the octahedral of DNA origami, and cannot effectively regulate the morphology of the nanoparticles, limiting the environmental responsiveness of signal output.
By preparing DNA origami elongated octahedral frame structure, connecting gold nanoparticles, carrying out silica coating and high-temperature calcination, the morphology of the nanoparticles is controlled, thereby realizing the transformation of the nanoparticles into dumbbell, rod-shaped and spherical shapes, and The gold-silver rod-shaped alloy nanoparticles were synthesized through silver growth agent.
The orderly periodic nanoparticle assembly in DNA origami crystals is realized, which enhances the environmental responsiveness and diversified morphological selection of nanoparticles, and provides a platform for building micro-nano devices with special functions.
Smart Images

Figure CN119082101A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of biotechnology, and in particular to a method for preparing a DNA origami crystal capable of regulating the morphology of loaded nanoparticles. Background Art
[0002] DNA origami technology is an important branch of DNA nanotechnology. DNA strictly follows the principle of base complementarity, and the base and phosphate backbone are conducive to chemical modification, which makes it have important application space in nanoparticle modification and self-assembly. DNA origami technology uses a long chain of DNA and hundreds of short chains of DNA for self-assembly. The constructed DNA origami monomer can reach nearly 100 nanometers, which can load colloidal-scale functional nanoparticles for highly ordered crystal assembly. DNA origami octahedron was first proposed by Tian Ye et al. in 2015 (article: Nature Nanotechnology, 2015, 10 (7): 637 44.), and in 2020, the three-dimensional nanoparticle superlattice construction of DNA origami octahedron with internal nanoparticles was realized (article: Nature Materials, 2020, 19: 789-796.). The efficient loading and diversified crystal assembly of gold nanoparticles were successfully achieved, providing a platform for the realization of micro-nano devices with special optical, electrical and magnetic signals.
[0003] However, to achieve effective signal output, the size of nanoparticles in the existing assembly needs to be further increased, and anisotropic nanoparticles need to be introduced so that the output signal can change accordingly according to environmental changes. However, due to the size limitation of the DNA origami octahedron itself, large-sized nanoparticles cannot be directly placed. In addition, it is also difficult to modify the surface DNA of anisotropic rod-shaped nanoparticles and directly place them. Therefore, it is necessary to indirectly regulate the morphology of the loaded particles and load the rod-shaped nanoparticles in the DNA origami octahedron.
[0004] Currently, there is a lack of a method to prepare DNA origami crystals that can regulate the morphology of loaded nanoparticles. Summary of the invention
[0005] In order to overcome the deficiencies in the prior art, the purpose of the present invention is to provide a method for preparing DNA origami crystals that regulate the morphology of loaded nanoparticles.
[0006] In order to achieve the above technical objectives, the technical solutions adopted by the present invention are as follows: In the first aspect, the present invention provides a method for preparing DNA origami crystals for regulating the morphology of loaded nanoparticles; in the second aspect, the present invention provides DNA origami crystals for regulating the morphology of loaded nanoparticles.
[0007] The first aspect of the present application provides a method for preparing a DNA origami crystal for regulating the morphology of loaded nanoparticles, comprising the following steps:
[0008] (1) Preparation of DNA origami elongated octahedral framework structure: The octahedral framework structure of DNA origami is synthesized by a M13mp18 scaffold chain, 136 DNA stapler chains, 8 DNA capture chains, and 24 DNA sticky end chains in a specific buffer solution through a 21-hour annealing process; the nucleotide sequence of the DNA origami monomer is as follows: SEQ NO. 1, 2, 3, 4, 5…192;
[0009] (2) Connecting gold nanoparticles to the DNA origami framework: The surface of the gold nanoparticles is modified with thiol DNA segments, which specifically bind to the DNA capture chain. After modification, the absorption peak intensity of the gold spheres at 520 nm is measured using UV-Vis to determine the concentration of the gold spheres; the gold spheres and the DNA origami framework are mixed in a ratio of 2:1, and annealed at a constant rate of 50-20°C for 33 hours to obtain a gold nanoparticle-DNA origami elongated octahedron composite structure;
[0010] (3) preparing a two-dimensional plane and performing in situ particle growth: including mixing the gold nanoparticle-DNA origami elongated octahedron composite structure with its complementary monomer and performing a slow cooling process;
[0011] (4) Silica coating: using structure-directing agents and inorganic silicon sources to coat silica;
[0012] (5) Tube furnace calcination: including calcination under argon protective gas, the calcination temperature is 400-550°C, and the time is 15-45 minutes to produce DNA origami crystals with regulated morphology of loaded nanoparticles.
[0013] Furthermore, in step (1), the nucleotide sequence of the DNA stapler chain is such as SEQ NO: 1, 2, 3, 4, 5...136; the nucleotide sequence of the capture chain is such as SEQ NO: 137, 138, 139,...144; the nucleotide sequence in the A base DNA sticky end chain is such as SEQ NO: 145, 146, 147,...168; the nucleotide sequence in the B base DNA sticky end chain is such as SEQ NO: 169, 170, 171,...192.
[0014] Furthermore, in step (1), when synthesizing the DNA origami elongated octahedron, its 8 DNA capture chains are divided into two groups, each with 4 chains, and are located in the upper and lower cavities of the DNA origami elongated octahedron. Each group can capture one gold nanoparticle, and the two groups can capture two gold balls in total.
[0015] Furthermore, in step (2), the density of thiol DNA modified on the surface of gold nanoparticles is low, and a salt aging method is required, with the addition amount of gold nanoparticles: thiol DNA being 1:100. The amount of gold nanoparticles added in the synthesis of gold nanoparticle-DNA origami octahedral composite structures far exceeds the required amount, so after the crystals are formed in step (3), it is necessary to remove the excess gold nanoparticles by washing the precipitate and replacing the supernatant.
[0016] Furthermore, in step (3), the amount of gold / silver growth agent added is proportional to the volume of the solution, with a ratio of 2, and to ensure uniform particle growth, the gold / silver growth agent is added in five times, and each time the reaction is carried out on a rotary mixer for 12 hours. After each growth, the precipitate needs to be cleaned to remove the unreacted growth agent.
[0017] Furthermore, in step (4), when the silica coating is performed, the thickness of the silica shell layer is changed according to the morphology of the target particles.
[0018] Furthermore, in step (5), when calcining in a tubular furnace, argon protective gas is required, the calcining temperature is 400-550° C., the calcining time is 15-45 min, and the mixture is cooled naturally.
[0019] Furthermore, in step (5), before calcination in a tubular furnace, when the DNA origami monolayer crystals wrapped with silica are deposited on a copper mesh, a pure carbon copper mesh with a single-layer film is used.
[0020] Furthermore, in step (5), when calcining in a tubular furnace is performed, the single crystal silicon wafer and the copper mesh need to be placed in a graphite crucible and then placed in the center of the tubular furnace.
[0021] The second aspect of the present application provides a DNA origami crystal with regulated morphology of loaded nanoparticles prepared by the method, wherein the crystal is loaded with nanoparticles with regulated morphology.
[0022] Beneficial effects: The present invention can regulate the morphology of nanoparticles in DNA origami crystals, and introduce anisotropic nanoparticles without being restricted by an external framework. In the process of regulating the morphology of nanoparticles, the present invention maintains the structure of the DNA origami crystals, so that the nanoparticles can still be arranged in an orderly periodic manner.
[0023] Compared with the prior art, the present invention has the following advantages:
[0024] (1) Diversity of morphology transformation: Through the process of silica coating and high-temperature calcination, the present invention can transform the morphology of nanoparticles from phase-dissociated dimers to dumbbells, rods and spheres, providing a variety of morphology options.
[0025] (2) Synthesis of functional nanoparticles: The present invention achieves the synthesis of gold-silver rod-shaped alloy nanoparticles through the addition of a silver growth agent and a calcination process, providing a new approach for preparing nanoparticles with special functions.
[0026] (3) Highly ordered crystal assembly: Using DNA origami technology, the present invention can achieve the orderly assembly of nanoparticles in DNA origami crystals, making it possible to construct highly ordered nanostructures.
[0027] (4) Environmental responsiveness: By regulating the morphology of nanoparticles, the present invention can make the output signal change accordingly according to environmental changes, thereby enhancing the environmental responsiveness of the nanoparticles.
[0028] (5) Technological innovation: The present invention provides a novel method to regulate the morphology of nanoparticles loaded in the DNA origami framework, solving the problem in the prior art of being unable to load large-sized or anisotropic nanoparticles.
[0029] (6) Application potential: The method of the present invention provides a platform for realizing micro-nano devices with special optical, electrical, and magnetic signals, and has broad application prospects, especially in the fields of biosensors, nanoelectronics, and materials science. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0031] Figure 1 This is a transmission electron microscope photograph of the ungrown DNA origami elongated octahedron-loaded nanogold double particles of the present invention.
[0032] Figure 2 This is a transmission electron microscope photograph of the DNA origami elongated octahedron loaded with nano-gold double particles that undergo in-situ gold growth according to the present invention.
[0033] Figure 3 Schematic diagram of the assembly of Example 1 of the present invention and a transmission electron micrograph of the crystal.
[0034] Figure 4 Schematic diagram of the assembly of Example 2 of the present invention and a transmission electron micrograph of the crystal.
[0035] Figure 5 Schematic diagram of the assembly of Example 3 of the present invention and a transmission electron micrograph of the crystal.
[0036] Figure 6 It is an assembly schematic diagram of comparative example 1 of the present invention and a transmission electron micrograph of the crystal.
[0037] Figure 7 Schematic diagram of the effect of calcination temperature on morphology of particles after in-situ growth and silica coating in the present invention. DETAILED DESCRIPTION
[0038] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present application more clearly understood, the present application is further described in detail in conjunction with the embodiments below. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.
[0039] In this application, the term "and / or" describes the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural. The character " / " generally indicates that the associated objects are in an "or" relationship.
[0040] The first aspect of the embodiment of the present application provides a method for preparing a DNA origami crystal for regulating the morphology of loaded nanoparticles, comprising the following steps:
[0041] (1) Preparation of DNA origami elongated octahedral framework structure: The DNA origami framework structure is synthesized by a M13mp18 scaffold chain, 136 DNA stapler chains, 8 DNA capture chains, and 24 DNA sticky end chains under a specific buffer solution through a 21-hour annealing procedure; (1) Preparation of DNA origami elongated octahedral framework structure: The octahedral framework structure of DNA origami is synthesized by a M13mp18 scaffold chain, 136 DNA stapler chains, 8 DNA capture chains, and 24 DNA sticky end chains under a specific buffer solution through a 21-hour annealing procedure; the nucleotide sequence of the DNA origami monomer is as shown in SEQ NO.1, 2, 3, 4, 5…192;
[0042] (2) Connecting gold nanoparticles to the DNA origami framework: The surface of the gold nanoparticles is modified with thiol DNA segments, which specifically bind to the DNA capture chain. After modification, the absorption peak intensity of the gold spheres at 520 nm is measured using UV-Vis to determine the concentration of the gold spheres; the gold spheres and the DNA origami framework are mixed in a ratio of 2:1, and annealed at a constant rate of 50-20°C for 33 hours to obtain a gold nanoparticle-DNA origami elongated octahedron composite structure;
[0043] (3) preparing a two-dimensional plane and performing in situ particle growth: including mixing the gold nanoparticle-DNA origami elongated octahedron composite structure with its complementary monomer and performing a slow cooling process;
[0044] (4) Silica coating: using structure-directing agents and inorganic silicon sources to coat silica;
[0045] (5) Tube furnace calcination: including calcination under argon protective gas, the calcination temperature is 400-550°C, and the time is 15-45 minutes to produce DNA origami crystals with regulated morphology of loaded nanoparticles.
[0046] In some embodiments, the nucleotide sequence of the DNA stapler strand is such as SEQ NOs: 1, 2, 3, 4, 5...136; the nucleotide sequence of the capture strand is such as SEQ NOs: 137, 138, 139,...144.
[0047] The 24 DNA sticky end chains are 24 A base DNA sticky end chains or 24 B base DNA sticky end chains.
[0048] The nucleotide sequence in the sticky end chain of the A base DNA is such as SEQ NO: 145, 146, 147, ... 168; the nucleotide sequence in the sticky end chain of the B base DNA is such as SEQ NO: 169, 170, 171, ... 192.
[0049] Nanoparticle size regulation: connect two small gold nanoparticles in the elongated octahedron of DNA origami, and increase the size of the two particles and reduce the distance between them by in situ growth; Nanoparticle morphology regulation: the grown dimer particles are coated with silica: fusion occurs at high temperature, resulting in morphological changes, and the shape changes from phase-separated dimer to dumbbell, rod and sphere.
[0050] In some embodiments, in step (1), when synthesizing the DNA origami elongated octahedron, its 8 DNA capture chains are divided into two groups, each with 4 chains, and are located in the upper and lower cavities of the DNA origami elongated octahedron. Each group can capture one gold nanoparticle, and the two groups can capture two gold balls in total.
[0051] In some embodiments, in step (2), the density of thiol DNA modified on the surface of gold nanoparticles is low, and a salt aging method is required, with the added amount of gold nanoparticles: thiol DNA being 1:100.
[0052] In some embodiments, in step (2), the amount of gold nanoparticles added to the synthesized gold nanoparticle-DNA origami octahedron composite structure far exceeds the required amount, so after the crystals are formed in step (3), it is necessary to remove excess gold nanoparticles by washing the precipitate and replacing the supernatant.
[0053] In some embodiments, in step (3), the amount of gold / silver growth agent added is proportional to the volume of the solution, with a ratio of 2, and to ensure uniform particle growth, the gold / silver growth agent is added in five times, and each time the growth agent is reacted on a rotary mixer for 12 hours. After each growth, the precipitate needs to be cleaned to remove the unreacted growth agent.
[0054] In some embodiments, in step (4), when silica coating is performed, the thickness of the silica shell layer is changed according to the morphology of the target particles.
[0055] In some embodiments, in step (5), when calcining in a tubular furnace, argon protective gas is required, the calcination temperature is 400-550° C., the calcination time is 15-45 min, and it is cooled naturally.
[0056] In some embodiments, in step (5), before the tube furnace calcination, when the DNA origami monolayer crystals wrapped with silica are deposited on the copper mesh, a pure carbon copper mesh with a single layer of film is used.
[0057] In some embodiments, in step (5), when calcining in a tube furnace is performed, the single crystal silicon wafer and the copper mesh need to be placed in a graphite crucible and then placed in the center of the tube furnace.
[0058] A second aspect of an embodiment of the present application provides a DNA origami crystal with regulated morphology of loaded nanoparticles obtained by the method, wherein the crystal is loaded with nanoparticles with regulated morphology.
[0059] Example 1
[0060] This embodiment is to adjust the morphology of nanoparticles loaded in the DNA origami framework to be dumbbell-shaped, including the following steps:
[0061] (1) Preparation of DNA origami elongated octahedron framework structure: A M13mp18 scaffold chain, 136 DNA stapler chains, 8 DNA capture chains, and 24 DNA sticky end chains were synthesized in a specific buffer solution through a 21-h annealing procedure to obtain a high yield of DNA origami elongated octahedron monomers with a concentration of about 10 nM.
[0062] (2) Connecting gold nanoparticles to the DNA origami framework: The surface of the gold nanoparticles is modified with a DNA segment with a thiol group (which can specifically bind to the DNA capture chain). After modification, the absorption peak intensity of the gold sphere at 520nm is measured using UV-Vis to determine the concentration of the gold spheres. The gold spheres and the DNA origami framework are mixed in a molar ratio of 2:1 and annealed at a constant rate of 50-20°C for 33h to obtain a gold nanoparticle-DNA origami elongated octahedron composite structure.
[0063] (3) Preparation of two-dimensional plane and in-situ particle growth: The prepared gold nanoparticle-DNA origami elongated octahedron composite structure is mixed with its complementary monomer in a 1:1 ratio and placed in a crystal incubator for a slow uniform cooling process to obtain a DNA origami single-layer plane with two gold balls connected in each monomer. A gold growth agent twice the volume of the solution is added to the obtained double gold ball origami plane solution to increase the particle size.
[0064] (4) Silica coating: The double gold sphere origami plane with increased particle size was washed and coated with silica using a structure-directing agent, N-trimethoxysilylpropyl-N,N,N-trimethylammonium chloride and an inorganic silicon source, tetraethyl orthosilicate. The amounts of reagents added were 0.2 μL and 0.16 μL, respectively.
[0065] (5) Tube furnace calcination: After silicon coating, the crystals are deposited on a copper mesh, dried, placed in a tube furnace, and calcined at 450 °C for 30 min to obtain a DNA origami monolayer plane whose particle morphology is transformed into dumbbell-shaped particles (two particles intersecting).
[0066] Example 2
[0067] The difference between Example 2 and Example 1 is that:
[0068] The present embodiment is to regulate the morphology of the nanoparticles loaded in the DNA origami framework to be rod-shaped, comprising the following steps: (1) preparing a DNA origami elongated octahedral framework structure: synthesizing an M13mp18 scaffold chain, 136 DNA stapler chains, 8 DNA capture chains, and 24 B-base DNA sticky end chains through a 21h annealing procedure in a specific buffer solution to obtain a high-yield DAN origami elongated octahedral monomer with a concentration of about 10nM.
[0069] (2) Connecting gold nanoparticles to the DNA origami framework: The surface of the gold nanoparticles is modified with a DNA segment with a thiol group (which can specifically bind to the DNA capture chain). After modification, the absorption peak intensity of the gold sphere at 520nm is measured using UV-Vis to determine the concentration of the gold spheres. The gold spheres and the DNA origami framework are mixed in a molar ratio of 2:1 and annealed at a constant rate of 50-20°C for 33h to obtain a gold nanoparticle-DNA origami elongated octahedron composite structure.
[0070] (3) Preparation of two-dimensional plane and in-situ particle growth: The prepared gold nanoparticle-DNA origami elongated octahedron composite structure is mixed with its complementary monomer in a 1:1 ratio and placed in a crystal incubator for a slow uniform cooling process to obtain a DNA origami single-layer plane with two gold balls connected in each monomer. A gold growth agent twice the volume of the solution is added to the obtained double gold ball origami plane solution to increase the particle size.
[0071] (4) Silica coating: The double gold sphere origami plane with increased particle size was washed and coated with silica using a structure-directing agent, N-trimethoxysilylpropyl-N,N,N-trimethylammonium chloride and an inorganic silicon source, tetraethyl orthosilicate. The amounts of reagents added were 0.2 μL and 0.16 μL, respectively.
[0072] (5) Tube furnace calcination: After silicon coating, the crystals were deposited on a copper mesh, dried, placed in a tube furnace, and calcined at 525 °C for 30 min to obtain a DNA origami monolayer plane with the particle morphology transformed into rod-shaped particles (aspect ratio of 2:1).
[0073] Example 3
[0074] The difference between Example 3 and Example 2 is that:
[0075] The present embodiment is to regulate the morphology of nanoparticles loaded in the DNA origami framework to be spherical, comprising the following steps: (1) preparing a DNA origami elongated octahedral framework structure: synthesizing an M13mp18 scaffold chain, 136 DNA stapler chains, 8 DNA capture chains, and 24 A-base DNA sticky end chains through a 21-hour annealing procedure in a specific buffer solution to obtain a high-yield DAN origami elongated octahedral monomer with a concentration of about 10 nM.
[0076] (2) Connecting gold nanoparticles to the DNA origami framework: The surface of the gold nanoparticles is modified with a DNA segment with a thiol group (which can specifically bind to the DNA capture chain). After modification, the absorption peak intensity of the gold sphere at 520nm is measured using UV-Vis to determine the concentration of the gold spheres. The gold spheres and the DNA origami framework are mixed in a molar ratio of 2:1 and annealed at a constant rate of 50-20°C for 33h to obtain a gold nanoparticle-DNA origami elongated octahedron composite structure.
[0077] (3) Preparation of two-dimensional plane and in-situ particle growth: The prepared gold nanoparticle-DNA origami elongated octahedron composite structure is mixed with its complementary monomer in a 1:1 ratio and placed in a crystal incubator for a slow uniform cooling process to obtain a DNA origami single-layer plane with two gold balls connected in each monomer. A gold growth agent twice the volume of the solution is added to the obtained double gold ball origami plane solution to increase the particle size.
[0078] (4) Silica coating: The double gold sphere origami plane with increased particle size was washed and coated with silica using a structure-directing agent, N-trimethoxysilylpropyl-N,N,N-trimethylammonium chloride and an inorganic silicon source, tetraethyl orthosilicate. The amounts of reagents added were 0.2 μL and 0.16 μL, respectively.
[0079] (5) Tube furnace calcination: After silicon coating, the crystals are deposited on a copper mesh, dried, and placed in a tube furnace. They are calcined at 550 °C for 45 min to obtain a DNA origami monolayer plane with a particle morphology transformed into a larger spherical shape (with a diameter 1.5 times the diameter of the double particles before calcination).
[0080] Comparative Example 1
[0081] The difference between Comparative Example 1 and Example 1 is that step (4) is not required.
[0082] In step (5), the DNA origami monolayer plane without silica coating is directly deposited on a copper mesh, dried, placed in a tube furnace, and calcined at 450° C. for 45 min.
[0083] In the comparative example, the ordered arrangement structure of the DNA origami monolayer plane was destroyed after calcination, and the size of the fused particles after calcination was inconsistent, with a very wide distribution range. However, the ordered arrangement structure of the DNA origami monolayer plane coated with silica was still maintained after calcination, and the particle size was uniform.
[0084] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, and the scope of protection of the present invention is defined by the attached claims, description and their equivalents.
Claims
1. A method for preparing DNA origami crystals for regulating the morphology of loaded nanoparticles. Features The steps include: (1) preparing a DNA origami elongated octahedral framework structure: the octahedral framework structure of the DNA origami is synthesized by a M13mp18 scaffold chain, 136 DNA stapler chains, 8 DNA capture chains, and 24 DNA sticky end chains in a specific buffer solution through a 21-hour annealing process; the nucleotide sequence of the DNA origami monomer is as SEQ NO. 1, 2, 3, 4, 5...192; (2) Connecting gold nanoparticles to the DNA origami framework: The surface of the gold nanoparticles is modified with thiol DNA segments, which specifically bind to the DNA capture chain. After modification, the absorption peak intensity of the gold spheres at 520 nm is measured using UV-Vis to determine the concentration of the gold spheres; the gold spheres and the DNA origami framework are mixed in a molar ratio of 2:1, and annealed at a constant rate of 50-20°C for 33 hours to obtain a gold nanoparticle-DNA origami elongated octahedron composite structure; (3) preparing a two-dimensional plane and performing in situ particle growth: including mixing the gold nanoparticle-DNA origami elongated octahedron composite structure with its complementary monomer and performing a slow cooling process; (4) Silica coating: using structure-directing agents and inorganic silicon sources to coat silica; (5) Tube furnace calcination: including calcination under argon protective gas, the calcination temperature is 400-550°C, and the time is 15-45 minutes to produce DNA origami crystals with regulated morphology of loaded nanoparticles.
2. The method for preparing DNA origami crystals for regulating the morphology of loaded nanoparticles according to claim 1, Features: In step (1), the nucleotide sequence of the DNA stapler chain is such as SEQ NO: 1, 2, 3, 4, 5...136; the nucleotide sequence of the capture chain is such as SEQ NO: 137, 138, 139,...144; the nucleotide sequence in the A base DNA sticky end chain is such as SEQ NO: 145, 146, 147,...168; the nucleotide sequence in the B base DNA sticky end chain is such as SEQ NO: 169, 170, 171,...
192.
3. The method for preparing DNA origami crystals for regulating the morphology of loaded nanoparticles according to claim 1, Features: In step (1), when synthesizing the DNA origami elongated octahedron, its 8 DNA capture chains are divided into two groups, 4 in each group, and are located in the upper and lower cavities of the DNA origami elongated octahedron. Each group can capture one gold nanoparticle, and the two groups can capture two gold balls in total.
4. The method for preparing DNA origami crystals for regulating the morphology of loaded nanoparticles according to claim 1, Features: In step (2), the density of thiol DNA modified on the surface of gold nanoparticles is low, and a salt aging method is required, with the added amount of gold nanoparticles: thiol DNA being 1:100; the amount of gold nanoparticles added in the synthesized gold nanoparticle-DNA origami octahedral composite structure far exceeds the required amount, so after the crystals are formed in step (3), it is necessary to remove excess gold nanoparticles by washing the precipitate and replacing the supernatant.
5. The method for preparing DNA origami crystals for regulating the morphology of loaded nanoparticles according to claims 1 and 4, Features: In step (3), the amount of gold / silver growth agent added is proportional to the volume of the solution, with a ratio of 2. In order to ensure uniform particle growth, the gold / silver growth agent is added in five times, and each time the reaction is carried out on a rotary mixer for 12 hours.
6. The method for preparing DNA origami crystals for regulating the morphology of loaded nanoparticles according to claim 1, Features: In step (4), when the silica coating is performed, the thickness of the silica shell layer is changed according to the morphology of the target particles.
7. The method for preparing DNA origami crystals for regulating the morphology of loaded nanoparticles according to claim 1, Features: In step (5), when calcining in a tubular furnace, argon protective gas is required, the calcination temperature is 400-550° C., the calcination time is 15-45 minutes, and the mixture is cooled naturally.
8. The method for preparing DNA origami crystals for regulating the morphology of loaded nanoparticles according to claim 1, Features: In step (5), before calcination in a tube furnace, when the DNA origami monolayer crystals wrapped with silica are deposited on a copper mesh, a pure carbon copper mesh with a single layer of film is used.
9. The method for preparing DNA origami crystals for regulating the morphology of loaded nanoparticles according to claim 1, Features: In step (5), when calcining in a tubular furnace, the single crystal silicon wafer and the copper mesh need to be placed in a graphite crucible and then placed in the center of the tubular furnace.
10. A DNA origami crystal with controlled morphology of loaded nanoparticles obtained by the method according to any one of claims 1 to 7, Features: The crystals are loaded with nanoparticles with controlled morphology.