Non-uniform layered ultra-fine grain steel with excellent obdurability and preparation method of non-uniform layered ultra-fine grain steel
By designing non-uniform layered ultrafine crystal structures and specific chemical components in low-carbon microalloy steel, combined with conventional process flow, the contradiction between strength and ductility is solved, the strength and toughness of the material is improved and process simplified, and the modern industrial complications are met. The demand for high performance materials.
Patent Information
- Application Number
- CN202411223054.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-09-03
AI Technical Summary
Low-carbon microalloy steels often sacrifice ductility and toughness while increasing their strength. It is difficult for the prior art to effectively prepare layered ultrafine crystal steels with excellent strength and toughness, especially in regulating their complex phase transformation mechanisms and chemical compositions. There are challenges.
By designing specific chemical components and process flows, non-uniform layered ultrafine crystal steel is prepared. The RD-ND surface shows inhomogeneous alternating distribution of ultrafine crystal layer and coarse crystal layer on the full thickness macroscopic, and Mn segregation phenomenon and The hot processing route forms a biphasic ultrafine crystal microstructure, combining conventional rolling and heat treatment equipment to optimize the strength and plasticity of the material.
The coordinated improvement of the strength and plasticity of the material has been achieved, which significantly improves the comprehensive service performance, meets the modern industry's demand for high-performance and cost-effective steel materials, and reduces its dependence on special equipment.
Smart Images

Figure CN119082606A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of preparation and processing of steel materials, and in particular to a non-uniform layered ultrafine-grained steel with excellent strength and toughness and a preparation method thereof. Background Art
[0002] In the modern industrial field, the demand for high-performance structural materials is growing, especially in the marine engineering, aerospace and automobile manufacturing industries that have extremely high requirements for material strength and plasticity. Low-carbon micro-alloyed steel is widely used due to its good processing performance and economy, but it often sacrifices ductility and toughness while improving its strength. Therefore, how to prepare low-carbon micro-alloyed steel with excellent comprehensive performance through process optimization and organizational regulation has always been a research hotspot in the industry.
[0003] Existing theoretical and experimental studies have shown that grain refinement is a toughening mechanism that can simultaneously improve the strength and toughness of steel materials. For example: Patent application number 202010240014.6 discloses a method for obtaining a needle-shaped ferrite ultrafine grain structure with a bimodal size distribution through controlled rolling and controlled cooling to achieve improved plasticity of pipeline steel; Patent application number 202110314137.4 provides a method for preparing a double gradient ultrafine grained low alloy steel plate with excellent ultra-low temperature toughness in crystal texture and grain size using an intermediate billet ultra-fast cooling process; Patent application number 202210829899.2 utilizes thermal cycling and deformation-induced ferrite mechanisms to achieve the preparation of ferrite ultrafine grained steel plates with good strength and plasticity matching under low reduction ratio conditions.
[0004] However, some studies have pointed out that layered ultrafine-grained materials may have greater potential in plasticity, work hardening ability and structural stability than single ultrafine-grained materials due to their more widely distributed heterogeneous interfaces and unique grain shapes. However, compared with the single non-ferrous metal materials commonly used to regulate layered ultrafine-grained structures, including Ti, Cu, etc., the more complex phase transformation mechanism and chemical composition in low-carbon microalloyed steels increase the difficulty of regulating layered ultrafine-grained structures. How to use existing technologies to prepare layered ultrafine-grained steels with excellent strength and toughness still faces challenges. Summary of the invention
[0005] In view of this, the present invention provides a non-uniform layered ultrafine-grained steel with excellent strength and toughness and a preparation method thereof, which is mainly intended to solve the "inverted" contradiction between strength and plasticity and toughness of current low-carbon microalloy steels during service. At the same time, the present invention utilizes the process flow of conventional rolling and heat treatment equipment to solve the current problems of complicated ultrafine-grained steel preparation process and high equipment requirements.
[0006] To achieve the above object, the technical solution provided by the present invention is as follows:
[0007] A non-uniform layered ultra-fine grain steel with excellent strength and toughness, the chemical composition of which includes, by mass percentage, C: 0.04-0.10%, Si: 0.10-0.30%, Mn: 1.00-2.20%, P: ≤0.008%, S: ≤0.004%, Ni: 0.20-0.60%, Cu: 0.40-0.70%, Nb: 0.015-0.045%, Ti: 0.005-0.030%, and the rest is Fe and inevitable impurities; the RD-ND surface of the ultra-fine grain steel presents the characteristics of non-uniform alternating distribution of ultra-fine grain layers and coarse grain layers in the full thickness macroscopically.
[0008] The ultrafine-grained steel of the present invention is prepared by selecting components with specific contents, and the obtained ultrafine-grained steel exhibits the characteristics of non-uniform alternating distribution of ultrafine-grained layers and coarse-grained layers on a millimeter-level longitudinal section. The specificity of this microstructure enables it to obtain a more excellent strength-toughness match.
[0009] The reasons for designing the chemical composition of the ultrafine grain steel of the present invention are as follows:
[0010] The C element can improve the strength by solid solution strengthening, precipitation strengthening and other methods. When its content is too low, the strength level is not easy to ensure, while when its content is too high, it affects the toughness and welding performance. Therefore, under the condition of ensuring strength, in order to expand the scope of application, the present invention reduces the C content as much as possible and controls it within the range of 0.04-0.10%.
[0011] In addition to ensuring strength, Si is also an important deoxidizing element during smelting. To ensure the effect, its addition amount should be above 0.10%, but at the same time, too high a content will have a negative impact on the surface quality and toughness of the steel plate. Therefore, in the present invention, the Si content is controlled in the range of 0.10-0.30% to ensure good toughness of the finished product.
[0012] Mn is an effective element for improving strength under low-carbon conditions. At the same time, it can reduce the austenite transformation temperature and refine the grain size, but its content is too high, which can easily cause serious segregation of the continuous casting billet and damage the low-temperature toughness. Therefore, the Mn content of low-carbon microalloyed steel is usually controlled below 2.5%. For example, the Mn content in the patent application number 202210829899.2 is limited to 1.20-1.60%. On the one hand, severe segregation is avoided. On the other hand, ultrafine ferrite and dispersed fine carbides are obtained through the fluctuation of the Mn element composition. Different from this, the present invention changes its thinking and focuses on the inherent Mn segregation phenomenon in the continuous casting billet. By utilizing its phase change characteristics, a novel dual-phase ultrafine grain microstructure with non-uniform layered distribution characteristics is prepared by designing a hot working route. Therefore, considering comprehensively, in order to ensure that there is an appropriate amount of Mn segregation in the continuous casting billet, the Mn content of the present invention should be controlled within the range of 1.00-2.20%.
[0013] On the basis of the aforementioned components, through thermal and kinetic simulation tests, and taking full account of the economy of the alloy elements and their influence on the comprehensive performance, the present invention designs a composite addition of four elements, namely: Ni: 0.20-0.60%, Cu: 0.40-0.70%, Nb: 0.015-0.045%, Ti: 0.005-0.030%.
[0014] P and S are harmful elements. From the perspective of clean steel, the lower the better. Considering the comprehensive economy, it is best to control the P content below 0.008% and the S content below 0.004%.
[0015] In some embodiments, considering the composite precipitation effect of Nb and Ti elements and the production cost, the content of Nb+Ti elements is controlled to be ≤0.045%; and because Cu and Ni are also stable supercooled austenite elements, they can affect the phase change characteristics of Mn segregation in the continuous casting billet, and the study also found that: the content of Mn+Ni+Cu in ultrafine-grained steel has an important influence on the stability of the process and the qualified rate of the finished product. Under the same process flow conditions, further controlling the content of Mn+Ni+Cu in ultrafine-grained steel to be ≤2.50% can ensure that it obtains more excellent and stable strength and toughness.
[0016] In some embodiments, there is chemical composition inhomogeneity between the ultrafine crystal layer and the coarse crystal layer, wherein the ultrafine crystal layer contains a higher content of Mn element than the coarse crystal layer.
[0017] In some embodiments, the volume fraction of the ultrafine crystal layer is 25-45%, the width of a single ultrafine crystal layer is 10-300 μm, and the average width is greater than 50 μm.
[0018] In some embodiments, the average grain size of the ultrafine crystal layer is 0.50-0.80 μm, and the grain size of the coarse crystal layer is less than 5.0 μm.
[0019] In some embodiments, the coarse-grained layer has a bimodal structure, wherein 5-25% of the grains have a size smaller than 1.0 μm, and 25-45% of the grains have a size larger than 3.0 μm.
[0020] In some embodiments, the crystal texture of the RD-ND plane varies in a gradient in the through-thickness direction, wherein: <110> / / The proportion of ND texture gradually decreases from 45-65% on the upper surface to 15-30% in the core; <111> / / ND gradually increases from 5-15% on the upper surface to 25-45% in the core.
[0021] In some embodiments, the volume fraction of martensite in the ultrafine grain layer is 20-35%, and the martensite is mainly (112) <110> The twin martensite has a twin thickness ranging from 4 to 15 nm.
[0022] In some embodiments, the yield strength of the ultrafine-grained steel is 500-700 MPa, the tensile strength is 800-1000 MPa, and the uniform elongation is 18-24%.
[0023] In some embodiments, the fracture toughness K of the ultrafine grain steel is Q 200~300MPa·m 1 / 2 , crack extension toughness K SS 250~350MPa·m 1 / 2 .
[0024] The method for preparing the above-mentioned non-uniform layered ultrafine-grained steel with excellent strength and toughness includes the following process flow:
[0025] S1 hot metal pretreatment → S2 converter smelting → S3 LF refining → S4 RH vacuum treatment → S5 continuous casting → S6 heating → S7 rough rolling → S8 intermediate cooling → S9 finishing rolling → S10 final cooling;
[0026] The heating time of S6 is less than 3 hours;
[0027] The S7 rough rolling has 3 to 5 passes and a reduction of 70 to 90%;
[0028] The intermediate-cooled steel billet in step S8 is cooled to room temperature at a cooling rate of 80 to 150 K / s;
[0029] The temperature of the S9 finishing rolling is in the austenite-ferrite two-phase region, the holding time is 1 to 3 hours, the rolling passes are 2 to 4 times, and the reduction is 60 to 80%;
[0030] The S10 final cooled steel billet is cooled to room temperature at a cooling rate of 50 to 70 K / s.
[0031] In some embodiments, the S6 heating temperature is 1323-1423K; the S7 rough rolling temperature is 1253-1323K; the S9 finishing rolling temperature is 993-1053K, and the final rolling temperature is 953-1013K.
[0032] In some embodiments, the S9 finishing rolling is asynchronous rolling, during which the upper roll speed is 0.5-2 m / s, and the lower roll speed is 0.55-4 m / s.
[0033] In some embodiments, the ratio of the lower roller speed to the upper roller speed is 1.1 to 2.0.
[0034] In some embodiments, the cumulative reduction of the S7 rough rolling and the S9 finishing rolling is ≥90%.
[0035] In some embodiments, the thickness ratio of the steel plate after S7 rough rolling to the finished product is 3.5 to 5.0.
[0036] In some embodiments, the reduction amount in each pass during the S7 rough rolling and the S9 finishing rolling is the same.
[0037] According to the above technical scheme, the present invention utilizes the inherent microscopic Mn segregation phenomenon in the continuous casting billet, and prepares a novel dual-phase ultrafine-grained microstructure with non-uniform layered distribution characteristics by designing a hot processing route. Compared with traditional steels with uniform microstructures, the present invention achieves a synergistic improvement in material strength and plasticity by rationally constructing a non-uniform layered structure in the material, while optimizing the fracture toughness and significantly improving the comprehensive service performance of the material, so that it can maintain stable performance in a variety of complex environments, meeting the urgent needs of modern industry for high-performance, cost-effective steel materials. In addition, the ultrafine-grained steel of the present invention uses conventional rolling and heat treatment equipment in the preparation process, which reduces the dependence on special equipment, is conducive to the large-scale promotion and application of the process, and shows important industrial application value and significant market potential.
[0038] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are listed below. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] The drawings described herein are used to provide a further understanding of the present invention and constitute a part of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:
[0040] Figure 1 is a process flow chart of some embodiments of the present invention;
[0041] Figure 2 is a schematic diagram of a non-uniform layered structure of some embodiments of the present invention;
[0042] Figure 3 are microstructure diagrams of some embodiments of the present invention. DETAILED DESCRIPTION
[0043] The technical scheme of the present invention will be clearly and completely described below in conjunction with the accompanying drawings and specific embodiments, but those skilled in the art will understand that the embodiments described below are part of the embodiments of the present invention, rather than all of the embodiments, and are only used to illustrate the present invention, and should not be considered to limit the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present invention. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products or detection services that can be purchased commercially.
[0044] The billet size obtained after the process flow S1 molten iron pretreatment → S2 converter smelting → S3 LF refining → S4 RH vacuum treatment → S5 continuous casting is 120×80×50mm 3 (length × width × thickness), the specific composition is shown in Table 1. The microstructure and properties of the steel billet will be regulated through the process flow of S6 heating → S7 rough rolling → S8 intermediate cooling → S9 finishing rolling → S10 final cooling.
[0045] For comparison, coarse-grained steel of Comparative Example 1 and ultrafine-grained steel of Comparative Example 2 with the same composition were prepared at the same time. The steel billets of the two comparative examples were subjected to a long-term homogenization treatment at 1373K / 24h before rolling to minimize the segregation band in the steel billet. For the present invention, in order to ensure a certain Mn segregation band content, the heating time of process S6 should be less than 3h, such as Figure 1 As shown, the heating time in the embodiment is 2 hours to achieve uniform austenitization.
[0046] In the present invention, a large reduction technology is adopted in the S7 rough rolling stage, that is: through 3 to 5 rolling passes, the cumulative reduction is controlled to 70 to 90% to crush the austenite grains and prepare the organization for the subsequent fine grain size; therefore, the rough rolling temperature is slightly higher and is controlled at 1253 to 1323K. Controlled cooling, as an important component of TMCP technology, is a key factor affecting the evolution of the microstructure of the steel billet after rolling. The cooling rate of the S8 intermediate cooling after rough rolling of the present invention is 80 to 150K / s. Under this cooling rate condition, due to the low C content and alloy element content in the steel plate, the hardenability is low, and after cooling to room temperature, a bainite-based matrix organization is formed; and because the steel billet has not undergone a long-term annealing treatment before hot rolling, it can be observed that there is an obvious Mn segregation band distributed along the rolling direction in the bainite matrix.
[0047] It was found that higher Mn content in the local microstructure of the steel lowers the phase transformation point from ferrite to austenite and preferentially transforms to austenite during heating. Therefore, in the present invention, during S9 finishing rolling, when the steel plate is heated to the austenite-ferrite two-phase region for the second time, local Mn-rich regions such as Mn segregation bands and grain boundaries will preferentially transform into austenite and retain element segregation. Further, after a holding time of 1 to 3 hours, austenite recrystallization will be suppressed in this region during rolling at a relatively low temperature, forming a grain morphology elongated along the rolling direction. At the same time, combined with a large reduction of 60 to 80% after 2 to 4 rolling passes and a cooling rate of 50 to 70 K / s in the S10 final cooling, a mixed ultrafine grain structure of martensite and ferrite cells is finally obtained; and the micron-sized near-equiaxed ferrite in the coarse-grained layer originates from the recrystallization of the untransformed bainite matrix during the warm rolling process at a relatively low temperature, and finally forms a unique bimodal structure of the coarse-grained layer, that is, some fine ultrafine grains are distributed at the intersection of grain boundaries on the coarse-grained matrix.
[0048] In addition, the study found that texture gradient has an important influence on HDI strengthening. Unlike conventional rolling, the asynchronous rolling process causes the surface of the steel plate to bear greater shear strain, and the reasonable setting of the upper and lower roller speeds is conducive to forming an ideal texture gradient structure in the steel plate, thereby improving the strength of the steel plate. Therefore, the S9 finishing rolling process in the present invention adopts asynchronous rolling, preferably controlling the upper roller speed to 0.5-2m / s, the lower roller speed to 0.55-4m / s, and the ratio of the lower roller speed to the upper roller speed to 1.1-2.0, so as to obtain a gradient change in the crystal texture in the steel plate.
[0049] Based on the above-mentioned components and process design, the non-uniform layered ultrafine-grained structure rationally constructed in the present invention can, on the one hand, produce HDI stress through the synergistic deformation mechanism, thereby obtaining an additional strengthening effect and ultimately improving the strength-plasticity matching of the steel plate; on the other hand, the layered structure of the alternating distribution of coarse-grained / ultrafine-grained layers and the elongated grain morphology in the ultrafine-grained layers can effectively hinder crack propagation and void connection, thereby increasing the energy dissipation rate, while the micron-sized ferrite in the coarse-grained layer has a higher tolerance to plastic deformation, can form deep dimples of larger size, and consume a large amount of energy when the crack propagates, ultimately effectively improving the fracture toughness of the steel plate through the combined action of the above mechanisms.
[0050] Reference Figure 1 The controlled rolling and controlled cooling process of the test steel in the embodiment of the present invention is specifically as follows:
[0051] The rough rolling temperature of S7 is about 1273K. After 4 rolling passes, the thickness of the steel billet is reduced to 10mm, in which the thickness is reduced by 10mm in each pass, and the cumulative reduction reaches 80%. Then, the cooling rate is controlled at about 100K / s to water cool the steel plate to room temperature, so that the steel plate obtains fine bainite structure under the conditions of large reduction and high cooling rate.
[0052] Furthermore, the steel plate was reheated to 1023K (austenite-ferrite two-phase region) in the S9 finishing process and kept warm for 1.5h, and then warmed on an asynchronous rolling mill. The upper and lower roller speeds during rolling were 1m / s and 1.5m / s respectively. The rolling process was performed for a total of 3 passes. The final thickness of the steel plate was about 2.5mm, with a reduction thickness of 2.5mm in each pass. The cumulative reduction of the final rough rolling and finishing rolling was as high as 95%. In order to ensure a fine grain size and comprehensively consider the load of the rolling mill, the final rolling temperature was controlled to be about 983K, and then the steel plate was water-cooled to room temperature at a cooling rate of about 60K / s. It should be noted that as the final process of production, the cooling rate of final cooling has a huge impact on the service performance of the steel plate. In the present invention, if the cooling rate is lower than 50K / s, on the one hand, it will affect the martensitic transformation of the final ultrafine grain layer, and on the other hand, it is not conducive to obtaining a fine grain size in the steel plate; and when the cooling rate is higher than 70K / s, the service performance of the steel plate will deteriorate due to the large quenching stress inside; therefore, the cooling rate of S10 final cooling should be controlled in the range of 50 to 70K / s.
[0053] Under the composition design system of the present invention, the overall grain size of the ultrafine-grained steel prepared by process optimization is relatively small. The non-uniform layered structure characteristics of the RD-ND plane in the full thickness macroscopic view of the test steel of the present invention are as follows: Figure 2 As shown in the figure, within the 2.5 mm range of the longitudinal section, the ultrafine grain layer is unevenly distributed on it. Due to the different density of grain boundaries, the ultrafine grain layer appears "convex" in the SEM image after corrosion, as shown in the figure. Figure 3 As shown in (a), the ultrafine-grained layer is a mixed ultrafine-grained structure of martensite and ferrite cells; while the coarse-grained layer is mainly a micron-sized near-equiaxed ferrite structure. The short arrows in the figure indicate that there are some tiny ultrafine grains distributed at the intersection of the grain boundaries on the coarse-grained matrix. Figure 3(b) Grain boundary map. Statistics show that the volume fraction of the ultrafine layer is about 36%, the average grain size is only 0.6μm, and the grain size of the coarse layer is also less than 5.0μm. The coarse layer also has a bimodal structure: some tiny ultrafine grains are distributed at the intersection of the grain boundaries on the coarse matrix, among which: ~10% of the grain size is less than 1.0μm, and ~34% of the grain size is greater than 3.0μm. In addition, the EBSD experimental results show that the crystal texture of the RD-ND plane in the full thickness direction of the test steel in the embodiment also has a gradient change: <110> / / The proportion of ND texture gradually decreases from 58% in the upper surface to 25% in the core; <111> / / ND gradually increases from 6% on the upper surface to 33% in the core; further TEM experimental results show that the ultrafine grain layer in the test steel of the embodiment contains a high density of dislocations, and the long ultrafine grains are mainly composed of nano / ultrafine martensite and ferrite cells, of which the volume fraction of martensite is about 29.3%, mainly (112) <110> The twin martensite has a twin thickness ranging from 4 to 15 nm.
[0054] The present invention utilizes the phase change characteristics of Mn segregation in the continuous casting billet, and through process control, the Mn segregation band area can be made different from the matrix area to obtain a different microstructure. The element detection results show that this Mn segregation can still be observed in the final non-uniform layered structure of the test steel of the embodiment of the present invention, that is, the ultrafine grain area of the double peak structure in the ultrafine grain layer and the coarse grain layer can be observed to have a higher Mn content than the coarse grain area; and the study found that the content, distribution, size, etc. of the ideal Mn segregation band obtained in the continuous casting billet through composition and process design are also closely related to the content, distribution, size, etc. of the final ultrafine grain layer. For example: similar to the Mn segregation band, the width of the ultrafine grain layer in the test steel of the embodiment is also different in size and unevenly distributed. The statistical results show that the width of a single ultrafine grain layer is in the range of 10 to 300 μm, and the average width is 53 μm.
[0055] Through conventional process regulation, the microstructure of the coarse-grained steel of Comparative Example 1 is mainly a nearly equiaxed ferrite-martensite dual-phase structure with an average grain size of about 2.9 μm; the microstructure of the ultrafine-grained steel of Comparative Example 2 is mainly composed of a martensite matrix and cementite, the original austenite grain boundaries are vaguely visible, the width of the martensite laths is about 200 to 300 nm, and it has a higher dislocation density.
[0056] The specific tensile properties of the test steels of the embodiment and the comparative example are summarized in Table 2. It can be seen that the coarse-grained steel of comparative example 1 has the lowest strength, which is 386MPa, but its uniform elongation is the highest, reaching 13.9%; the ultrafine-grained steel of comparative example 2 with a single-phase martensite matrix has the highest yield strength, which is 751MPa, but its uniform elongation is the lowest, which is only 4.3%; and the test steel of the embodiment with a non-uniform layered ultrafine grain structure shows the best strength-plasticity match, with a yield strength of 545MPa, which is about 41.2% higher than the coarse-grained steel of comparative example 1. At the same time, the uniform elongation of the test steel of the embodiment is 11.5%, which is about 2.7 times that of the ultrafine-grained steel of comparative example 2. It is worth noting that the tensile strength of the test steel of the embodiment reaches 880MPa, which is the highest among the three test steels, and even 77MPa higher than the ultrafine-grained steel of comparative example 2, which comes from its excellent work hardening ability.
[0057] According to the standard ASTM E1820, single-sided bending specimens were prepared along the rolling directions of three test steel plates to test the fracture toughness of the material, thereby effectively evaluating the damage tolerance of structural materials during crack initiation and propagation. As shown in the results in the table, the test steel in the embodiment has the best crack initiation toughness, and its K Q 240.2MPa·m 1 / 2 , which is 14.8% and 32.9% higher than that of the test steels in Comparative Example 1 and Comparative Example 2. When the crack Δa expands to about 0.8 mm, the crack extension toughness K SS 262.4MPa·m 1 / 2 and 240.7MPa m 1 / 2 , while the K of the test steel in the example SS Increased to 302.4MPa·m 1 / 2 The above results show that the experimental steel with non-uniform layered ultrafine grain structure has the best fracture toughness.
[0058] Based on the above results, the test steel of the embodiment of the present invention has better strength-ductility-toughness matching and excellent comprehensive service performance.
[0059] Table 1 Chemical composition of three test steels (mass fraction / %)
[0060]
[0061] Table 2 Room temperature mechanical properties of three test steels
[0062]
[0063] The terms "including" and "having" and any variations thereof in the specification and claims of the present invention and the above-mentioned drawings are intended to cover non-exclusive inclusions. For example, a process, method, system, product or apparatus comprising a series of steps or units is not necessarily limited to those steps or units explicitly listed, but may include other steps or units not explicitly listed or inherent to these processes, methods, products or apparatuses.
[0064] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the purpose and scope of the technical solution, which should be included in the scope of the claims of the present invention.
Claims
1. A non-uniform layered ultrafine grain steel with excellent strength and toughness, characterized in that: The chemical composition of the ultrafine grain steel includes, by mass percentage, C: 0.04-0.10%, Si: 0.10-0.30%, Mn: 1.00-2.20%, P: ≤0.008%, S: ≤0.004%, Ni: 0.20-0.60%, Cu: 0.40-0.70%, Nb: 0.015-0.045%, Ti: 0.005-0.030%, and the rest is Fe and unavoidable impurities; the RD-ND surface of the ultrafine grain steel shows the characteristics of non-uniform alternating distribution of ultrafine grain layers and coarse grain layers in the full thickness macroscopically.
2. The ultrafine grain steel according to claim 1, characterized in that: The chemical composition of the ultrafine grain steel is Nb+Ti:≤0.045%, and Mn+Ni+Cu:≤2.50%.
3. The ultrafine grain steel according to claim 1, characterized in that: There is chemical composition inhomogeneity between the ultrafine crystal layer and the coarse crystal layer, wherein the ultrafine crystal layer contains a higher content of Mn element than the coarse crystal layer.
4. The ultrafine grain steel according to claim 1, characterized in that: The volume fraction of the ultrafine crystal layer is 25-45%, the width of a single ultrafine crystal layer is 10-300 μm, and the average width is greater than 50 μm.
5. The ultrafine grain steel according to claim 1, characterized in that: The average grain size of the ultrafine crystal layer is 0.50-0.80 μm, and the grain size of the coarse crystal layer is less than 5.0 μm.
6. The ultrafine grain steel according to claim 5, characterized in that: The coarse-grained layer has a bimodal structure characteristic, wherein 5-25% of the grains have a size smaller than 1.0 μm, and 25-45% of the grains have a size larger than 3.0 μm.
7. The ultrafine grain steel according to claim 1, characterized in that: The crystal texture of the RD-ND surface changes gradually in the full thickness direction, wherein: <110> / / The proportion of ND texture gradually decreases from 45-65% on the upper surface to 15-30% in the core; <111> / / ND gradually increases from 5-15% on the upper surface to 25-45% in the core.
8. The ultrafine grain steel according to claim 1, characterized in that: The volume fraction of martensite in the ultrafine grain layer is 20-35%, and the martensite is mainly (112) <110> The twin martensite has a twin thickness ranging from 4 to 15 nm.
9. The ultrafine grain steel according to claim 1, characterized in that: The yield strength of the ultrafine-grained steel is 500-700 MPa, the tensile strength is 800-1000 MPa, and the uniform elongation is 18-24%.
10. The ultrafine grain steel according to claim 1, characterized in that: The fracture toughness K of the ultrafine grain steel Q 200~300MPa·m 1 / 2 , crack extension toughness K SS 250~350MPa·m 1 / 2 .
11. A method for preparing ultrafine grain steel according to any one of claims 1 to 10, characterized in that: The process flow of the preparation method comprises: S1 molten iron pretreatment → S2 converter smelting → S3 LF refining → S4 RH vacuum treatment → S5 continuous casting → S6 heating → S7 rough rolling → S8 intermediate cooling → S9 finishing rolling → S10 final cooling; The heating time of S6 is less than 3 hours; The S7 rough rolling has 3 to 5 passes and a reduction of 70 to 90%; The intermediate-cooled steel billet in step S8 is cooled to room temperature at a cooling rate of 80 to 150 K / s; The temperature of the S9 finishing rolling is in the austenite-ferrite two-phase region, the holding time is 1 to 3 hours, the rolling passes are 2 to 4 times, and the reduction is 60 to 80%; The S10 final cooled steel billet is cooled to room temperature at a cooling rate of 50 to 70 K / s.
12. The method for preparing ultrafine grain steel according to claim 11, characterized in that: The temperature of the S6 heating is 1323-1423K; the temperature of the S7 rough rolling is 1253-1323K; the temperature of the S9 finishing rolling is 993-1053K, and the final rolling temperature is 953-1013K.
13. The method for preparing ultrafine grain steel according to claim 11, characterized in that: The S9 finishing rolling is asynchronous rolling, during which the upper roll speed is 0.5-2 m / s, and the lower roll speed is 0.55-4 m / s.
14. The method for preparing ultrafine grain steel according to claim 13, characterized in that: The ratio of the lower roller speed to the upper roller speed is 1.1 to 2.
0.
15. The method for preparing ultrafine grain steel according to claim 11, characterized in that: The cumulative reduction of the S7 rough rolling and the S9 finishing rolling is ≥90%.
16. The method for preparing ultrafine grain steel according to claim 11, characterized in that: The thickness ratio of the steel plate after S7 rough rolling to the finished product is 3.5 to 5.
0.
17. The method for preparing ultrafine grain steel according to claim 11, characterized in that: The reduction amount in each pass during the S7 rough rolling and S9 finishing rolling is the same.
Citation Information
Patent Citations
Low-carbon bainite steel plate for large line energy welding and manufacturing method of low-carbon bainite steel plate
CN108677088A
Low-carbon micro-alloy steel with gradient ultra-fine grain structure and preparation method for same
CN109735766A
Engineering heat treatment method of ultrahigh-strength steel for compressor impeller
CN114150233A
Ultrafine grain steel plate and preparation method thereof
CN115323265A
Fe-BASED METAL PLATE
JP2016183359A