Degradable magnesium alloy with antibacterial and bone-promoting effects as well as preparation method and application of degradable magnesium alloy
By adding Gd, Ag, Ga, and Zr elements to the magnesium alloy and adopting hot extrusion solution process, the mechanical properties and biocompatibility of magnesium alloys are improved, and the mechanical properties, corrosion rate and antibacterial properties of existing magnesium alloys are solved. and the shortcomings in bone promotion have achieved higher clinical application potential.
Patent Information
- Application Number
- CN202411198991.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-12-06
AI Technical Summary
The existing biomedical magnesium alloys have shortcomings in mechanical properties, corrosion rate, antibacterial and bone promotion, and cannot meet the needs of clinical applications.
Developed a magnesium alloy containing Gd 3-7%, Ag 0.1-1.0%, Ga 0.2-2.0%, Zr 0.1-0.6%, and it is prepared by hot extrusion and solid solution processes to improve its tensile strength and yield strength. Antibacterial and osteopromoting properties.
The tensile strength of magnesium alloy is achieved by 400-450MPa, yield strength of 300-320MPa, elongation after break of 16.0-18.0%, corrosion rate of neutral salt spray 0.1-0.3mm/y, and weight loss rate of Hank's solution 0.2-0.4mm/y , significantly improving its antibacterial and bone-promoting effects.
Smart Images

Figure BDA0005017564420000051
Abstract
Description
Technical Field
[0001] The invention relates to a degradable magnesium alloy with antibacterial and bone-promoting effects, and a preparation method and application thereof. Background Art
[0002] Materials research in the biomedical field has been seeking a new material with good biocompatibility, antibacterial properties and the ability to promote bone tissue growth. Stainless steel, titanium alloys and cobalt-based alloys are often used in orthopedic implants due to their high mechanical strength and toughness. However, since their Young's modulus is much higher than that of human bones, they are prone to produce a "stress shielding effect", which is not conducive to bone tissue reconstruction. In addition, since such alloys are non-degradable, long-term retention in the body can easily lead to problems such as rejection and infection, and ultimately require secondary surgery to remove them, greatly increasing the patient's pain and economic burden. Therefore, it is particularly urgent to develop new degradable biomaterials that have antibacterial properties and can promote bone tissue growth.
[0003] Magnesium alloys are a new generation of medical implant metal materials with the characteristics of biodegradability and Young's modulus similar to bone tissue. However, the current mechanical properties of magnesium alloys are low, the corrosion rate is too fast, and the antibacterial and bone-promoting properties are insufficient, which cannot meet the clinical application needs. In response to these problems, domestic and foreign researchers have conducted a lot of research and development. The Mg-Ca-Zn alloy screws developed by South Korea's U&I company are used for fracture repair and have good biocompatibility; they are used for fixing or tightening kits, but their mechanical properties are still low. The rare earth magnesium alloy WE43 developed by Syntellix AG in Germany can be used for a variety of indications in orthopedics and trauma surgery. The biological implant application of WE43 fully demonstrates that rare earth magnesium alloys with low rare earth content have no toxic side effects. However, the corrosion rate of WE43 alloy is too fast, and there is no obvious antibacterial and bone-promoting effect, which requires further breakthroughs. Mg-Nd-Zn-Zr developed by Shanghai Jiaotong University and Huchuang Medical Technology Co., Ltd. in China is undergoing clinical trials, but the antibacterial and bone-promoting benefits have not yet been clarified. CN112472868B discloses a biodegradable MgNdZnSc biomedical magnesium alloy, whose mechanical yield strength is only 97MPa, which is still relatively low. CN114075629B discloses a biodegradable ultrafine-grained magnesium alloy, whose tensile strength is ≤300MPa, and there is no clear corrosion rate index. At present, the comprehensive toughness, corrosion resistance, antibacterial and bone promotion of biomedical magnesium alloys are still difficult problems that need to be solved urgently. Summary of the invention
[0004] An object of the present invention is to provide a magnesium alloy, wherein the magnesium alloy comprises the following metal elements in percentage by weight:
[0005] Gd 3-7%, Ag 0.1-1.0%, Ga 0.2-2.0%, Zr 0.1-0.6%, and the balance Mg.
[0006] In certain embodiments, the magnesium alloy has a tensile strength of 400-450 MPa, a yield strength of 300-320 MPa, an elongation after fracture of 16.0-18.0%, a neutral salt spray corrosion rate of 0.1-0.3 mm / y, and a Hank's solution weight loss rate of 0.2-0.4 mm / y.
[0007] In certain embodiments, the magnesium alloy has antibacterial and osteopromoting effects.
[0008] Another object of the present invention is to provide a method for preparing a magnesium alloy, comprising:
[0009] Mg-20Gd, 99.99Ag, 99.99Ga, Mg-30Zr and 99.99Mg are melted respectively, and the fused alloy or metal is cast into a metal mold to prepare a magnesium alloy ingot, wherein the magnesium alloy contains the following metal elements in percentage by weight: Gd 3-7%, Ag 0.1-1.0%, Ga 0.2-2.0%, Zr 0.1-0.6%, and the balance Mg;
[0010] The magnesium alloy ingot is subjected to hot extrusion and solid solution processes to obtain the magnesium alloy.
[0011] In certain embodiments, the melting temperature of 99.99Mg is 650°C, the melting temperature of Mg-20Gd is 740°C, the melting temperature of 99.99Ag is 750°C, and the melting temperature of Mg-30Zr is 780°C.
[0012] In some embodiments, the hot extrusion has an extrusion ratio of 16-25:1 and an extrusion speed of 0.1-0.5 mm / s. In some embodiments, the solution temperature of the solution process is 450-480°C, the solution time is 15-20 h, and the aging temperature is 180-250°C, and the aging time is 10-60 h.
[0013] Application of the magnesium alloy of the present invention in the field of biological orthopedics.
[0014] Another object of the present invention is to provide a medical implant, which is made of the magnesium alloy. DETAILED DESCRIPTION
[0015] In order to better illustrate the purpose, complete technical route and advantages of the present invention, the present invention will be further described in detail below in conjunction with specific embodiments. However, the embodiments described below are only part of the embodiments of the present invention and do not include all embodiments. Based on the embodiments of the present invention, other embodiments that can be obtained by those skilled in the art without paying creative work all belong to the protection scope of the present invention.
[0016] In the embodiments described below, unless otherwise specified, the conventional methods used are technical means generally recognized or commonly used by those skilled in the art, and the instruments, reagents, consumables, etc. used in the embodiments of the present invention can be obtained through regular commercial channels.
[0017] The "China New Materials Industry Development Report" compiled by the Department of Chemical Engineering, Metallurgy and Materials Engineering of the Chinese Academy of Engineering and the Chinese Materials Research Society clearly puts forward the performance requirements for biomedical magnesium alloys: room temperature tensile strength ≥300MPa, yield strength ≥220MPa, elongation ≥20%, harmful impurities ≤500ppm; uniform degradation rate in artificial plasma ≤0.3mm / y, 90-day strength drop ≤20%, 180-day strength drop ≤50%, cytotoxicity level 1.
[0018] In order to meet the performance requirements of biomedical magnesium alloys, the present invention provides a degradable magnesium alloy with antibacterial and bone-promoting properties, which comprises 3-7wt.% Gd, 0.1-1.0wt.% Ag, 0.2-2.0wt.% Ga, 0.1-0.6wt.% Zr, and the balance Mg. The magnesium alloy has a tensile strength of 400-450MPa, a yield strength of 300-320MPa, an elongation after fracture of 16.0-18.0%, a neutral salt spray corrosion rate of 0.1-0.3mm / y, and a Hank's solution weight loss rate of 0.2-0.4mm / y.
[0019] The Mg / Ag composite in magnesium alloy effectively promotes antibacterial properties, the Mg / Ga composite is beneficial to promoting bone cell formation, the Mg / Gd / Ag / Ga composite promotes mechanical strengthening and toughening, and Zr is a good grain refiner, synergistically improving strength and toughness. The Mg element is needed by the body.
[0020] The magnesium alloy of the present invention has obvious antibacterial effect. After Mg / Ag is composited, Mg-Ag microgalvanic corrosion is formed in body fluids, which promotes the release of Ag ions, hinders the work of bacterial oxygen metabolism enzymes, and effectively curbs bacterial reproduction, thereby achieving an antibacterial effect and reducing the risk of wound infection.
[0021] The magnesium alloy of the present invention has an obvious bone-promoting effect. After Mg / Ga is compounded, it can enhance the expression of alkaline phosphatase (Alpl), osteogenic factor (Osx) and Runt-related transcription factor 2 (Runx2), promote the formation of osteoblasts, effectively form new bone tissue, and also inhibit osteoclast differentiation, thus comprehensively playing a bone-promoting role.
[0022] The magnesium alloy of the present invention has excellent strength and toughness. After Mg / Gd / Ag / Ga are compounded, MgGdAg and MgGdGa strengthening phases are formed, which effectively inhibit dislocation movement and greatly improve strength and toughness. In addition, Zr has a significant grain refinement effect, simultaneously improves strength and plasticity, and comprehensively improves strength and toughness.
[0023] Example 1
[0024] Alloy composition: Gd 6wt.%, Ag 0.1wt.%, Ga 0.2wt.%, Zr 0.6wt.%, and the balance Mg.
[0025] Preparation of alloy ingots: Add in the form of Mg-20Gd (Jiangxi Shida Magnesium Alloy Technology Co., Ltd.), 99.99Ag, 99.99Ga, Mg-30Zr (Jiangxi Shida Magnesium Alloy Technology Co., Ltd.) and 99.99Mg respectively; add the following alloys in sequence through a resistance furnace: 99.99Mg melting temperature is 650°C, Mg-20Gd melting temperature is 740°C, 99.99Ag melting temperature is 750°C, 99.99Ga melting temperature is 760°C, Mg-30Zr melting temperature is 780°C, after all the above alloys or metals are completely melted, cast into a metal mold gravity casting ingot with a diameter of 200mm and a height of 500mm.
[0026] Hot processing technology: The hot extrusion process has an extrusion ratio of 25:1 and an extrusion speed of 0.1 mm / s.
[0027] Heat treatment system: solution treatment at 450°C for 15 hours; aging at 180°C for 60 hours.
[0028] The prepared alloy was subjected to tensile mechanics and neutral salt spray corrosion resistance tests. The tensile mechanics was tested according to the standard GB / T228.1-2010 "Metallic Material Tensile Test Method". The neutral salt spray corrosion resistance was tested according to the standard GB / T10125-2012 "Artificial Atmosphere Corrosion Test-Salt Spray Test".
[0029] The results show that the ingot has a tensile strength of 410 MPa, a yield strength of 305 MPa, an elongation of 22.0%, a neutral salt spray corrosion rate of 0.2 mm / y, and a Hank's solution weight loss rate of 0.3 mm / y.
[0030] The antibacterial activity was tested in vitro by plate spreading method.
[0031] The results showed that the ingot had an in vitro bactericidal rate of 97% for Escherichia coli and 97% for Staphylococcus aureus, and the minimum inhibitory concentration was 16 μg / mL.
[0032] PCR polymerase chain reaction was used to test the osteopromoting properties.
[0033] The magnesium alloy sample in this embodiment is a disc with a diameter of 10 mm and a thickness of 2 mm. It is polished with 1000# and 2000# SiC sandpaper respectively, cleaned with acetone and anhydrous ethanol ultrasonic vibration for 10 minutes respectively, blown dry and sterilized with ultraviolet light for 60 minutes on each side, and used immediately after sterilization.
[0034] The samples were placed in a 24-well plate and were placed in a 1.25 cm 2 / mL soaked in α-MEM medium containing 10% FBS, placed in a cell culture incubator at 37°C containing 5% CO2, after 72 hours, the extract was filtered with a 0.22μm filter and the extract was diluted 6 times for in vitro cell test.
[0035] Mouse embryo osteoblast precursor cells (C3T3-E1 cells, provided by the Central Laboratory of the Affiliated Stomatological Hospital of China Medical University, 10-15 generations) were added to α-MEM medium containing 10% FBS and placed in a cell culture incubator at 37°C and 5% CO2 volume fraction. The medium was changed every other day. When the confluence reached 80%-90%, 0.25% trypsin was used for digestion and passage. In subsequent experiments, MC3T3-E1 cells will be used to test the bone-promoting properties of magnesium alloys.
[0036] 1 mL of a concentration of 5 × 10 4 / mL cell suspension, inoculated in a 6-well plate, placed in a cell culture incubator at 37℃, CO2 volume fraction of 5% for 24 hours. After the cells adhered to the wall, the original culture medium was discarded, and after rinsing with PBS 3 times, 1mL of magnesium alloy extract was added to continue culturing, and the medium was changed every other day. After 3 days and 7 days of culture, the culture plate was removed, washed once with PBS, 1mL Trizol was added to each well, and gently shaken to make the lysate evenly distributed on the cell surface. Repeatedly blow until there is no obvious precipitation, transfer the cell lysate to a 1.5mL EP tube, stand at room temperature for 5 minutes, centrifuge at 4℃12000g for 5 minutes, transfer the supernatant to a new 1.5mL EP tube, add 200μL chloroform, shake evenly and stand for 5 minutes. Then, after centrifugation at 4℃12000g for 15 minutes, transfer the supernatant to a new 1.5mL EP tube, add 500μL isopropanol, mix well and stand at room temperature for 10 minutes. After centrifugation at 4°C 12000g for 10 minutes, the supernatant was discarded, and the precipitate was washed twice with 1mL 75% ethanol, centrifuged at 4°C 12000g for 5 minutes, the supernatant was discarded and the precipitate was retained. After drying at room temperature, the precipitate was dissolved in 20μL DEPC water. The content and quality of total RNA were determined by spectrophotometry at 260nm and 260 / 280nm, respectively. The extracted total RNA was reversed into cDNA using the PrmeScriptTm RT cDNA reverse transcription kit. The target genes ALP, OCN and Runt-related transcription factor 2 (RUNX-2) were quantified using the TBGreenTm Premix Ex TaqTm II kit.
[0037] Reaction system:
[0038]
[0039] Reaction conditions: pre-denaturation at 95°C for 2 min, 95°C for 15 s, 60°C for 60 s, 40 cycles.
[0040] Primer sequences
[0041] ALP
[0042] F:CATGTTCCTGGGAGATGGTAT;
[0043] R:GTGTTGTACGTCTTGGAGAGA.
[0044] OCN
[0045] F: ACCATCTTTCTGCTCACTCTGCT;
[0046] R:CCTTATTGCCCTCCTGCTTG.
[0047] RUNX-2
[0048] F: GCCACTTACCACAGAGCTATTA;
[0049] R: GGCGGTCAGAGAACAAACTA.
[0050] The results showed that the expression levels of osteogenesis-related genes were alkaline phosphatase (ALP) at 1.9, Runt-related transcription factor 2 (RUNX-2) at 1.8, and osteocalcin (OCN) at 1.5.
[0051] Example 2
[0052] Alloy composition: Gd 6wt.%, Ag 1.0wt.%, Ga 0.2wt.%, Zr 0.6wt.%, and the balance Mg.
[0053] Preparation of alloy ingot: Mg-20Gd, 99.99Ag, 99.99Ga, Mg-30Zr and 99.99Mg are added respectively. The following alloys are added in sequence through a resistance furnace: 99.99Mg has a melting temperature of 650°C, Mg-20Gd has a melting temperature of 740°C, 99.99Ag has a melting temperature of 750°C, 99.99Ga has a melting temperature of 760°C, and Mg-30Zr has a melting temperature of 780°C. After all the above alloys or metals are completely melted, they are cast into a metal mold for gravity casting of an ingot with a diameter of 200mm and a height of 500mm.
[0054] Hot processing technology: The hot extrusion process has an extrusion ratio of 25:1 and an extrusion speed of 0.1 mm / s.
[0055] Heat treatment system: solution treatment at 450°C for 15 hours; aging at 180°C for 60 hours.
[0056] The prepared alloy was subjected to tensile mechanics and neutral salt spray corrosion resistance tests. The tensile mechanics was tested according to the standard GB / T228.1-2010 "Metallic Material Tensile Test Method". The neutral salt spray corrosion resistance was tested according to the standard GB / T10125-2012 "Artificial Atmosphere Corrosion Test-Salt Spray Test".
[0057] The results show that the ingot has a tensile strength of 430 MPa, a yield strength of 330 MPa, an elongation of 21%, a neutral salt spray corrosion rate of 0.3 mm / y, and a Hank's solution weight loss rate of 0.4 mm / y.
[0058] The antibacterial activity was tested in vitro by plate spreading method.
[0059] The results showed that the ingot had an in vitro bactericidal rate of 98% for Escherichia coli and 98% for Staphylococcus aureus, and the minimum inhibitory concentration was 15 μg / mL.
[0060] PCR polymerase chain reaction was used to test the bone-promoting properties, see Example 1.
[0061] The results showed that the expression levels of osteogenesis-related genes were ALP 1.9, RUNX-2 1.8, and OCN 1.5.
[0062] Example 3
[0063] Alloy composition: Gd 3wt.%, Ag 1.0wt.%, Ga 0.2wt.%, Zr 0.6wt.%, and the balance Mg.
[0064] Preparation of alloy ingot: Mg-20Gd, 99.99Ag, 99.99Ga, Mg-30Zr and 99.99Mg are added respectively. The following alloys are added in sequence through a resistance furnace: 99.99Mg has a melting temperature of 650°C, Mg-20Gd has a melting temperature of 740°C, 99.99Ag has a melting temperature of 750°C, 99.99Ga has a melting temperature of 760°C, and Mg-30Zr has a melting temperature of 780°C. After all the above alloys or metals are completely melted, they are cast into a metal mold for gravity casting of an ingot with a diameter of 200mm and a height of 500mm.
[0065] Hot processing technology: The hot extrusion process has an extrusion ratio of 25:1 and an extrusion speed of 0.1 mm / s.
[0066] Heat treatment system: solution treatment at 450°C for 15 hours; aging at 180°C for 60 hours.
[0067] The prepared alloy was subjected to tensile mechanics and neutral salt spray corrosion resistance tests. The tensile mechanics was tested according to the standard GB / T228.1-2010 "Metallic Material Tensile Test Method". The neutral salt spray corrosion resistance was tested according to the standard GB / T10125-2012 "Artificial Atmosphere Corrosion Test-Salt Spray Test".
[0068] The results show that the tensile strength is 400MPa, the yield strength is 300MPa, the elongation after fracture is 25%, the neutral salt spray corrosion rate is 0.1mm / y, and the Hank's solution weight loss rate is 0.2mm / y.
[0069] The antibacterial activity was tested in vitro by plate spreading method.
[0070] The results showed that the ingot had an in vitro bactericidal rate of 97% for Escherichia coli and 97% for Staphylococcus aureus, and the minimum inhibitory concentration was 16 μg / mL.
[0071] PCR polymerase chain reaction was used to test the bone-promoting properties, see Example 1.
[0072] The results showed that the expression levels of osteogenesis-related genes were ALP 1.8, RUNX-2 1.7, and OCN 1.5.
[0073] Example 4
[0074] Alloy composition: Gd 6wt.%, Ag 0.1wt.%, Ga 2.0wt.%, Zr 0.6wt.%, and the balance Mg.
[0075] Preparation of alloy ingot: Mg-20Gd, 99.99Ag, 99.99Ga, Mg-30Zr and 99.99Mg are added respectively. The following alloys are added in sequence through a resistance furnace: 99.99Mg has a melting temperature of 650°C, Mg-20Gd has a melting temperature of 740°C, 99.99Ag has a melting temperature of 750°C, 99.99Ga has a melting temperature of 760°C, and Mg-30Zr has a melting temperature of 780°C. After all the above alloys or metals are completely melted, they are cast into a metal mold for gravity casting of an ingot with a diameter of 200mm and a height of 500mm.
[0076] Hot processing technology: The hot extrusion process has an extrusion ratio of 25:1 and an extrusion speed of 0.1 mm / s.
[0077] Heat treatment system: solution treatment at 450°C for 15 hours; aging at 180°C for 60 hours.
[0078] The prepared alloy was subjected to tensile mechanics and neutral salt spray corrosion resistance tests. The tensile mechanics was tested according to the standard GB / T228.1-2010 "Metallic Material Tensile Test Method". The neutral salt spray corrosion resistance was tested according to the standard GB / T10125-2012 "Artificial Atmosphere Corrosion Test-Salt Spray Test".
[0079] The results show that the tensile strength is 420MPa, the yield strength is 315MPa, the elongation after fracture is 21%, the neutral salt spray corrosion rate is 0.2mm / y, and the Hank's solution weight loss rate is 0.3mm / y.
[0080] The antibacterial activity was tested in vitro by plate spreading method.
[0081] The results showed that the in vitro bactericidal rate of Escherichia coli was 97%, the bactericidal rate of Staphylococcus aureus was 97%, and the minimum inhibitory concentration was 16μg / mL.
[0082] PCR polymerase chain reaction was used to test the bone-promoting properties, see Example 1.
[0083] The results showed that the expression levels of osteogenesis-related genes were ALP 2.0, RUNX-2 1.9, and OCN 1.6.
[0084] Comparative Example 1
[0085] Alloy composition: Gd 2wt.%, Ag 0.1wt.%, Ga 0.2wt.%, Zr 0.6wt.%, and the balance is Mg.
[0086] Preparation of alloy ingots: Add the following alloys in the form of Mg-20Gd, 99.99Ag, 99.99Ga, Mg-30Zr and 99.99Mg respectively through a resistance furnace: 99.99Mg has a melting temperature of 650°C, Mg-20Gd has a melting temperature of 740°C, 99.99Ag has a melting temperature of 750°C, 99.99Ga has a melting temperature of 760°C, and Mg-30Zr has a melting temperature of 780°C. After all the above alloys or metals are completely melted, cast them into a metal mold for gravity casting to form an ingot with a diameter of 200 mm and a height of 500 mm.
[0087] Hot processing technology: The hot extrusion process has an extrusion ratio of 25:1 and an extrusion speed of 0.1 mm / s.
[0088] Heat treatment system: solution treatment at 450°C for 15 hours; aging at 180°C for 60 hours.
[0089] The prepared alloy was subjected to tensile mechanics and neutral salt spray corrosion resistance tests. The tensile mechanics was tested according to the standard GB / T228.1-2010 "Metallic Material Tensile Test Method". The neutral salt spray corrosion resistance was tested according to the standard GB / T10125-2012 "Artificial Atmosphere Corrosion Test-Salt Spray Test".
[0090] The results show that the ingot has a tensile strength of 240 MPa, a yield strength of 100 MPa, an elongation of 26.0%, a neutral salt spray corrosion rate of 0.05 mm / y, and a Hank's solution weight loss rate of 0.1 mm / y.
[0091] The antibacterial activity was tested in vitro by plate spreading method.
[0092] The results showed that the ingot had an in vitro bactericidal rate of 96% for Escherichia coli and 96% for Staphylococcus aureus, and the minimum inhibitory concentration was 18 μg / mL.
[0093] PCR polymerase chain reaction was used to test the bone-promoting properties, see Example 1.
[0094] The results showed that the expression levels of osteogenesis-related genes were ALP 1.6, RUNX-2 1.6, and OCN 1.3.
[0095] Comparative Example 2
[0096] Alloy composition: Gd 10wt.%, Ag 0.1wt.%, Ga 0.2wt.%, Zr 0.6wt.%, and the balance Mg.
[0097] Preparation of alloy ingots: Add the following alloys in the form of Mg-20Gd, 99.99Ag, 99.99Ga, Mg-30Zr and 99.99Mg respectively through a resistance furnace: 99.99Mg has a melting temperature of 650°C, Mg-20Gd has a melting temperature of 740°C, 99.99Ag has a melting temperature of 750°C, 99.99Ga has a melting temperature of 760°C, and Mg-30Zr has a melting temperature of 780°C. After all the above alloys or metals are completely melted, cast them into a metal mold for gravity casting to form an ingot with a diameter of 200 mm and a height of 500 mm.
[0098] Hot processing technology: The hot extrusion process has an extrusion ratio of 25:1 and an extrusion speed of 0.1 mm / s.
[0099] Heat treatment system: solution treatment at 450°C for 15 hours; aging at 180°C for 60 hours.
[0100] The prepared alloy was subjected to tensile mechanics and neutral salt spray corrosion resistance tests. The tensile mechanics was tested according to the standard GB / T228.1-2010 "Metallic Material Tensile Test Method". The neutral salt spray corrosion resistance was tested according to the standard GB / T10125-2012 "Artificial Atmosphere Corrosion Test-Salt Spray Test".
[0101] The results show that the ingot has a tensile strength of 480MPa, a yield strength of 350MPa, an elongation of 10.0%, a neutral salt spray corrosion rate of 0.5mm / y, and a Hank's solution weight loss rate of 0.8mm / y.
[0102] The antibacterial activity was tested in vitro by plate spreading method.
[0103] The results showed that the in vitro bactericidal rate of Escherichia coli and Staphylococcus aureus of the ingot was 97%, 977%, and the minimum inhibitory concentration was 18μg / mL.
[0104] PCR polymerase chain reaction was used to test the bone-promoting properties, see Example 1.
[0105] The results showed that the expression levels of osteogenesis-related genes were ALP 1.8, RUNX-2 1.8, and OCN 1.5.
[0106] Comparative Example 3
[0107] Alloy composition: Gd 6wt.%, Ag 2wt.%, Ga 0.2wt.%, Zr 0.6wt.%, and the balance is Mg.
[0108] Preparation of alloy ingot: Mg-20Gd, 99.99Ag, 99.99Ga, Mg-30Zr and 99.99Mg are added respectively. The following alloys are added in sequence through a resistance furnace: 99.99Mg has a melting temperature of 650°C, Mg-20Gd has a melting temperature of 740°C, 99.99Ag has a melting temperature of 750°C, 99.99Ga has a melting temperature of 760°C, and Mg-30Zr has a melting temperature of 780°C. After all the above alloys or metals are completely melted, they are cast into a metal mold for gravity casting of an ingot with a diameter of 200mm and a height of 500mm.
[0109] Hot processing technology: The hot extrusion process has an extrusion ratio of 25:1 and an extrusion speed of 0.1 mm / s.
[0110] Heat treatment system: solution treatment at 450°C for 15 hours; aging at 180°C for 60 hours.
[0111] The prepared alloy was subjected to tensile mechanics and neutral salt spray corrosion resistance tests. The tensile mechanics was tested according to the standard GB / T228.1-2010 "Metallic Material Tensile Test Method". The neutral salt spray corrosion resistance was tested according to the standard GB / T10125-2012 "Artificial Atmosphere Corrosion Test-Salt Spray Test".
[0112] The results show that the ingot has a tensile strength of 470 MPa, a yield strength of 360 MPa, an elongation of 6.0%, a neutral salt spray corrosion rate of 0.9 mm / y, and a Hank's solution weight loss rate of 1.4 mm / y.
[0113] The antibacterial activity was tested in vitro by plate spreading method.
[0114] The results showed that the ingot had an in vitro bactericidal rate of 99% for Escherichia coli and 99% for Staphylococcus aureus, and a minimum inhibitory concentration of 15 μg / mL.
[0115] PCR polymerase chain reaction was used to test the bone-promoting properties, see Example 1.
[0116] The results showed that the expression levels of osteogenesis-related genes were ALP 1.8, RUNX-2 1.8, and OCN 1.5.
[0117] Comparative Example 4
[0118] Alloy composition: Gd 2wt.%, Ag 0.1wt.%, Zr 0.6wt.%, and the balance is Mg.
[0119] Preparation of alloy ingot: Mg-20Gd, 99.99Ag, Mg-30Zr and 99.99Mg are added respectively. The following alloys are added in sequence through a resistance furnace: 99.99Mg has a melting temperature of 650°C, Mg-20Gd has a melting temperature of 740°C, 99.99Ag has a melting temperature of 750°C, and Mg-30Zr has a melting temperature of 780°C. After all the above alloys or metals are completely melted, they are cast into a metal mold for gravity casting of an ingot with a diameter of 200mm and a height of 500mm.
[0120] Hot extrusion process: extrusion ratio 25:1, extrusion speed 0.1mm / s;
[0121] Hot drawing process: heating temperature 300℃, drawing speed 3.5mm / s, after 30 times of hot drawing, a wire with a diameter of 1.0mm is obtained;
[0122] Heat treatment system: solution treatment at 450°C for 15 hours; aging at 180°C for 60 hours.
[0123] The prepared alloy was subjected to tensile mechanics and neutral salt spray corrosion resistance tests. The tensile mechanics was tested according to the standard GB / T228.1-2010 "Metallic Material Tensile Test Method". The neutral salt spray corrosion resistance was tested according to the standard GB / T10125-2012 "Artificial Atmosphere Corrosion Test-Salt Spray Test".
[0124] The results show that the wire diameter is 1.0mm, the tensile strength is 420MPa, the yield strength is 110MPa, the elongation after fracture is 30.0%, the neutral salt spray corrosion rate is 0.1mm / y, and the Hank's solution weight loss rate is 0.2mm / y.
[0125] Comparative Example 5
[0126] Alloy composition: Gd 10wt.%, Ag 0.1wt.%, Zr 0.6wt.%, and the balance Mg.
[0127] Preparation of alloy ingot: Mg-20Gd, 99.99Ag, Mg-30Zr and 99.99Mg are added respectively. The following alloys are added in sequence through a resistance furnace: 99.99Mg has a melting temperature of 650°C, Mg-20Gd has a melting temperature of 740°C, 99.99Ag has a melting temperature of 750°C, and Mg-30Zr has a melting temperature of 780°C. After all the above alloys or metals are completely melted, they are cast into a metal mold for gravity casting of an ingot with a diameter of 200mm and a height of 500mm.
[0128] Hot extrusion process: extrusion ratio 25:1, extrusion speed 0.1mm / s;
[0129] Hot drawing process: heating temperature 300℃, drawing speed 3.5mm / s, after 30 times of hot drawing, a wire with a diameter of 1.0mm is obtained;
[0130] Heat treatment system: solution treatment at 450°C for 15 hours; aging at 180°C for 60 hours.
[0131] The prepared alloy was subjected to tensile mechanics and neutral salt spray corrosion resistance tests. The tensile mechanics was tested according to the standard GB / T228.1-2010 "Metallic Material Tensile Test Method". The neutral salt spray corrosion resistance was tested according to the standard GB / T10125-2012 "Artificial Atmosphere Corrosion Test-Salt Spray Test".
[0132] The results show that the wire diameter is 1.0mm, the tensile strength is 520MPa, the yield strength is 400MPa, the elongation after fracture is 10.5%, the neutral salt spray corrosion rate is 0.2mm / y, and the Hank's solution weight loss rate is 0.4mm / y.
[0133] Comparative Example 6
[0134] Alloy composition: Gd 6wt.%, Ag 2.0wt.%, Zr 0.6wt.%, the balance is Mg;
[0135] Preparation of alloy ingot: Mg-20Gd, 99.99Ag, Mg-30Zr and 99.99Mg are added respectively. The following alloys are added in sequence through a resistance furnace: 99.99Mg has a melting temperature of 650°C, Mg-20Gd has a melting temperature of 740°C, 99.99Ag has a melting temperature of 750°C, and Mg-30Zr has a melting temperature of 780°C. After all the above alloys or metals are completely melted, they are cast into a metal mold for gravity casting of an ingot with a diameter of 200mm and a height of 500mm.
[0136] Hot extrusion process: extrusion ratio 25:1, extrusion speed 0.1mm / s;
[0137] Hot drawing process: heating temperature 300℃, drawing speed 3.5mm / s, after 30 times of hot drawing, a wire with a diameter of 1.0mm is obtained;
[0138] Heat treatment system: solution treatment at 450°C for 15 hours; aging at 180°C for 60 hours.
[0139] The prepared alloy was subjected to tensile mechanics and neutral salt spray corrosion resistance tests. The tensile mechanics was tested according to the standard GB / T228.1-2010 "Metallic Material Tensile Test Method". The neutral salt spray corrosion resistance was tested according to the standard GB / T10125-2012 "Artificial Atmosphere Corrosion Test-Salt Spray Test".
[0140] The results show that the wire diameter is 1.0mm, the tensile strength is 560MPa, the yield strength is 440MPa, the elongation after fracture is 6.5%, the neutral salt spray corrosion rate is 0.4mm / y, and the Hank's solution weight loss rate is 0.6mm / y.
[0141] The preferred embodiments of the present invention have been specifically described above, but the present invention is not limited to the embodiments. Those skilled in the art may make various equivalent modifications or substitutions without violating the spirit of the present invention. These equivalent modifications or substitutions are all included in the scope defined by the claims of this application.
Claims
1. A magnesium alloy, characterized in that: The magnesium alloy contains the following metal elements in percentage by weight: Gd 3-7%, Ag 0.1-1.0%, Ga 0.2-2.0%, Zr 0.1-0.6%, and the balance Mg.
2. The magnesium alloy according to claim 1, characterized in that The magnesium alloy has a tensile strength of 400-450 MPa, a yield strength of 300-320 MPa, an elongation after fracture of 16.0-18.0%, a neutral salt spray corrosion rate of 0.1-0.3 mm / y, and a Hank's solution weight loss rate of 0.2-0.4 mm / y.
3. The magnesium alloy according to claim 1, characterized in that The magnesium alloy has antibacterial and bone-promoting effects.
4. A method for preparing a magnesium alloy, comprising: Mg-20Gd, 99.99Ag, 99.99Ga, Mg-30Zr and 99.99Mg are melted respectively, and the fused alloy or metal is cast into a metal mold to prepare a magnesium alloy ingot, wherein the magnesium alloy contains the following metal elements in percentage by weight: Gd 3-7%, Ag 0.1-1.0%, Ga 0.2-2.0%, Zr 0.1-0.6%, and the balance Mg; The magnesium alloy ingot is subjected to hot extrusion and solid solution processes to obtain the magnesium alloy.
5. The method according to claim 4, characterized in that The melting temperature of 99.99Mg is 650°C, the melting temperature of Mg-20Gd is 740°C, the melting temperature of 99.99Ag is 750°C, and the melting temperature of Mg-30Zr is 780°C.
6. The method according to claim 4, characterized in that The hot extrusion has an extrusion ratio of 16-25:1 and an extrusion speed of 0.1-0.5 mm / s.
7. The method according to claim 4, characterized in that The solution temperature of the solution process is 450-480° C., and the solution time is 15-20 hours; the aging temperature is 180-250° C., and the aging time is 10-60 hours.
8. Use of the magnesium alloy according to any one of claims 1 to 3 in the field of biological orthopedics.