Timepiece component and method for manufacturing same

Through injection molding and laser ablation technology, the formation of watch parts with relief and different colors/textures solves the problem of difficulty in manufacturing durable and beautiful watch parts in the prior art, and achieves high precision and multi-sensory experience effects.

CN119087770APending Publication Date: 2024-12-06ROLEX SA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410716900.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-06-05
Filing Date
2024-06-04
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The prior art is difficult to effectively manufacture watch parts with embossed parts and different colors/textures, and it is difficult to provide a durable, aesthetic and multi-sensory experience.

Method used

Injection molding is used to form a rough blank, cover the coating, and part of the coating is removed by laser ablation and textured to form watch parts with relief, different colors and textures.

Benefits of technology

Achieving high-precision, environmental stress resistance and high hardness watch components, providing a durable and beautiful appearance and allowing for a multi-sensory experience.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119087770A_ABST
    Figure CN119087770A_ABST
Patent Text Reader

Abstract

The invention relates to a method for producing a timepiece component, comprising the following steps: (10) forming a blank (200E1), in particular by injection molding, comprising at least one base surface (210) and at least one projection (220) projecting from the base surface (210), (20) forming at least one coating (250), the at least one coating (250) covers at least a part of the base surface (210) and / or at least a part of the at least one projection (220), (30) removes at least a part of the at least one coating (250) by laser ablation, (40) is treated by laser, at least a portion of the base surface (210) and / or at least a portion of the projections (220) and / or at least a portion of the at least one coating (250) are textured.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates generally to the manufacture of timepiece components and in particular the invention may relate to the manufacture of timepiece components having portions in relief and portions covered by a coating. Background Art

[0002] In the prior art of watch parts with embossed parts, European patent document EP 3 892151A1 is known, which discloses a watch part with a coating covering part, and may include embossed decorative inserts. However, the document does not propose a solution to texturize certain parts of the parts, nor does it propose the same parts with embossed parts, which have a special appearance relative to the base of the parts. Such watch parts (with coatings and embossed parts) are usually used as visible parts of watches, so they should be made accurately and reliably to ensure that the most beautiful appearance is continuously provided to users. Patent document WO2018109065A1 relates to a method for manufacturing a non-conductive material protective element or dial, wherein a base made of non-conductive material is covered with a resin sacrificial layer that is etched and then mechanically polished, and the resin sacrificial layer is finally dissolved by a chemical method. Summary of the invention

[0003] One object of the present invention is to improve the prior art as described above and, in particular, to first propose a method for manufacturing a timepiece component, which method allows to efficiently, quickly, accurately and robustly prepare a timepiece component with a relief portion and a portion of a different color and / or a different texture, thereby providing the user with a timepiece component with a durable and beautiful appearance. The present invention also aims to propose a timepiece component with a raised or embossed portion and a portion of a different color and / or a different texture, thereby providing the user with a timepiece component with an aesthetic appearance, which is durable and has a pleasant tactile sensation that allows a multi-sensory experience of the pattern.

[0004] To this end, a first aspect of the invention relates to a method for manufacturing a timepiece component, comprising the following steps:

[0005] - forming a blank, in particular by injection molding, the blank comprising at least one base surface and at least one projection protruding from the base surface,

[0006] - forming at least one coating layer covering at least a portion of the base surface and / or covering at least a portion of at least one protrusion,

[0007] - removing at least a portion of said at least one coating layer by laser ablation,

[0008] At least a portion of the base surface previously covered with at least one coating and / or at least a portion of at least one elevation previously covered with at least one coating and / or at least a portion of at least one coating is textured by laser treatment.

[0009] The method according to the above embodiment comprises the step of covering the base surface and at least one protrusion with a coating, and then comprises the step of removing the coating or at least one coating and texturing the visible surface of the component. Thus, a watch component having a protruding or embossed portion, a coating-covered portion and a textured portion can be proposed, the component having a beautiful appearance and / or a very high manufacturing accuracy, because the coating delimitation and / or texturing is completed by laser processing. Blanks and / or coating materials resistant to environmental stress or impact, high wear resistance and / or high hardness can also be proposed, and laser processing can easily remove the coating or at least one coating and / or texture the blank. It can be noted that at least one coating can be formed, which covers at least a portion of the base surface and / or at least a portion of at least one protrusion, that is, a single-layer coating can be formed, but two, three or even more layers of coating can also be formed. It can be considered that some layers of the coating cover all parts of the rough blank, or all parts visible to the user. It can also be considered that some layers of the coating partially cover the rough blank or partially cover the parts visible to the user.

[0010] The manufacturing method and / or the timepiece component may also have one or more of the following features, used alone or in combination.

[0011] According to one embodiment, the step of removal by laser ablation and the step of texturing by laser treatment are at least partially carried out simultaneously and / or are performed using the same laser source. In particular, it is conceivable that, on the portion where the entire coating is removed, a texture is formed on the previously coated material during the same single laser beam operation or during the same multiple laser beam operations to remove the coating on the watch component. In other words, the removal step and the texturing step are carried out simultaneously in the same irradiation operation, during the same single operation of the laser beam. A very high precision is thus obtained, since the boundaries of the coated areas correspond to the boundaries of the textured areas: there is no offset or "neither coated nor textured" area between the coated and textured areas. In other words, the laser ablation of the coating is carried out simultaneously with the texturing, and this allows reaching the bare textured surface directly from the coated surface. In other words, the step of removing by laser ablation and the step of texturing by laser treatment are carried out at least partially simultaneously, that is, they are carried out simultaneously and / or the laser beam irradiating the part (i.e., the laser beam is irradiated in one single operation) has the result that at least one layer of coating is removed and at least a portion of the base surface previously covered with at least one layer of coating and / or at least a portion of at least one protrusion previously covered with at least one layer of coating and / or at least a portion of at least one layer of coating is texturized simultaneously.

[0012] According to one embodiment, the step of removing by laser ablation is performed such that:

[0013] - locally removing the total thickness of the coating and optionally the thickness of the blank starting from the base surface, and / or

[0014] - local removal of a coating thickness that is less than the total coating thickness, and / or

[0015] - Local removal of a variable thickness of the coating that is much smaller than the total thickness of the coating. The ablation and / or texturing process performed using a laser source allows multiple removals and / or texturings of the same part: at certain locations, the removal of the entire coating can be considered, with the possibility of texturing the rough material at other locations, partial removal of the coating, i.e. only certain layers of the coating can be considered, while at other locations, the removal of a variable part of the coating can be considered, and finally at other locations, texturing of the coating can be considered.

[0016] Preferably, the removal step is performed simultaneously with the texturing step and / or is performed using the same laser source as the texturing step. According to a specific embodiment, the two steps are performed on a coating covering at least a portion of the base surface, at least a portion of the surface forming the top of the at least one projection, at least a portion of the surface forming the side of the at least one projection, and the two steps are aimed at removing the coating covering at least a portion of the base surface, and texturing at least a portion of the base surface. According to this embodiment, at least one projection is coated (preferably coated entirely) with at least one layer of said coating, wherein the base surface of the rough blank is uncoated (preferably uncoated entirely), and the base surface of the rough blank is textured (preferably textured entirely). According to this embodiment, there is no transition or offset zone between the coated area and the textured area, because at the originally coated base surface, the removal of the coating and the texturing of the material are performed as the same laser processing operation: the uncoated area is textured at the same time.

[0017] According to one embodiment, the step of removing by laser ablation and / or the step of texturing by laser treatment are performed on the side of the protruding portion. In particular, the step of removing by laser ablation and / or the step of texturing by laser treatment can be performed on the side of the protruding portion, and the protruding portion forms a clearance angle relative to the normal of the base surface, preferably between 5° and 25°, specifically between 10° and 20°.

[0018] According to one embodiment, the laser texturing of the side surfaces can be different from the laser texturing of the base and / or top surfaces of the projections. In other words, the coating on the side, base and / or top surfaces of the projections and the blank material of the blank are textured in different, specific or unique ways.

[0019] According to one embodiment, the at least one protrusion forms a closed pattern, such as an "O" (letter O) or a "0" (zero), or any other closed pattern or decoration. "Closed pattern" refers in particular to any pattern that comprises a part of a closed pattern, such as a "4" or a "9". According to one embodiment, the closed pattern comprises or has an inner surface, such as being arranged at the same height as or aligned with the at least one base surface. According to one embodiment, a coating is formed on the inner surface. According to one embodiment, the coating formed on the inner surface is at least partially removed by laser ablation and / or at least partially textured by laser treatment. Preferably, when the coating formed on the inner surface is at least partially removed, the inner surface is at least partially textured. Therefore, the step of at least partially ablating the coating formed on the inner surface and the step of texturing the inner surface can be performed simultaneously.

[0020] According to one embodiment, the at least one protrusion forms or has at least two reliefs with a spacing of less than 5 mm, less than 3 mm or less than 2 mm.

[0021] According to one embodiment, the step of removing by laser ablation and / or the step of texturing by laser treatment is performed using an ultrashort pulse laser source, and preferably using a pulsed laser source arranged to emit nanosecond pulses, more preferably picosecond pulses, even more preferably femtosecond pulses. Such a laser source allows high-precision treatment and / or no thermal impact on the rest of the part. Generally, it is conceivable to generate a relative movement between the watch component and the laser source by means of a moving stage and / or a moving mirror.

[0022] According to one embodiment, the manufacturing method may comprise a step of machining and / or grinding the rough blank, which is performed at the end of the step of forming the rough blank, in particular between the step of forming the rough blank and the step of forming at least one layer of said coating. It is generally conceivable to machine and / or grind the entire or part of the functional surface of the timepiece component before performing the coating, but it is also possible to machine / grind the surface of the timepiece component at other times.

[0023] According to one embodiment, the manufacturing method may comprise a step of grinding the rough blank, said step being performed at the end of the step of forming the rough blank, in particular between the step of forming the rough blank and the step of forming at least one layer of said coating. The grinding step generally causes a change in the surface state, in particular a change in the roughness, and / or a change in the surface appearance, such as a change in the glossiness. It is generally conceivable to grind the entire or part of the visible surface of the timepiece component before forming at least one coating, but it is also possible to grind the surface of the timepiece component at other times.

[0024] According to one embodiment, the step of forming at least one coating layer comprises a physical vapor deposition (PVD deposition) step, and / or a chemical vapor deposition (CVD deposition) step, and / or an atomic layer deposition (ALD deposition) step. Such methods allow the formation of very hard coatings (for example, with a hardness higher than 500 HV, preferably higher than 1000 HV, even preferably higher than 1500 HV), and / or with a specific color or at least different from the color of the base material of the rough blank. In other words, at least one coating layer is a decorative layer, and the rest is intended to form the outer surface of the watch component (subject to friction, impact, moisture, etc.).

[0025] According to one embodiment, the forming green body step is performed to form a green body comprising a ceramic material and / or a metallic material and / or a cermet. A cermet is generally a material having a ceramic skeleton in which a metallic phase is present.

[0026] According to one embodiment, the step of forming at least one coating layer includes forming at least one ceramic material layer and / or at least one material layer containing a metal compound.

[0027] According to one embodiment, the step of forming at least one coating layer comprises forming at least one layer comprising:

[0028] - metal carbides, in particular tungsten carbide and / or titanium carbide, and / or zirconium carbide, and / or tantalum carbide, and / or niobium carbide, and / or chromium carbide, and / or hafnium carbide, and / or

[0029] - at least one metal nitride, in particular chromium nitride and / or boron nitride, and / or zirconium nitride, and / or titanium nitride, and / or tantalum nitride, and / or niobium nitride, and / or hafnium nitride, and / or

[0030] - A combination of the above-mentioned various metal carbides and / or a combination of the above-mentioned various metal nitrides, and / or an alloy combination of the above-mentioned metal nitrides and the above-mentioned metal carbides.

[0031] According to one embodiment, the metal of the coating layer is selected from tungsten (W), and / or titanium (Ti), and / or zirconium (Zr), and / or tantalum (Ta), and / or niobium (Nb), and / or chromium (Cr), and / or hafnium (Hf), and / or gold (Au) and / or palladium (Pd), and / or platinum (Pt), or their alloys, such as titanium aluminum (TiAl), chromium aluminum (CrAl), and hafnium titanium (HfTi) alloys.

[0032] According to one embodiment, the texturizing step is used to texturize at least one layer of coating and / or the base surface and / or the protrusions by forming a satin finish, and / or a brush finish, and / or a snail finish, and / or a sunburst finish, and / or at least one Côtes de Genève finish, and / or a pearlescent finish, and / or a ring finish and / or any type of decoration, in particular a repeating patterned decoration.

[0033] According to one embodiment, the at least one base surface is a conical or dome-shaped or convex surface. In particular, the at least one base surface may not be a plane. According to one embodiment, the at least one protrusion has a conical or dome-shaped or convex upper surface. In particular, the at least one upper surface may not be a plane.

[0034] A second aspect of the present invention may relate to a method of manufacturing a timepiece, comprising the following steps:

[0035] - providing a timepiece component manufactured according to the manufacturing method of the first aspect of the invention,

[0036] - assembling the timepiece component into a timepiece so as to place at least a portion of the timepiece component in a visible part of the timepiece, wherein:

[0037] - at least one of said coatings has been at least partially removed and / or textured, and / or

[0038] The base surface and / or at least one of the projections is textured.

[0039] A third aspect of the invention may relate to a timepiece component intended to be mounted in a timepiece, the timepiece component comprising a body, or in the form of a body, formed from a blank according to the manufacturing method of the first aspect of the invention. According to one embodiment, the timepiece component may be an assembly of several parts. In particular, the timepiece component may be a watch bezel of a single part, or the timepiece component may be a watch bezel comprising, for example, a bezel ring (base) and a bezel plate (attached or knocked into or embedded in the bezel ring).

[0040] According to one embodiment, the body comprises a base, at least one protrusion or relief protruding relative to the base, and comprises a top and at least one side arranged between the base and the top. The top preferably has a surface parallel to the base, but may also have a surface not parallel to the base. The top of the body and the at least one side of the protrusion are covered by a coating formed by the manufacturing method according to the first aspect of the present invention, and the base of the body is textured by the manufacturing method according to the first aspect of the present invention.

[0041] In other words, the watch components include:

[0042] The main body includes:

[0043] - base surface,

[0044] at least one raised portion or relief portion protruding relative to said base surface and comprising a top portion and at least one side portion arranged between the base surface and the top portion,

[0045] wherein the top and the at least one side are covered with a coating (at least one coating), and wherein the base surface is textured,

[0046] - the base surface is coated simultaneously with the top surface and the at least one side surface,

[0047] The coating of the base surface is removed by a laser treatment which is also used (preferably simultaneously) for texturing the base surface and which uses a laser source emitting ultrashort pulses (nanosecond, picosecond or femtosecond range).

[0048] According to the above-described embodiment, a timepiece component is obtained having at least one coated protrusion, in particular having a plurality of coated protrusions (including end portions and side surfaces), and a textured base surface, without intermediate transition zones between these surfaces.

[0049] According to one embodiment, the timepiece component may form a protective part of the timepiece, such as a bezel, or a bezel plate, or a dial, or a crown, a push button or a buckle.

[0050] According to one embodiment, at least one protrusion comprises at least one top and a side surface arranged between the top of at least one protrusion and the base surface, and wherein the at least one side surface forms a back angle with the normal of the base surface, preferably between 5° and 25°, specifically between 10° and 20°. BRIEF DESCRIPTION OF THE DRAWINGS

[0051] Other features and advantages of the present invention will become more apparent from the following detailed description of embodiments of the invention, which are described by way of non-limiting examples and illustrated in the accompanying drawings.

[0052] Figure 1 shows a perspective portion of a timepiece comprising a timepiece component according to the invention, in this particular example forming a bezel plate of the timepiece;

[0053] Figure 2 Shows Figure 1 A perspective view of the bezel of a clock in

[0054] Figure 3a Shows Figure 2 A simplified schematic diagram of a method for manufacturing a bezel plate in the first step;

[0055] Figure 3b Shows Figure 2 The second step of the simplified schematic diagram of the method for manufacturing the bezel plate;

[0056] Figure 3c Shows Figure 2 The third step of the simplified schematic diagram of the method for manufacturing the bezel plate;

[0057] Figure 4Shown in Figure 3a In the first step of the manufacturing method, Figure 2 A section of the bezel disk along the axis II-II of the figure;

[0058] Figure 5 Shown in Figure 3b In the second step of the manufacturing method, Figure 4 The cross section of

[0059] Figure 6 Shown in Figure 3c In a first variation of the third step of the manufacturing method, Figure 4 The cross section of

[0060] Figure 7 Shown in Figure 3c In a second variation of the third step of the manufacturing method, Figure 4 The cross section of

[0061] Figure 8 Shown in Figure 3c In a third variation of the third step of the manufacturing method, Figure 4 cross section. DETAILED DESCRIPTION

[0062] Figure 1 A perspective portion of a timepiece P is shown, generally comprising;

[0063] -Case 100,

[0064] a timepiece component according to the invention, in this particular example forming a bezel, said bezel comprising a dial 200 connected to a bezel ring 230 notched and mounted in rotation on case 100,

[0065] - Display interface 300, which may include a dial, hour markers, hands and numbers, to provide the user with hour and minute indications.

[0066] Figure 2 Shows Figure 1 A perspective view of a bezel plate 200 of a timepiece P in FIG. The bezel plate 200 comprises:

[0067] - base surface 210,

[0068] - protrusions 220 protruding from the base surface 210, where the numbers and hour markers are formed. Figure 2 As can be seen in the example in FIG. 1 , the bezel is a rotating part and the base surface 210 inclined relative to the axis of rotation is conical.

[0069] Figure 2 The bezel plate 200 in the embodiment is provided in combination with a bezel ring 230 including a side portion, the bezel ring having a bezel ring 230 having a side portion. Figure 1The notch shown allows the user to Figure 1 The case 100 of the timepiece P in the embodiment of the present invention rotates the bezel.

[0070] Of course, the bezel plate 200 and / or more specifically the bezel ring 230 may include a functional surface as a bottom surface that is processed to allow for Figure 1 The watch ring can be rotatably connected and installed on the watch case 100 of the watch P. Alternatively, the watch ring can be fixed to the watch case 100.

[0071] The present disclosure is intended to propose that the bezel plate 200 is modified by a raised or embossed pattern and a different color and / or texture on the base, but for the sake of clarity, Figure 1 and Figure 2 These different colors and / or textures are not shown. For this purpose, see Figure 3c (or Figures 6 to 8 ), which shows different aspects between the surfaces of the manufactured part.

[0072] Therefore, the present disclosure relates to a timepiece component, such as Figure 2 The bezel plate 200 in the embodiment of the present invention may specifically relate to a bezel or a dial having a colored raised or positive relief pattern on its base, such as a textured ceramic or metal material.

[0073] To this end, in order to specifically obtain the bezel plate 200, the present disclosure relates to a method comprising in particular Figure 3a to Figure 3c The successive steps are shown very schematically in FIG. 1 and are described as follows:

[0074] -(10- Figure 3a ): forming a blank 200E1, in particular by injection molding, comprising at least one base surface 210 and at least one protrusion 220 protruding from the base surface 210,

[0075] -(20- Figure 3b ): forming at least one coating layer 250, covering at least a portion of the base surface 210 and / or at least a portion of the protrusion 220, to obtain a rough blank 200E2 with a coating,

[0076] -(30- Figure 3c ): removing at least a portion of at least one layer of the coating 250 by laser ablation, and preferably simultaneously

[0077] (40): Texturing at least a portion of the base surface 210 previously covered with the coating 250 or at least one coating layer by laser treatment to obtain the bezel plate 200.

[0078] The above description of the manufacturing method lists the main steps of the method and lists the following features in detail.

[0079] The first step 10 is therefore to obtain a blank 200E1 having a protrusion 220 .

[0080] According to the first embodiment and the first sub-step of step 10 of forming the blank 200E1, the blank 200E1 can be obtained by a molding process such as injection molding or pressing.

[0081] The injected component material can be a metal, a composite material, a metal ceramic or an engineering ceramic. Advantageously, the engineering ceramic can be mostly or mainly (by mass or mole) composed of zirconium oxide and / or aluminum oxide. Therefore, zirconium oxide and / or aluminum oxide may be the main elements in the ceramic. Various elements known to those skilled in the art can be added to this engineering ceramic to improve its performance, such as Hf, Y, Al, Si, Mg, Fe, Ni, Cr, Zn, Co, Mn, Cu, Ti, Ta, W, Pt. Yttrium zirconium oxide (2Y-ZrO2 or 3Y-ZrO2) as described in patent application WO2022101450 can be used for the rough blank of watch parts. Alternatively, the engineering ceramic used can be made of glass, sapphire or mineral materials, for example.

[0082] If it is a metal, the injection molding may include injecting a molten or glassy (i.e., the injection temperature is lower than the melting temperature and higher than the glass transition temperature) metal alloy into an injection mold. After cooling, a rough blank 200E1 of a watch component, such as an amorphous material (e.g., metallic glass), may be obtained. In particular, the material of the rough blank may be any amorphous alloy whose GFA (English: Glass Forming Ability) allows obtaining an amorphous structure of conventional watch component dimensions, in particular an amorphous metal alloy, including a metal matrix formed by at least one metal of elements such as nickel (Ni), copper (Cu), palladium (Pd), platinum (Pt), iron (Fe), cobalt (Co), titanium (Ti), niobium (Nb), zirconium (Zr), and alloys or mixtures thereof.

[0083] If it is an engineering ceramic or a metal ceramic, the rough blank 200E1 is obtained in particular by an injection molding process, including a step of sintering the green body obtained after injection molding. For example, the metal ceramic that can be considered includes a tungsten carbide, and / or titanium carbide, and / or zirconium carbide type ceramic phase, and a metal binder containing one or more elements of Ag, Pd, Co, Ni, Mo, Ru, Rh, Os, Ir, Pt, Au.

[0084] According to another embodiment, the blank 200E1 may be obtained by rotary or punch die forging, or by pressing.

[0085] The parts to be forged are preferably based on metal or metal alloys.

[0086] According to another embodiment, the rough blank 200E1 can be obtained by machining a ceramic part or a metal part or a metal-ceramic part, in particular by laser machining or by mechanical machining.

[0087] therefore, Figure 3a The view of FIG. 2 shows a rough blank 200E1 formed according to one of the above-mentioned techniques.

[0088] One may consider forming a one-piece (blank 200E1 from a single component) or, alternatively, a composite component and / or assembly, with a bezel ring made of a first material and a bezel disk 200 made of a second material.

[0089] Figure 4 The bezel plate 200 obtained in the first step is shown. Figure 2 The rough blank 200E1 includes a protruding portion 220 protruding relative to the base surface 210 , and the protruding portion includes a top portion 220s and a side surface 220f disposed between the top portion 220s and the base surface 210 .

[0090] The protrusions 220 extend from the base surface 210 to a distance or height of less than 1 mm, preferably less than 0.5 mm, and very preferably less than 0.3 mm, along the normal 210n of the base surface 210. These patterns may extend from the base surface 210 of the blank 200E1 to a height of at least 0.1 mm, even 0.15 mm, even 0.2 mm, even 0.25 mm, even 0.5 mm.

[0091] Advantageously, the side surface 220f of the protrusion 220 also forms a 90° angle with the base surface. Figure 4 , the angle a between the side surface 220f and the normal 210n of the base surface 210 may be equal to 15°. More generally, this angle a is less than or equal to 30°, even less than or equal to 25°, even less than or equal to 20°, even less than or equal to 15°, even less than or equal to 10°, even less than or equal to 5°. Alternatively, this angle may be equal to 0°. Still in Figure 4 In the embodiment, it can be noted that the normal line of the base surface 210 and the normal line of the bottom surface of the part form an angle b. In this non-limiting embodiment, the angle b is not 0°, that is, the base surface 210 is generally conical.

[0092] The second sub-step of step 10 of forming the blank 200E1 may be machining, in particular grinding (eg, grinding with a grinding wheel) the surface forming the inner diameter and / or outer diameter, and the surface forming the bottom of the blank 200E1 of the bezel plate 200 .

[0093] Of course, this step can be postponed and / or completed after any step of the method. In particular, it is contemplated that the side portion 230 with the notch can be processed, for example, at the end of the manufacturing method.

[0094] The third sub-step of step 10 of forming the rough blank 200E1 may be to grind the obtained rough blank 200E1.

[0095] For example, this may be a grinding step that allows the state of at least one visible surface of the blank 200E1, preferably all surfaces of the blank 200E1, to be changed by an intermediate medium. This step may comprise, for example, applying mechanical stress to the abrasive mixture by impacts, such as vibrations, oscillations or rotational impacts, in the grooves (friction finishing) of at least one blank 200E1 of the bezel disk 200, preferably a plurality of blanks 200E1. It also includes, for example, but is not limited to hammering and / or trovalisation, and / or sandblasting and / or shot peening and / or wet blasting of at least one visible surface of the blank 200E1, in particular all surfaces of the blank 200E1.

[0096] Alternatively, this step may comprise a laser polishing step, or, for metal parts, an electrochemical polishing step.

[0097] It may then be considered to sand the top 220s of the protrusion 220 of the rough blank 200E1, particularly at the upper surface thereof.

[0098] The manufacturing method may then proceed to step 20, i.e., forming at least one coating layer 250 on a portion of the rough blank 200E1 to obtain a rough blank 200E2 with a coating. In detail, this step may be to form at least one coating layer 250 on a portion of the rough blank 200E1 to obtain a rough blank 200E2 with a coating. Figure 3b or Figure 5 At least one coating 250 is deposited on the visible face of the blank 200E1 (shown in cross section in FIG). Preferably, the material of the deposited layer is a metal or a metal alloy or a ceramic. The deposit may have a metallic or ceramic appearance. This step allows the formation of at least one coating on the upper surface of the projection 220 and on the side 220f of said projection 220, which may be advantageously facilitated by the fact that said side forms an angle greater than 0° with the normal 210n of the base 210 of the blank 200E1. This step also allows the formation of at least one layer on the base 210 from which the projection 220 may extend.

[0099] The deposition method may be performed in a closed chamber 510, preferably by physical vapor deposition (PVD). Alternatively, the deposition may be performed by chemical deposition (CVD) or atomic layer deposition (ALD).

[0100] Advantageously, such techniques, which are well known to the skilled person, allow obtaining, for example, nitrides (CrN, TiN, ZrN, etc.), carbides (TiC, WC) or combinations thereof (TiCN, AlTiCN).

[0101] Preferably, in this embodiment, a metal carbide layer or a metal nitride layer is selected, for example:

[0102] -Tungsten carbide, titanium carbide, zirconium carbide, tantalum carbide, niobium carbide, chromium carbide, hafnium carbide.

[0103] -Titanium nitride, zirconium nitride, chromium nitride, tantalum nitride, niobium nitride, hafnium nitride, boron nitride.

[0104] The range of possible recommendations is very broad. A variety of combinations may be considered, for example:

[0105] - Combinations of two metal alloy nitrides and / or carbides, such as TiAlN / CrAlN;

[0106] - Combinations of nitrides and carbides, such as HfTiCN, which can produce a golden metallic luster.

[0107] Preferably, chromium nitride CrN is selected in this embodiment in view of its high hardness (for example, hardnesses above 1000 HV, preferably above 1500 HV, can be obtained). More generally, a ceramic-based hard layer may be preferred to form a coating or at least partially form a coating, if possible with a metallic appearance.

[0108] Of course, it is possible to consider depositing several superimposed layers to form a coating. For example, a silicon nitride Si3N4 layer can be combined with a titanium nitride layer to obtain a specific effect.

[0109] Thus, the second main step 20 may comprise a series of sub-steps of depositing superimposed layers comprising or based on different materials.

[0110] Other layers are also conceivable. For example, a layer comprising or based on carbon, usually referred to as DLC (English: Diamond-Like Carbon), may be deposited. Alternatively, a layer comprising or based on oxide may be deposited.

[0111] It is of course possible to combine different layers to obtain specific hardnesses and / or effects, if the layers are technically compatible.

[0112] Thus, it is conceivable to deposit at least one layer of a metal oxide, in particular tantalum oxide, for example stoichiometric tantalum oxide Ta2O5, or titanium oxide, or silicon oxide, or aluminum oxide, or a metal alloy oxide, or a metal nitride or a metal alloy.

[0113] Figure 5 Shows Figure 4, wherein the part is placed in a closed chamber 510 to apply a coating 250 covering the entire base surface 210 and all protrusions 220, thereby obtaining a coated rough blank 200E2. Schematically, the base material of the rough blank 200E2 is represented by M1, and the material of the coating 250 or a layer of coating 250 is represented by M2, to clearly indicate that a coated rough blank 200E2 including at least two materials (base material M1 and at least one layer of coating material M2) is obtained.

[0114] After coating 250 is applied to the exposed surfaces of blank 200E1 (typically all visible surfaces), it may be desirable to remove the coating from a portion of these surfaces to provide additional visual effects with a different color and / or a different texture.

[0115] To this end, the third main step 30 consists in removing at least one layer on one of the exposed surfaces by means of a laser source 610 , while the fourth step 40 consists in texturing the base surface 210 .

[0116] Preferably, in a third step 30 , the coating is removed from all or part of the base surface 210 .

[0117] Alternatively or additionally, the coating may be removed from all or part of the surface of the projection 220 .

[0118] The step 30 of removing at least one deposited layer is preferably performed simultaneously with the step 40 of texturing the treated surface.

[0119] The laser source 610 used is preferably an ultrashort pulse laser source 610, such as a nanosecond, picosecond or femtosecond pulse laser.

[0120] The laser source 610 can locally remove material, the thickness of which may exceed the thickness of at least one previously deposited layer. It can be noted that the material removal should not embrittle the watch component. The maximum laser ablation thickness can be defined according to the material and / or geometric dimensions of the part. It is also possible to consider performing multiple operations.

[0121] The laser source 610 can also form an aesthetic relief on at least one decorative layer and / or on the exposed substrate surface. In particular, the laser source 610 can form an aesthetic relief on the substrate surface by removing at least one previously deposited layer. For example, the possibility of texturing the surface can be cited, forming a satin finish, a brushed finish, a snail finish, a sunburst finish or generating Geneva waves, pearlescent finish or ring finish.

[0122] Figure 3c The sunray pattern formed on the base surface 210 is schematically shown.

[0123] according to Figure 6In the first embodiment shown, laser ablation is performed on the base surface 210 and on the side surfaces of the coated blank 200E2, the thickness of which is at least equal to the thickness of at least one deposited layer, and at the same time the removed base surface 210 is textured to form, for example, a sunburst pattern (in this figure, the textured area is indicated by ZT to indicate its location). The protrusions 220 (and their tops 220s or side surfaces 220s) are not affected by the laser beam here. Therefore, the laser beam has a dual function, namely to remove the material layer M2 from the coating 250 and to decorate the base surface 210 of the coated blank 200E2.

[0124] According to the second embodiment, in particular, Figure 7 As shown, a portion of the base surface 210 ( Figure 7 ), and it is considered that a laser source 610 is used to machine a cavity or a slit and texture in the material M1 of the coated blank 200E2, such as Figure 7 In this figure, the textured area is denoted by ZT to indicate its location.

[0125] According to a third embodiment, in particular, Figure 8 As shown, laser ablation can be performed locally on the blank, on the projection 220 (and / or its sides and / or base), on variable thickness. In the same operation, the same laser can be used to texture the exposed surface of the part locally.

[0126] like Figure 8 As shown, ablating with varying thickness can produce very attractive aesthetic effects. For example, this can produce a color gradient in at least one deposited layer. This can give the entire piece a glossy and convex feel. In this figure, the textured area is denoted by ZT to indicate its location.

[0127] Industrial Applications

[0128] The manufacturing method and / or the timepiece component according to the invention can be used in industrial applications.

[0129] It will be understood that various modifications and improvements apparent to those skilled in the art can be made to the various embodiments of the invention described in this specification without departing from the scope of the invention.

Claims

1. A method for manufacturing a watch component, comprising the following steps: (10) forming a blank (200E1), in particular by injection molding, the blank comprising at least one base surface (210) and at least one protrusion (220) protruding from the base surface (210), -(20) forming at least one coating layer (250) covering at least a portion of the base surface (210) and / or covering at least a portion of the at least one protrusion (220), - (30) removing at least a portion of the at least one coating layer (250) by laser ablation, -(40) texturing at least a portion of the base surface (210) previously covered with the at least one layer of coating (250) and / or at least a portion of the at least one protrusion (220) previously covered with the at least one layer of coating (250), and / or at least a portion of the at least one layer of coating (250) by laser processing.

2. The manufacturing method according to claim 1, wherein the step of removing (30) by laser ablation is performed so that: - locally removing the total thickness of the coating (250) and optionally removing the thickness of the blank (200E1) starting from the base surface (210), and / or - locally removing a thickness of the coating (250) that is less than the total thickness of the coating (250), and / or - locally removing a variable thickness of the coating (250) that is much smaller than the total thickness of the coating (250).

3. The manufacturing method according to any one of the above claims, wherein the at least one protrusion (220) comprises at least one surface forming a top (220s) and at least one surface forming a side surface (220f), wherein the side surface is disposed between the top (220s) and the base surface (210), The step of forming the at least one coating layer (250) is used to form the coating layer (250) to cover at least a portion of the base surface (210), at least a portion of the surface forming the top (220s) of the at least one protrusion (220), and at least a portion of the surface forming the side (220f) of the at least one protrusion (220), wherein a removal step (30) is performed to remove the coating (250) covering the base surface (210), And wherein a texturing step (40) is performed to texture at least a portion of the base surface (210).

4. The manufacturing method according to any of the preceding claims, wherein the step of removing by laser ablation (30) and the step of texturing by laser treatment (40) are at least partially performed simultaneously and / or are performed using the same laser source (610).

5. A manufacturing method according to any of the preceding claims, wherein the step of removing by laser ablation (30) and / or the step of texturing by laser processing (40) is performed using an ultrashort pulse laser source (610), and preferably using a pulsed laser source (610) configured to emit nanosecond pulses, more preferably picosecond pulses, and even more preferably femtosecond pulses.

6. The manufacturing method according to any one of the preceding claims, comprising a step of machining and / or grinding the rough blank (200E1), which is performed at the end of the step (10) of forming the rough blank (200E1), in particular between the step (10) of forming the rough blank (200E1) and the step (20) of forming the at least one layer of coating (250).

7. The manufacturing method according to any one of the above claims, comprises a step of grinding the rough blank (200E1), which is performed between the step (10) of forming the rough blank (200E1) and the step (20) of forming the at least one layer of coating (250).

8. A manufacturing method according to any one of the preceding claims, wherein the step (20) of forming the at least one layer of coating (250) comprises a physical vapor deposition (PVD) step, and / or a chemical vapor deposition (CVD) step, and / or an atomic layer deposition (ALD) step.

9. The manufacturing method according to any one of the preceding claims, wherein the step (20) of forming the at least one coating layer (250) comprises forming at least one layer of ceramic material and / or at least one layer of material containing a metal compound.

10. The manufacturing method according to any one of the preceding claims, wherein the step (20) of forming the at least one coating layer (250) comprises forming at least one layer comprising: - metal carbides, in particular tungsten carbide and / or titanium carbide, and / or zirconium carbide, and / or tantalum carbide, and / or niobium carbide, and / or chromium carbide, and / or hafnium carbide, and / or - at least one metal nitride, in particular chromium nitride and / or boron nitride, and / or zirconium nitride, and / or titanium nitride, and / or zirconium carbide, and / or tantalum nitride, and / or niobium nitride, and / or hafnium nitride, and / or - a combination of the various metal carbides and / or a combination of the various metal nitrides, and / or an alloy combination of the metal nitrides and the metal carbides.

11. A manufacturing method according to any of the above claims, wherein the metal of at least one layer of the coating (250) is selected from tungsten (W), and / or titanium (Ti), and / or zirconium (Zr), and / or tantalum (Ta), and / or niobium (Nb), and / or chromium (Cr), and / or hafnium (Hf), or their alloys, such as titanium aluminum (TiAl), chromium aluminum (CrAl), and hafnium titanium (HfTi) alloys.

12. A manufacturing method according to any of the preceding claims, wherein the texturizing step (40) is used to texturize the at least one coating layer (250) and / or the base surface (210) and / or the protrusion (220) by forming a satin finish, and / or a brush finish, and / or a snail finish, and / or a sunburst finish, and / or at least one Geneva wave, and / or a pearlescent finish, and / or a ring finish and / or any type of repeating patterned decoration.

13. A timepiece component intended to be mounted in a timepiece, comprising a body, or in the form of a body, formed from a blank (200E1) according to the manufacturing method of any one of claims 1 to 12.

14. A watch component according to the above claims, wherein the body comprises a base surface (210), at least one protrusion (220) protruding relative to the base surface (210), and comprises a top (220s) and at least one side surface (220f) arranged between the base surface (210) and the top (220s), wherein the top (220s) and the at least one side surface (220f) are covered with a coating (250) formed according to the manufacturing method according to any one of claims 1 to 12, and wherein the base surface (210) has been textured according to the manufacturing method according to any one of claims 1 to 12.

15. The timepiece component according to claim 13 or 14, forming a protective component of a timepiece, such as a bezel (200), or a bezel plate, or a dial, or a crown, a push button or a buckle.

16. A timepiece component according to any one of claims 13 to 15, wherein the at least one protrusion (220) comprises at least one top (220s) and a side surface (220f) arranged between the top (220s) of the protrusion (220) and the base surface (210), and wherein the at least one side surface (220f) forms a clearance angle with a normal (210n) of the base surface (210), preferably between 5° and 25°, specifically between 10° and 20°.

17. Timepiece component according to any one of claims 13 to 16, wherein the blank (200E1) comprises a ceramic material and / or a metallic material and / or a cermet.