Preparation method of aluminum-based nano composite material with molten salt added in high proportion and product
By stirring at 800°C to 850°C and dissolving in water, the problem of low nanoparticle content in the prior art was solved, and the preparation of high proportion of added aluminum-based nanocomposites was realized, which improved the material performance. Large-scale production provides important solutions.
Patent Information
- Application Number
- CN202411198726.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-12-06
AI Technical Summary
The content of nanoparticles in the existing aluminum-based nanocomposite preparation methods is relatively low, which limits the comprehensive performance of the material, making it difficult to prepare high-proportion added aluminum-based nanocomposite powder.
By mixing pure aluminum powder, nanoparticles, NaCl powder and KCl powder at 800℃-850℃, then breaking and fully dissolving in water, the chloride salt is removed by ultrasonic centrifugation technology to realize the molten salt system of nanoparticles in pure aluminum powder. The self-dispersion in the process makes a high proportion of aluminum-based nanocomposite material added.
The content of nanoparticles in aluminum-based nanocomposites has been successfully improved, the comprehensive performance of the materials has been improved, and an important method for large-scale production has been provided.
Smart Images

Figure CN119082533A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metal-based composite materials, and relates to a preparation method and product of a molten salt-assisted high-proportion addition aluminum-based nanocomposite material. Background Art
[0002] Aluminum-based nanocomposites are advanced composite materials that combine the excellent properties of aluminum and nanomaterials, making them widely used in the military, 3C and aerospace fields. First, aluminum-based nanocomposites have high strength and hardness, which means that at the same thickness, they can withstand greater pressure and impact, making them more advantageous in the manufacture of military equipment such as armored vehicles, aircraft and drones; secondly, aluminum-based nanocomposites have good electrical and thermal conductivity, which makes them have a wide range of application potential in electronic equipment and the energy industry. In addition, its lightweight properties make it very attractive in the aerospace field because it can reduce the weight of aircraft and spacecraft and improve their fuel efficiency and performance; and the good corrosion resistance of aluminum-based nanocomposites gives it a longer service life in harsh environments; finally, the properties of aluminum-based nanocomposite powders can be adjusted by changing the type and size of nanoparticles, making them multifunctional and meeting the specific needs of different fields.
[0003] At present, the common preparation methods of aluminum-based nanocomposites include mechanical alloying, gas atomization, sol-gel, etc. However, due to process limitations, the content of nanoparticles in aluminum-based nanocomposites prepared by these methods is relatively low, usually not exceeding 10%, which greatly limits the comprehensive performance of aluminum-based nanocomposite powders.
[0004] Therefore, how to prepare aluminum-based nanocomposite powder with high proportion of addition through appropriate process methods has become one of the important issues in the industry. Summary of the invention
[0005] In view of this, one of the objects of the present invention is to provide a method for preparing an aluminum-based nanocomposite material with the assistance of a molten salt and a high proportion of addition; a second object of the present invention is to provide an aluminum-based nanocomposite material with the assistance of a molten salt and a high proportion of addition.
[0006] In order to achieve the above object, the present invention provides the following technical solutions:
[0007] 1. A method for preparing a molten salt-assisted high-proportion addition aluminum-based nanocomposite material, the preparation method comprising the following steps:
[0008] (1) adding a mixture A obtained by mixing pure aluminum powder, nanoparticles, NaCl powder and KCl powder into a crucible, placing the mixture in a melting furnace, heating the mixture to 800° C.-850° C. and stirring the mixture, taking the mixture out and cooling it to obtain a mixture B;
[0009] (2) crushing the mixture B, adding water to fully dissolve it, and then ultrasonically centrifuging to obtain a solid mixture C;
[0010] (3) repeatedly adding water to the solid mixture C to fully dissolve it and then subjecting it to ultrasonic centrifugation to remove the chloride salt to obtain a molten salt-assisted high-proportion aluminum-based nanocomposite material;
[0011] In step (1), the mass ratio of nanoparticles to pure aluminum powder in the mixture A is greater than or equal to 3:7, and the nanoparticles are any one or more of oxide nanoparticles, carbide nanoparticles or boride nanoparticles.
[0012] Preferably, the oxide nanoparticles are Al 2 O 3 or ZrO; the carbide nanoparticles are any one or more of TiC, SiC, WC or VC; the boride nanoparticles are TiB 2 ;
[0013] The size of the nanoparticles is 10 to 500 nm.
[0014] Preferably, in step (1), the ratio of the total mass of pure aluminum powder and nanoparticles to the total mass of NaCl powder and KCl powder is 1:1 to 1:20.
[0015] Preferably, in step (1), the mixing time is 2 to 5 hours;
[0016] The smelting furnace is a resistance furnace or a medium frequency induction smelting furnace.
[0017] Preferably, in step (1), the stirring speed is 50 to 500 rpm, and the stirring time is 20 to 60 min.
[0018] Preferably, in step (2) and step (3), the ultrasonic time is 10 to 60 min, the centrifugal speed is 2000 to 5000 rpm, and the centrifugal time is 1 to 20 min.
[0019] 2. The aluminum-based nanocomposite material with high proportion addition assisted by molten salt prepared according to the above preparation method.
[0020] The beneficial effects of the present invention are as follows: the present invention discloses a method for preparing an aluminum-based nanocomposite material with high proportion of addition assisted by molten salt, which mainly comprises mixing pure aluminum powder, nanoparticles, NaCl powder and KCl powder, stirring at 800°C-850°C, and dissolving the chloride salt therein by repeatedly adding water and then ultrasonic centrifuging. The mass ratio of the nanoparticles to the pure aluminum powder used in the preparation method of the present invention is greater than or equal to 3:7, and the aluminum-based nanocomposite material with high proportion of nanoparticles added is finally prepared by self-dispersing the nanoparticles in the pure aluminum powder molten salt system. The preparation method of the present invention is of great significance to the large-scale production of aluminum-based nanocomposite material powder with high proportion of addition.
[0021] Other advantages, objectives and features of the present invention will be described in the following description to some extent, and to some extent, will be obvious to those skilled in the art based on the following examination and study, or can be taught from the practice of the present invention. The objectives and other advantages of the present invention can be realized and obtained through the following description. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention will be described in detail below in conjunction with the accompanying drawings, wherein:
[0023] Figure 1 The Al-50%TiB prepared in Example 1 2 Low magnification SEM image of aluminum-based nanocomposite powder;
[0024] Figure 2 The Al-50%TiB prepared in Example 1 2 High magnification SEM image (a) and EDS image (b) of aluminum-based nanocomposite powder. DETAILED DESCRIPTION
[0025] The following describes the embodiments of the present invention by specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention. It should be noted that the illustrations provided in the following embodiments only illustrate the basic concept of the present invention in a schematic manner, and the following embodiments and features in the embodiments can be combined with each other without conflict.
[0026] Example 1
[0027] A molten salt-assisted high-proportion aluminum-based nanocomposite material (Al-50%TiB 2Aluminum-based nanocomposite powder), the specific preparation method is as follows:
[0028] (1) 50g of pure aluminum powder and 50g of TiB with an average particle size of 300nm were mixed. 2 Nanoparticle powder, 300g NaCl powder and 700g KCl powder were added into a mixer and mixed for 3h to obtain mixture A, which was added into a graphite crucible and placed into a melting furnace. The mixture was heated to 850°C and stirred at 450rpm for 45min. The mixture was taken out and naturally cooled in air to obtain mixture B.
[0029] (2) The mixture B is crushed and placed in a glass centrifuge tube, water is added to fully dissolve it, and after ultrasonication for 35 minutes, the mixture is centrifuged at a speed of 4500 rm for 10 minutes to obtain a solid mixture C;
[0030] (3) The solid mixture C is repeatedly added with water to fully dissolve and then ultrasonically centrifuged for 6 times to remove the chloride salt to obtain a molten salt-assisted high-proportion aluminum-based nanocomposite material (Al-50% TiB 2 Aluminum-based nanocomposite powder), its SEM image is as follows Figure 2 shown.
[0031] Example 2
[0032] A molten salt-assisted high-proportion aluminum-based nanocomposite material (Al-30% SiC aluminum-based nanocomposite material powder), the specific preparation method is as follows:
[0033] (1) 70 g of pure aluminum powder, 30 g of SiC nanoparticle powder with an average particle size of 50 nm, 500 g of NaCl powder and 500 g of KCl powder were added to a mixer and mixed for 3 h to obtain a mixture A, which was added to a graphite crucible and placed in a melting furnace. The mixture was heated to 820° C. and stirred at 300 rpm for 30 min. The mixture was taken out and naturally cooled in air to obtain a mixture B;
[0034] (2) The mixture B is crushed and placed in a glass centrifuge tube, water is added to fully dissolve it, and after ultrasonication for 20 minutes, the mixture is centrifuged at a speed of 3000 rm for 5 minutes to obtain a solid mixture C;
[0035] (3) The solid mixture C is repeatedly added with water to fully dissolve and then ultrasonically centrifuged for 4 times to remove the chloride salt to obtain a molten salt-assisted high-proportion aluminum-based nanocomposite material (Al-30% SiC aluminum-based nanocomposite material powder). The SEM image is as follows: Figure 1 shown.
[0036] Example 3
[0037] A molten salt-assisted high-proportion aluminum-based nanocomposite material (Al-40%Al 2 O 3 Aluminum-based nanocomposite powder), the specific preparation method is as follows:
[0038] (1) 60 g pure aluminum powder and 40 g Al with an average particle size of 500 nm were mixed. 2 O 3 Nanoparticle powder, 30g NaCl powder and 70g KCl powder were added into a mixer and mixed for 2h to obtain mixture A, which was added into a graphite crucible and placed into a melting furnace. The mixture was heated to 800°C and stirred at 50rpm for 60min. The mixture was taken out and naturally cooled in air to obtain mixture B.
[0039] (2) The mixture B is crushed and placed in a glass centrifuge tube, water is added to fully dissolve it, and after ultrasonication for 60 minutes, the mixture is centrifuged at a speed of 5000 rm for 1 minute to obtain a solid mixture C;
[0040] (3) The solid mixture C is repeatedly added with water to fully dissolve and then ultrasonically centrifuged for 6 times to remove the chloride salt to obtain a molten salt-assisted high-proportion aluminum-based nanocomposite material (Al-40% Al 2 O 3 Aluminum-based nanocomposite powder).
[0041] Example 4
[0042] A molten salt-assisted high-proportion addition aluminum-based nanocomposite material (Al-90% ZrO aluminum-based nanocomposite material powder), the specific preparation method is as follows:
[0043] (1) 10 g of pure aluminum powder, 90 g of ZrO nanoparticle powder with an average particle size of 10 nm, 600 g of NaCl powder and 1400 g of KCl powder were added to a mixer and mixed for 5 h to obtain a mixture A, which was added to a graphite crucible and placed in a melting furnace. The mixture was heated to 820° C. and stirred at 500 rpm for 20 min. The mixture was taken out and naturally cooled in air to obtain a mixture B;
[0044] (2) The mixture B is crushed and placed in a glass centrifuge tube, water is added to fully dissolve it, and after ultrasonication for 10 minutes, the mixture is centrifuged at a speed of 2000 rm for 20 minutes to obtain a solid mixture C;
[0045] (3) The solid mixture C is repeatedly added with water to fully dissolve and then ultrasonically centrifuged for 6 times to remove chloride salt to obtain a molten salt-assisted high-proportion aluminum-based nanocomposite material (Al-90% ZrO aluminum-based nanocomposite material powder).
[0046] Example 5
[0047] The "TiB 2 " are replaced by "TiC", "SiC", "WC" and "VC" respectively, and the method of Example 1 is followed to obtain Al-50%TiC aluminum-based nanocomposite powder, Al-50%SiC aluminum-based nanocomposite powder, Al-50%WC aluminum-based nanocomposite powder and Al-50%VC aluminum-based nanocomposite powder respectively.
[0048] Figure 1 The molten salt-assisted high-proportion aluminum-based nanocomposite material (Al-50% TiB 2 Aluminum-based nanocomposite powder) low magnification SEM image. Figure 1 It can be seen that under low magnification (350 times) viewing field, Al-50%TiB 2 The nanocomposite powders have good sphericity. Figure 2 The molten salt-assisted high-proportion aluminum-based nanocomposite material (Al-50% TiB 2 High magnification SEM image (a) and EDS image (b) of aluminum-based nanocomposite powder. Figure 2 It can be seen in a that in the high magnification (35000 times) field of view, the molten salt-assisted high-proportion added aluminum-based nanocomposite material (Al-50% TiB 2 Aluminum-based nanocomposite powder) The powder grains are fine, basically below 10μm, and the white phase between / inside the grain boundaries is the nanoparticles (as shown in the red frame); Figure 2 The red frame area in a is further magnified 200,000 times, and the distribution of TiB2 nanoparticles can be clearly seen, and EDS characterization also confirms the presence of Ti element (such as Figure 2 (b)
[0049] Similarly, electron microscope scanning was performed on the molten salt-assisted high-proportion addition aluminum-based nanocomposites prepared in Examples 2 to 5, and the obtained SEM and EDS images were similar to those of the molten salt-assisted high-proportion addition aluminum-based nanocomposites in Example 1, both of which have the characteristics of fine powder grain structure and nanoparticles distributed along grain boundaries or within the crystals, and EDS characterization can calibrate the presence of related elements.
[0050] In summary, the present invention discloses a method for preparing a molten salt-assisted high-proportion aluminum-based nanocomposite material, which mainly comprises mixing pure aluminum powder, nanoparticles, NaCl powder and KCl powder, stirring at 800°C-850°C, and dissolving the chloride salt therein by repeatedly adding water and then ultrasonic centrifuging. The mass ratio of the nanoparticles to the pure aluminum powder used in the preparation method of the present invention is greater than or equal to 3:7, and the nanoparticles are self-dispersed in the pure aluminum powder molten salt system to finally prepare an aluminum-based nanocomposite material with a high proportion of nanoparticles added. The preparation method of the present invention is of great significance to the large-scale production of aluminum-based nanocomposite material powder with a high proportion of addition.
[0051] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the purpose and scope of the technical solution, which should be included in the scope of the claims of the present invention.
Claims
1. A method for preparing a molten salt-assisted high-proportion addition aluminum-based nanocomposite material, characterized in that: The preparation method comprises the following steps: (1) adding a mixture A obtained by mixing pure aluminum powder, nanoparticles, NaCl powder and KCl powder into a crucible, placing the mixture in a melting furnace, heating the mixture to 800° C.-850° C. and stirring the mixture, taking the mixture out and cooling it to obtain a mixture B; (2) crushing the mixture B, adding water to fully dissolve it, and then ultrasonically centrifuging to obtain a solid mixture C; (3) repeatedly adding water to the solid mixture C to fully dissolve it and then subjecting it to ultrasonic centrifugation to remove the chloride salt to obtain a molten salt-assisted high-proportion aluminum-based nanocomposite material; In step (1), the mass ratio of nanoparticles to pure aluminum powder in the mixture A is greater than or equal to 3:7, and the nanoparticles are any one or more of oxide nanoparticles, carbide nanoparticles or boride nanoparticles.
2. The preparation method according to claim 1, characterized in that: The oxide nanoparticles are Al2O3 or ZrO; the carbide nanoparticles are any one or more of TiC, SiC, WC or VC; the boride nanoparticles are TiB2; and the size of the nanoparticles is 10 to 500 nm.
3. The preparation method according to claim 1, characterized in that: In step (1), the ratio of the total mass of the pure aluminum powder and the nanoparticles to the total mass of the NaCl powder and the KCl powder is 1:1 to 1:
20.
4. The preparation method according to claim 1, characterized in that: In step (1), the mixing time is 2 to 5 hours; The smelting furnace is a resistance furnace or a medium frequency induction smelting furnace.
5. The preparation method according to claim 1, characterized in that: In step (1), the stirring speed is 50 to 500 rpm, and the stirring time is 20 to 60 min.
6. The preparation method according to claim 1, characterized in that: In step (2) and step (3), the ultrasonic time is 10 to 60 minutes, the centrifugal speed is 2000 to 5000 rpm, and the centrifugal time is 1 to 20 minutes.
7. The aluminum-based nanocomposite material prepared by the preparation method according to any one of claims 1 to 6 with the assistance of molten salt and high proportion addition.