Degradable magnesium alloy with antibacterial effect and preparation method and application thereof
By preparing magnesium alloy wire materials containing Gd, Ag, Ga, and Zr, the problems of the inability to degrade and insufficient antibacterial properties of existing gastrointestinal anastomosis materials are solved, and biodegradable, antibacterial and strong magnesium alloy wire materials are realized. Suitable for gastrointestinal anastomosis.
Patent Information
- Application Number
- CN202411198430.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-12-06
AI Technical Summary
Existing gastrointestinal anastomosis materials such as titanium alloy cannot degrade and remain in the body for a long time. The antibacterial and toughness of magnesium alloys are insufficient, corrosion resistance is poor, and the degradation rate is too fast, which cannot meet clinical needs.
A magnesium alloy is prepared, containing Gd 3-7%, Ag 0.1-1.0%, Ga 0.2-2.0%, Zr 0.1-0.6%, and magnesium alloy wire material is prepared by hot extrusion, hot extraction molding and solid solution processes. It has a filamentous structure, tensile strength of 455-500MPa, yield strength of 320-360MPa, neutral salt spray corrosion rate is 0.1-0.2mm/y, Hank's solution weight loss rate is 0.2-0.3mm/y, and has good antibacterial and strong toughness.
It realizes biodegradable magnesium alloy wire, has excellent antibacterial, corrosion-resistant and tough, meets the performance requirements of biomedical implant applications, and is especially suitable for gastrointestinal anastomosis.
Abstract
Description
Technical Field
[0001] The invention relates to a degradable magnesium alloy with antibacterial effect and a preparation method and application thereof. Background Art
[0002] Gastrointestinal anastomosis is the most important key technology in digestive tract reconstruction surgery, which directly affects the patient's postoperative recovery. There is an urgent need for antibacterial and degradable materials for gastrointestinal anastomosis staples. Currently, most of the staples used in gastrointestinal anastomosis surgery are made of titanium alloy, which cannot be degraded and remain in the body for a long time.
[0003] Magnesium alloy is a new generation of gastrointestinal anastomotic staple metal material with the characteristics of biodegradability and good toughness. However, the current gastrointestinal anastomotic staple magnesium alloy is not antibacterial and tough enough. In addition, it has poor corrosion resistance and a fast degradation rate in the body, resulting in mechanical instability, which cannot meet the clinical application requirements. Summary of the invention
[0004] An object of the present invention is to provide a magnesium alloy comprising the following metal elements in percentage by weight: Gd 3-7%, Ag 0.1-1.0%, Ga 0.2-2.0%, Zr 0.1-0.6%, and the balance Mg.
[0005] In certain embodiments, the magnesium alloy is in filamentary form.
[0006] In certain embodiments, the magnesium alloy wire has a diameter of 1.0 mm, a tensile strength of 455-500 MPa, a yield strength of 320-360 MPa, an elongation after fracture of 19.0-25.0%, a neutral salt spray corrosion rate of 0.1-0.2 mm / y, and a Hank's solution weight loss rate of 0.2-0.3 mm / y.
[0007] Another object of the present invention is to provide a method for preparing a magnesium alloy wire, comprising:
[0008] Mg-20Gd, 99.99Ag, Mg-30Zr and 99.99Mg are melted respectively, and the melted alloy or metal is cast into a metal mold to prepare a magnesium alloy ingot, wherein the magnesium alloy contains the following metal elements in weight percentage: Gd 4-6wt.%, Ag 0.1-0.3wt.%, Zr 0.6wt.%, and the balance Mg;
[0009] The magnesium alloy ingot is subjected to hot extrusion, hot drawing and solid solution processes to obtain the magnesium alloy wire.
[0010] In certain embodiments, the melting temperature of 99.99Mg is 650°C, the melting temperature of Mg-20Gd is 740°C, the melting temperature of 99.99Ag is 750°C, and the melting temperature of Mg-30Zr is 780°C.
[0011] In certain embodiments, the hot extrusion has an extrusion ratio of 16-25:1 and an extrusion speed of 0.1-0.5 mm / s.
[0012] In certain embodiments, the heating temperature of the hot drawing forming is 300° C. and the drawing speed is 3.5 mm / s.
[0013] In certain embodiments, the solution temperature of the solution process is 450-480°C, and the solution time is 15-20h; the aging temperature is 180-250°C, and the aging time is 10-60h.
[0014] The magnesium alloy of the present invention can be used in the field of biomedical implant applications.
[0015] Another object of the present invention is to provide a medical implant, which is made of the magnesium alloy.
[0016] In certain embodiments, the medical implant is a gastrointestinal stapler. DETAILED DESCRIPTION
[0017] In order to better illustrate the purpose, complete technical route and advantages of the present invention, the present invention will be further described in detail below in conjunction with specific embodiments. However, the embodiments described below are only part of the embodiments of the present invention and do not include all embodiments. Based on the embodiments of the present invention, other embodiments that can be obtained by those skilled in the art without paying creative work all belong to the protection scope of the present invention.
[0018] In the embodiments described below, unless otherwise specified, the conventional methods used are technical means generally recognized or commonly used by those skilled in the art, and the instruments, reagents, consumables, etc. used in the embodiments of the present invention can be obtained through regular commercial channels.
[0019] The "China New Materials Industry Development Report" compiled by the Department of Chemical Engineering, Metallurgical and Materials Engineering of the Chinese Academy of Engineering and the Chinese Materials Research Society clearly puts forward the performance requirements for biomedical magnesium alloys: room temperature tensile strength ≥300MPa, yield strength ≥220MPa, elongation ≥20%, harmful impurities ≤500ppm; uniform degradation rate in artificial plasma ≤0.3mm / y, 90-day strength drop ≤20%, 180-day strength drop ≤50%, cytotoxicity level 1.
[0020] In order to meet the performance requirements of biomedical magnesium alloys, the present invention provides a degradable magnesium alloy with antibacterial and bone-promoting properties, which contains 4-6wt.% Gd, 0.1-0.3wt.% Ag, 0.6wt.% Zr, and the balance Mg. When the magnesium alloy is in filament form, the diameter of the wire is 1.0mm, the tensile strength is 455-500MPa, the yield strength is 320-360MPa, the elongation after fracture is 19.0-25.0%, the neutral salt spray corrosion rate is 0.1-0.2mm / y, and the Hank's solution weight loss rate is 0.2-0.3mm / y.
[0021] The magnesium alloy of the present invention has the characteristics of antibacterial, low corrosion rate and excellent strength and toughness. The contained Ag element has good antibacterial effect; Gd forms a dense Gd2O3 passivation film, reduces the corrosion rate and improves corrosion resistance; Gd and Mg elements form a strengthening phase, greatly improving the mechanical properties, and Zr is a good grain refiner, which synergistically improves strength and toughness.
[0022] Example 1
[0023] Alloy composition: Gd 6wt.%, Ag 0.1wt.%, Zr 0.6wt.%, and the balance is Mg.
[0024] Preparation of alloy ingots: Add in the form of Mg-20Gd (Jiangxi Shida Magnesium Alloy Technology Co., Ltd.), 99.99Ag, Mg-30Zr (Jiangxi Shida Magnesium Alloy Technology Co., Ltd.) and 99.99Mg respectively; add the following alloys in sequence through a resistance furnace: 99.99Mg melting temperature is 650°C, Mg-20Gd melting temperature is 740°C, 99.99Ag melting temperature is 750°C, Mg-30Zr melting temperature is 780°C. After all the above alloys or metals are completely melted, cast them into a metal mold for gravity casting to form an ingot with a diameter of 200 mm and a height of 500 mm.
[0025] Hot processing technology: The hot extrusion process has an extrusion ratio of 25:1 and an extrusion speed of 0.1 mm / s.
[0026] Hot drawing process: heating temperature 300℃, drawing speed 3.5mm / s, after 30 times of hot drawing, a wire with a diameter of 1.0mm is obtained.
[0027] Heat treatment system: solution treatment at 450°C for 15 hours; aging at 180°C for 60 hours.
[0028] The prepared alloy was subjected to tensile mechanics and neutral salt spray corrosion resistance tests. The tensile mechanics was tested according to the standard GB / T228.1-2010 "Metallic Material Tensile Test Method". The neutral salt spray corrosion resistance was tested according to the standard GB / T10125-2012 "Artificial Atmosphere Corrosion Test-Salt Spray Test".
[0029] The results show that the wire has a diameter of 1.0 mm, a tensile strength of 480 MPa, a yield strength of 340 MPa, an elongation of 20.0%, a neutral salt spray corrosion rate of 0.15 mm / y, and a Hank's solution weight loss rate of 0.25 mm / y, and can be used in biomedical implant applications.
[0030] The antibacterial activity was tested in vitro by plate spreading method.
[0031] The results showed that the in vitro bactericidal rate of Escherichia coli and Staphylococcus aureus was 80%, 79%, and the minimum inhibitory concentration was 230 mg / mL.
[0032] Example 2
[0033] Alloy composition: Gd 6wt.%, Ag 0.3wt.%, Zr 0.6wt.%, and the balance is Mg.
[0034] Preparation of alloy ingot: Mg-20Gd, 99.99Ag, Mg-30Zr and 99.99Mg are added respectively. The following alloys are added in sequence through a resistance furnace: 99.99Mg has a melting temperature of 650°C, Mg-20Gd has a melting temperature of 740°C, 99.99Ag has a melting temperature of 750°C, and Mg-30Zr has a melting temperature of 780°C. After all the above alloys or metals are completely melted, they are cast into a metal mold for gravity casting of an ingot with a diameter of 200mm and a height of 500mm.
[0035] Hot processing technology: The hot extrusion process has an extrusion ratio of 25:1 and an extrusion speed of 0.1 mm / s.
[0036] Hot drawing process: heating temperature 300℃, drawing speed 3.5mm / s, after 30 times of hot drawing, a wire with a diameter of 1.0mm is obtained.
[0037] Heat treatment system: solution treatment at 450°C for 15 hours; aging at 180°C for 60 hours.
[0038] The prepared alloy was subjected to tensile mechanics and neutral salt spray corrosion resistance tests. The tensile mechanics was tested according to the standard GB / T228.1-2010 "Metallic Material Tensile Test Method". The neutral salt spray corrosion resistance was tested according to the standard GB / T10125-2012 "Artificial Atmosphere Corrosion Test-Salt Spray Test".
[0039] The results show that the wire has a diameter of 1.0 mm, a tensile strength of 500 MPa, a yield strength of 350 MPa, an elongation of 17.0%, a neutral salt spray corrosion rate of 0.2 mm / y, and a Hank's solution weight loss rate of 0.3 mm / y, and can be used in biomedical implant applications.
[0040] The antibacterial activity was tested in vitro by plate spreading method.
[0041] The results showed that the in vitro bactericidal rate of Escherichia coli and Staphylococcus aureus was 80.2% and 72.5% respectively, and the minimum inhibitory concentration was 230 mg / mL.
[0042] Example 3
[0043] Alloy composition: Gd 4wt.%, Ag 0.1wt.%, Zr 0.6wt.%, and the balance is Mg.
[0044] Preparation of alloy ingot: Mg-20Gd, 99.99Ag, Mg-30Zr and 99.99Mg are added respectively. The following alloys are added in sequence through a resistance furnace: 99.99Mg has a melting temperature of 650°C, Mg-20Gd has a melting temperature of 740°C, 99.99Ag has a melting temperature of 750°C, and Mg-30Zr has a melting temperature of 780°C. After all the above alloys or metals are completely melted, they are cast into a metal mold for gravity casting of an ingot with a diameter of 200mm and a height of 500mm.
[0045] Hot processing technology: The hot extrusion process has an extrusion ratio of 25:1 and an extrusion speed of 0.1 mm / s.
[0046] Hot drawing process: heating temperature 300℃, drawing speed 3.5mm / s, after 30 times of hot drawing, a wire with a diameter of 1.0mm is obtained.
[0047] Heat treatment system: solution treatment at 450°C for 15 hours; aging at 180°C for 60 hours.
[0048] The prepared alloy was subjected to tensile mechanics and neutral salt spray corrosion resistance tests. The tensile mechanics was tested according to the standard GB / T228.1-2010 "Metallic Material Tensile Test Method". The neutral salt spray corrosion resistance was tested according to the standard GB / T10125-2012 "Artificial Atmosphere Corrosion Test-Salt Spray Test".
[0049] The results show that the wire has a diameter of 1.0 mm, a tensile strength of 460 MPa, a yield strength of 310 MPa, an elongation of 25.0%, a neutral salt spray corrosion rate of 0.1 mm / y, and a Hank's solution weight loss rate of 0.2 mm / y, and can be used in biomedical implant applications.
[0050] The antibacterial activity was tested in vitro by plate spreading method.
[0051] The results showed that the in vitro bactericidal rate of Escherichia coli and Staphylococcus aureus was 78.2% and 69.8%, respectively, and the minimum inhibitory concentration was 250 mg / mL.
[0052] Comparative Example 1
[0053] Alloy composition: Gd 2wt.%, Ag 0.1wt.%, Zr 0.6wt.%, and the balance is Mg.
[0054] Preparation of alloy ingot: Mg-20Gd, 99.99Ag, Mg-30Zr and 99.99Mg are added respectively. The following alloys are added in sequence through a resistance furnace: 99.99Mg has a melting temperature of 650°C, Mg-20Gd has a melting temperature of 740°C, 99.99Ag has a melting temperature of 750°C, and Mg-30Zr has a melting temperature of 780°C. After all the above alloys or metals are completely melted, they are cast into a metal mold for gravity casting of an ingot with a diameter of 200mm and a height of 500mm.
[0055] Hot extrusion process: extrusion ratio 25:1, extrusion speed 0.1mm / s;
[0056] Hot drawing process: heating temperature 300℃, drawing speed 3.5mm / s, after 30 times of hot drawing, a wire with a diameter of 1.0mm is obtained;
[0057] Heat treatment system: solution treatment at 450°C for 15 hours; aging at 180°C for 60 hours.
[0058] The prepared alloy was subjected to tensile mechanics and neutral salt spray corrosion resistance tests. The tensile mechanics was tested according to the standard GB / T228.1-2010 "Metallic Material Tensile Test Method". The neutral salt spray corrosion resistance was tested according to the standard GB / T10125-2012 "Artificial Atmosphere Corrosion Test-Salt Spray Test".
[0059] The results show that the wire diameter is 1.0mm, the tensile strength is 420MPa, the yield strength is 110MPa, the elongation after fracture is 30.0%, the neutral salt spray corrosion rate is 0.1mm / y, and the Hank's solution weight loss rate is 0.2mm / y.
[0060] Comparative Example 2
[0061] Alloy composition: Gd 10wt.%, Ag 0.1wt.%, Zr 0.6wt.%, and the balance Mg.
[0062] Preparation of alloy ingot: Mg-20Gd, 99.99Ag, Mg-30Zr and 99.99Mg are added respectively. The following alloys are added in sequence through a resistance furnace: 99.99Mg has a melting temperature of 650°C, Mg-20Gd has a melting temperature of 740°C, 99.99Ag has a melting temperature of 750°C, and Mg-30Zr has a melting temperature of 780°C. After all the above alloys or metals are completely melted, they are cast into a metal mold for gravity casting of an ingot with a diameter of 200mm and a height of 500mm.
[0063] Hot extrusion process: extrusion ratio 25:1, extrusion speed 0.1mm / s;
[0064] Hot drawing process: heating temperature 300℃, drawing speed 3.5mm / s, after 30 times of hot drawing, a wire with a diameter of 1.0mm is obtained;
[0065] Heat treatment system: solution treatment at 450°C for 15 hours; aging at 180°C for 60 hours.
[0066] The prepared alloy was subjected to tensile mechanics and neutral salt spray corrosion resistance tests. The tensile mechanics was tested according to the standard GB / T228.1-2010 "Metallic Material Tensile Test Method". The neutral salt spray corrosion resistance was tested according to the standard GB / T10125-2012 "Artificial Atmosphere Corrosion Test-Salt Spray Test".
[0067] The results show that the wire diameter is 1.0mm, the tensile strength is 520MPa, the yield strength is 400MPa, the elongation after fracture is 10.5%, the neutral salt spray corrosion rate is 0.2mm / y, and the Hank's solution weight loss rate is 0.4mm / y.
[0068] Comparative Example 3
[0069] Alloy composition: Gd 6wt.%, Ag 2.0wt.%, Zr 0.6wt.%, the balance is Mg;
[0070] Preparation of alloy ingot: Mg-20Gd, 99.99Ag, Mg-30Zr and 99.99Mg are added respectively. The following alloys are added in sequence through a resistance furnace: 99.99Mg has a melting temperature of 650°C, Mg-20Gd has a melting temperature of 740°C, 99.99Ag has a melting temperature of 750°C, and Mg-30Zr has a melting temperature of 780°C. After all the above alloys or metals are completely melted, they are cast into a metal mold for gravity casting of an ingot with a diameter of 200mm and a height of 500mm.
[0071] Hot extrusion process: extrusion ratio 25:1, extrusion speed 0.1mm / s;
[0072] Hot drawing process: heating temperature 300℃, drawing speed 3.5mm / s, after 30 times of hot drawing, a wire with a diameter of 1.0mm is obtained;
[0073] Heat treatment system: solution treatment at 450°C for 15 hours; aging at 180°C for 60 hours.
[0074] The prepared alloy was subjected to tensile mechanics and neutral salt spray corrosion resistance tests. The tensile mechanics was tested according to the standard GB / T228.1-2010 "Metallic Material Tensile Test Method". The neutral salt spray corrosion resistance was tested according to the standard GB / T10125-2012 "Artificial Atmosphere Corrosion Test-Salt Spray Test".
[0075] The results show that the wire diameter is 1.0mm, the tensile strength is 560MPa, the yield strength is 440MPa, the elongation after fracture is 6.5%, the neutral salt spray corrosion rate is 0.4mm / y, and the Hank's solution weight loss rate is 0.6mm / y.
[0076] Comparative Example 4
[0077] Alloy composition: Gd 2wt.%, Ag 0.1wt.%, Ga 0.2wt.%, Zr 0.6wt.%, and the balance is Mg.
[0078] Preparation of alloy ingots: Add the following alloys in the form of Mg-20Gd, 99.99Ag, 99.99Ga, Mg-30Zr and 99.99Mg respectively through a resistance furnace: 99.99Mg has a melting temperature of 650°C, Mg-20Gd has a melting temperature of 740°C, 99.99Ag has a melting temperature of 750°C, 99.99Ga has a melting temperature of 760°C, and Mg-30Zr has a melting temperature of 780°C. After all the above alloys or metals are completely melted, cast them into a metal mold for gravity casting to form an ingot with a diameter of 200 mm and a height of 500 mm.
[0079] Hot processing technology: The hot extrusion process has an extrusion ratio of 25:1 and an extrusion speed of 0.1 mm / s.
[0080] Heat treatment system: solution treatment at 450°C for 15 hours; aging at 180°C for 60 hours.
[0081] The prepared alloy was subjected to tensile mechanics and neutral salt spray corrosion resistance tests. The tensile mechanics was tested according to the standard GB / T228.1-2010 "Metallic Material Tensile Test Method". The neutral salt spray corrosion resistance was tested according to the standard GB / T10125-2012 "Artificial Atmosphere Corrosion Test-Salt Spray Test".
[0082] The results show that the ingot has a tensile strength of 240 MPa, a yield strength of 100 MPa, an elongation after fracture of 26.0%, a neutral salt spray corrosion rate of 0.05 mm / y, and a Hank's solution weight loss rate of 0.1 mm / y.
[0083] Comparative Example 5
[0084] Alloy composition: Gd 10wt.%, Ag 0.1wt.%, Ga 0.2wt.%, Zr 0.6wt.%, and the balance Mg.
[0085] Preparation of alloy ingots: Add the following alloys in the form of Mg-20Gd, 99.99Ag, 99.99Ga, Mg-30Zr and 99.99Mg respectively through a resistance furnace: 99.99Mg has a melting temperature of 650°C, Mg-20Gd has a melting temperature of 740°C, 99.99Ag has a melting temperature of 750°C, 99.99Ga has a melting temperature of 760°C, and Mg-30Zr has a melting temperature of 780°C. After all the above alloys or metals are completely melted, cast them into a metal mold for gravity casting to form an ingot with a diameter of 200 mm and a height of 500 mm.
[0086] Hot processing technology: The hot extrusion process has an extrusion ratio of 25:1 and an extrusion speed of 0.1 mm / s.
[0087] Heat treatment system: solution treatment at 450°C for 15 hours; aging at 180°C for 60 hours.
[0088] The prepared alloy was subjected to tensile mechanics and neutral salt spray corrosion resistance tests. The tensile mechanics was tested according to the standard GB / T228.1-2010 "Metallic Material Tensile Test Method". The neutral salt spray corrosion resistance was tested according to the standard GB / T10125-2012 "Artificial Atmosphere Corrosion Test-Salt Spray Test".
[0089] The results show that the ingot has a tensile strength of 480 MPa, a yield strength of 350 MPa, an elongation after fracture of 10.0%, a neutral salt spray corrosion rate of 0.5 mm / y, and a Hank's solution weight loss rate of 0.8 mm / y.
[0090] Comparative Example 6
[0091] Alloy composition: Gd 6wt.%, Ag 2wt.%, Ga 0.2wt.%, Zr 0.6wt.%, and the balance is Mg.
[0092] Preparation of alloy ingot: Mg-20Gd, 99.99Ag, 99.99Ga, Mg-30Zr and 99.99Mg are added respectively. The following alloys are added in sequence through a resistance furnace: 99.99Mg has a melting temperature of 650°C, Mg-20Gd has a melting temperature of 740°C, 99.99Ag has a melting temperature of 750°C, 99.99Ga has a melting temperature of 760°C, and Mg-30Zr has a melting temperature of 780°C. After all the above alloys or metals are completely melted, they are cast into a metal mold for gravity casting of an ingot with a diameter of 200mm and a height of 500mm.
[0093] Hot processing technology: The hot extrusion process has an extrusion ratio of 25:1 and an extrusion speed of 0.1 mm / s.
[0094] Heat treatment system: solution treatment at 450°C for 15 hours; aging at 180°C for 60 hours.
[0095] The prepared alloy was subjected to tensile mechanics and neutral salt spray corrosion resistance tests. The tensile mechanics was tested according to the standard GB / T228.1-2010 "Metallic Material Tensile Test Method". The neutral salt spray corrosion resistance was tested according to the standard GB / T10125-2012 "Artificial Atmosphere Corrosion Test-Salt Spray Test".
[0096] The results show that the ingot has a tensile strength of 470 MPa, a yield strength of 360 MPa, an elongation after fracture of 6.0%, a neutral salt spray corrosion rate of 0.9 mm / y, and a Hank's solution weight loss rate of 1.4 mm / y.
[0097] The preferred embodiments of the present invention have been specifically described above, but the present invention is not limited to the embodiments. Those skilled in the art may make various equivalent modifications or substitutions without violating the spirit of the present invention. These equivalent modifications or substitutions are all included in the scope defined by the claims of this application.
Claims
1. A magnesium alloy, characterized in that: The magnesium alloy contains the following metal elements in percentage by weight: Gd 4-6wt.%, Ag 0.1-0.3wt.%, Zr 0.6wt.%, and the balance Mg.
2. The magnesium alloy according to claim 1, characterized in that The magnesium alloy is in filament form.
3. The magnesium alloy according to claim 2, characterized in that: The magnesium alloy wire has a diameter of 1.0 mm, a tensile strength of 455-500 MPa, a yield strength of 320-360 MPa, an elongation after fracture of 19.0-25.0%, a neutral salt spray corrosion rate of 0.1-0.2 mm / y, and a Hank's solution weight loss rate of 0.2-0.3 mm / y.
4. A method for preparing a magnesium alloy wire, comprising: Mg-20Gd, 99.99Ag, Mg-30Zr and 99.99Mg are melted respectively, and the melted alloy or metal is cast into a metal mold to prepare a magnesium alloy ingot, wherein the magnesium alloy contains the following metal elements in weight percentage: Gd 4-6wt.%, Ag 0.1-0.3wt.%, Zr 0.6wt.%, and the balance Mg; The magnesium alloy ingot is subjected to hot extrusion, hot drawing and solid solution processes to obtain the magnesium alloy wire.
5. The method according to claim 4, characterized in that The melting temperature of 99.99Mg is 650°C, the melting temperature of Mg-20Gd is 740°C, the melting temperature of 99.99Ag is 750°C, and the melting temperature of Mg-30Zr is 780°C.
6. The method according to claim 4, characterized in that The hot extrusion has an extrusion ratio of 16-25:1 and an extrusion speed of 0.1-0.5 mm / s.
7. The method according to claim 4, characterized in that The heating temperature of the hot drawing forming is 300° C. and the drawing speed is 3.5 mm / s.
8. The method according to claim 4, characterized in that The solution temperature of the solution process is 450-480° C., and the solution time is 15-20 hours; the aging temperature is 180-250° C., and the aging time is 10-60 hours.
9. A medical implant, characterized in that: The medical implant is made of the magnesium alloy according to any one of claims 1 to 3.
10. The medical implant according to claim 9, characterized in that The medical implant is a gastrointestinal anastomosis stapler.