Electrolyte and lithium ion battery
By using electrolyte additives containing furan, fluorine and sulfonamide functional groups in lithium-ion batteries, the inorganic lithium salt interface film is formed, which solves the problem of volume expansion of silicon-based negative electrode materials and the circulation stability of high Ni positive electrode materials, and improves the circulation of the battery and rate performance enhances safety performance.
Patent Information
- Application Number
- CN202411067159.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-12-06
AI Technical Summary
The silicon-based negative electrode material in lithium-ion batteries causes unstable solid electrolyte interface film due to volume expansion, affecting circulation stability, high Ni content of positive electrode material reduces circulation stability, and the existing additive improvement effect is limited.
An electrolyte additive is adopted, whose structure contains furan, fluorine and sulfonamide functional groups, has low LUMO and high HOMO energy levels, and jointly forms inorganic lithium salts Li2S, Li3N and LiF to form a dense interface film, and inhibits vinyl carbonate on the surface of the positive electrode. Dehydrogenation reaction improves the circulation and safety performance of lithium-ion batteries.
Significantly improve the circulation performance, rate performance and safety performance of lithium-ion batteries, enhance the oxidation resistance and high temperature performance of the electrolyte, reduce the organic component content of SEI membrane, and extend the battery life.
Smart Images

Figure CN119092824A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of lithium ion batteries, and in particular relates to an electrolyte and a lithium ion battery. Background Art
[0003] Anode materials with high specific capacity are an important breakthrough in improving the energy density of lithium-ion batteries. Silicon-based materials are considered to be the most likely anode materials to replace graphite because of their high theoretical specific capacity (Si: 4200mAh / g, SiO: 2650mAh / g), suitable discharge potential and relatively abundant reserves in nature. However, there are many problems in the commercial application of single silicon in lithium-ion batteries. First, silicon-based materials as anodes will have volume expansion problems during battery cycles, and may cause the rupture of active particles, silicon powderization and active material shedding. Secondly, the silicon anode is accompanied by a large volume expansion during the first cycle. Due to the change in silicon volume, the solid electrolyte interface film (SEI) will rupture. The newly exposed silicon on the surface will produce a new SEI film, and at the same time, it will continuously consume lithium ions in the electrolyte, reducing the first coulomb efficiency. More seriously, during the cycle, due to the volume change of the electrode material, the SEI film at the silicon anode interface repeatedly grows and ruptures, greatly affecting the cycle stability. Due to the volume effect of silicon-based negative electrode materials, it is difficult for silicon-based negative electrodes to form stable solid electrolyte interface films in the electrolyte, and the electrode structure is destroyed during the battery cycle. New solid electrolyte interface films will continue to form on the exposed silicon-based surface, leading to corrosion of the negative electrode material and capacity attenuation.
[0004] The high Ni content in the positive electrode LiNixCoyMnzO2 (NCM) can promote more Ni 2+ Participate in the redox process (Ni 2 + Ni 4+ ), which can improve the energy density of the battery. However, the cycle stability of the positive electrode material decreases significantly, which is mainly because the increase in Ni content increases the Li + / Ni 2+ Mixing; secondly, the isotropic stress-strain destroys the layered structure of the positive electrode, which will cause particle breakage in the late cycle; it will also lead to the dissolution of transition metal ions and the decomposition of the electrolyte under high voltage.
[0005] In order to improve the interface stability of high-Ni materials, surface coating and electrolyte additives are commonly used methods. By forming an inert layer on the surface of the positive electrode, the oxidative decomposition of the electrolyte on the surface of the positive electrode material is inhibited. Single functional additives are usually used for improvement, but the improvement effect is limited.
[0006] The silicon negative electrode has a very high gram capacity, but its volume expansion is large and the interface film is very unstable. It is usually improved by using vinylene carbonate (VC) additives, but VC itself has poor stability and the degree of improvement is limited. Summary of the invention
[0007] In order to solve the technical problem of poor stability of the solid electrolyte interface film in the above-mentioned prior art, the purpose of the present invention is to provide an electrolyte and a lithium ion battery.
[0008] The present invention provides an electrolyte additive, the general structural formula of the electrolyte additive is as follows (I):
[0009]
[0010] Among them, at least one of R1 to R5 is a F atom, and R1 to R5 are each independently a H atom, a methyl group or an amino group.
[0011] The electrolyte additive of the present invention is a compound of the above-mentioned general structural formula. On the one hand, compared with the constituent solvents in the electrolyte, namely linear carbonates and cyclic carbonates, the electrolyte additive has the properties of low LUMO and high HOMO energy levels, showing a dual regulatory effect on electrolyte solvation and electrode interface; on the other hand, it promotes the formation of rich inorganic lithium salts, namely Li2S, Li3N and LiF, on the surfaces of the positive and negative electrodes. The synergistic effect of the three inorganic lithium salts can better protect the positive and negative electrode interfaces. Li3N is a layered solid electrolyte with a two-dimensional ion migration channel and a room temperature conductivity of 10-3S / c m, high ionic conductivity, rich in LiF and benzene ring skeletons, can form a dense and rigid solid electrolyte interface film, and LiF and Li2S have high thermal stability; thirdly, inhibit the dehydrogenation reaction of ethylene carbonate (EC) occurring on the surface of the positive electrode NCM. The acidity of the electrolyte increases when EC undergoes dehydrogenation reaction, which intensifies the disproportionation reaction of trivalent manganese. Once divalent manganese is produced, it will dissolve in the electrolyte due to its high solubility. Subsequently, divalent manganese will migrate to the negative electrode due to the electric field and deposit on the SEI film, which has a strong destructive effect on the SEI film. For the electrolyte itself, divalent manganese will also have a catalytic decomposition effect. The electrolyte additive of the present invention contains multiple functional groups such as furan, fluorine and sulfonamide. The furan of Lewis acid not only has a medium dielectric constant but also has a low Li + Desolvation energy ensures that Li +While having good complexing ability, furan also has the advantages of low melting point and low viscosity, and can be widely used in low-temperature fields, and has good effects in solving low-temperature charging and improving fast charging; fluorine has weak solvation and can form an interface film rich in LiF; sulfonamide can improve the oxidation resistance of the electrolyte, and can make high-nickel positive electrode materials have good stability at high voltage; F, aromatic groups and sulfonamides in the molecular structure of the electrolyte additive have a conjugated system, making the molecular structure more stable; fluorine and sulfonyl have flame retardant effects. The electrolyte additive of the present invention can improve the cycle performance, rate performance and safety performance of lithium-ion batteries through the coordinated regulation of the above-mentioned effects.
[0012] Preferably, the electrolyte additive comprises at least one of the following structural formulas:
[0013]
[0014] The electrolyte additive described in this solution includes at least one of the above structural formulas. The electrolyte additive described in the above structural formula can further improve the cycle performance, rate performance and safety performance of the lithium-ion battery.
[0015] The invention provides an electrolyte comprising the electrolyte additive.
[0016] Preferably, in the electrolyte, the mass fraction of the electrolyte additive is 1% to 4%.
[0017] In the electrolyte of this solution, the mass fraction of the electrolyte additive is 1% to 4%, which can fully realize the above-mentioned technical effects of the electrolyte additive and ensure the improvement of the cycle performance and rate performance of the lithium-ion battery while maintaining a reasonable cost.
[0018] Preferably, the electrolyte further comprises linear carbonate and cyclic carbonate.
[0019] Preferably, the linear carbonate includes at least one of dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), and methyl propyl carbonate (MPC), and the cyclic carbonate includes at least one of ethylene carbonate (EC), fluoroethylene carbonate (FEC), and propylene carbonate (PC).
[0020] Preferably, the electrolyte further comprises a sulfur-containing additive and a lithium salt additive; in the electrolyte, the mass fraction of the sulfur-containing additive is 1% to 3%, and the mass fraction of the lithium salt additive is 0.5 to 1%.
[0021] The electrolyte described in this scheme also includes a sulfur-containing additive and a lithium salt additive; in the electrolyte, the mass fraction of the sulfur-containing additive is 1% to 3%, and the mass fraction of the lithium salt additive is 0.5 to 1%. The electrolyte includes the sulfur-containing additive and the lithium salt additive, and the mass fractions of the sulfur-containing additive and the lithium salt additive are within this range, which can form a stable and dense SEI film on the electrode surface, improve the high temperature performance of the electrolyte, inhibit gas expansion and reduce the internal resistance of the battery, and reduce the content of organic components in the SEI film.
[0022] Preferably, the sulfur-containing additive includes at least one of 1,3-propane sultone, vinyl sulfate, propylene sulfite, and propenyl-1,3-sultone.
[0023] Preferably, the lithium salt additive includes at least one of LiPO2F2, LiODFB, LiODFP, and LiBOB.
[0024] Preferably, the electrolyte also includes lithium hexafluorophosphate LiPF6 with a concentration of 1.2 to 1.5 mol / L.
[0025] The present invention also provides a lithium ion battery comprising the electrolyte. DETAILED DESCRIPTION
[0026] In order to enable those skilled in the art to better understand the solutions of the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only embodiments of a part of the present invention, rather than all embodiments.
[0027] Example 1
[0028] The structural formula of the electrolyte additive in this embodiment is as follows:
[0029]
[0030] N-(Furan-2-methyl)4-fluorobenzenesulfonamide
[0031] Preparation of electrolyte
[0032] S1. Dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), fluoroethylene carbonate (FEC), and ethylene carbonate (EC) are mixed in a mass ratio of 40:30:15:15, and the mixture is stirred to obtain a first mixture;
[0033] S2. Add lithium hexafluorophosphate LiPF6 to the first mixture and stir, and after stirring and mixing evenly, obtain a second mixture;
[0034] S3. Add electrolyte additives, sulfur-containing additive 1,3-propane sultone (PS) and lithium salt additive LiPO2F2 to the second mixture and stir. After stirring and mixing evenly, an electrolyte is obtained. In the electrolyte of this embodiment, the concentration of LiPF6 is 1.3 mol / L, the mass fraction of the electrolyte additive is 3%, the mass fraction of 1,3-propane sultone is 2%, and the mass fraction of LiPO2F2 is 0.8%.
[0035] Example 2
[0036] The structural formula of the electrolyte additive used in the preparation of the electrolyte in this embodiment is as follows:
[0037]
[0038] Other than that, the same as in Example 1.
[0039] Example 3
[0040] The structural formula of the electrolyte additive used in the preparation of the electrolyte in this embodiment is as follows:
[0041]
[0042] Other than that, the same as in Example 1.
[0043] Example 4
[0044] The preparation of the electrolyte in this example is the same as in Example 1 except that the mass fraction of the electrolyte additive N-(furan-2-methyl) 4-fluorobenzenesulfonamide is 6%.
[0045] Example 5
[0046] The preparation of the electrolyte in this example is the same as in Example 1 except that the mass fraction of the electrolyte additive N-(furan-2-methyl) 4-fluorobenzenesulfonamide is 0.7%.
[0047] Example 6
[0048] The preparation of the electrolyte of this embodiment is the same as that of Embodiment 1, except that the mass of the sulfur-containing additive 1,3-propane sultone in Embodiment 1 is replaced by the base solvent (DMC, EMC, FEC, and EC are configured as the base solvent in a mass ratio of 40:30:15:15).
[0049] Example 7
[0050] The preparation of the electrolyte in this embodiment is the same as that in Example 1, except that the mass of the lithium salt additive LiPO2F2 in Example 1 is replaced by the base solvent (DMC, EMC, FEC, and EC are configured as the base solvent in a mass ratio of 40:30:15:15).
[0051] Example 8
[0052] The preparation of the electrolyte in this embodiment is the same as that in Embodiment 1 except that the mass fraction of 1,3-propane sultone is 3.5% and the mass fraction of LiPO2F2 is 1.3%.
[0053] Example 9
[0054] The preparation of the electrolyte in this embodiment is the same as that in Embodiment 1 except that the mass fraction of 1,3-propane sultone is 0.7% and the mass fraction of LiPO2F2 is 0.3%.
[0055] Comparative Example 1
[0056] The preparation of the electrolyte of this comparative example is the same as that of Example 1, except that the electrolyte additive N-(furan-2-methyl) 4-fluorobenzenesulfonamide in Example 1 is replaced by the base solvent (DMC, EMC, FEC, and EC are configured as the base solvent in a mass ratio of 40:30:15:15).
[0057] Comparative Example 2
[0058] The electrolyte additives of this comparative example are 2-methyltetrahydrofuran, methyl trifluoroethyl carbonate and trifluoromethanesulfonamide.
[0059] Preparation of electrolyte
[0060] S1. Dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), fluoroethylene carbonate (FEC), and ethylene carbonate (EC) are mixed in a mass ratio of 40:30:15:15, and the mixture is stirred to obtain a first mixture;
[0061] S2. Add lithium hexafluorophosphate LiPF6 to the first mixture and stir, and after stirring and mixing evenly, obtain a second mixture;
[0062] S3. Add electrolyte additives 2-methyltetrahydrofuran, methyl trifluoroethyl carbonate, trifluoromethanesulfonamide, sulfur-containing additive 1,3-propane sultone (PS) and lithium salt additive LiPO2F2 to the second mixture and stir. After stirring and mixing evenly, an electrolyte is obtained. In the electrolyte of this embodiment, the concentration of LiPF6 is 1.3 mol / L, the mass fraction of 2-methyltetrahydrofuran is 0.66%, the mass fraction of methyl trifluoroethyl carbonate is 1.20%, the mass fraction of trifluoromethanesulfonamide is 1.14%, the mass fraction of 1,3-propane sultone is 2%, and the mass fraction of LiPO2F2 is 0.8%.
[0063] Comparative Example 3
[0064] The structural formula of the electrolyte additive used in the preparation of the comparative example electrolyte is as follows:
[0065]
[0066] Other than that, the same as in Example 1.
[0067] Comparative Example 4
[0068] The structural formula of the electrolyte additive used in the preparation of the comparative example electrolyte is as follows:
[0069]
[0070] Other than that, the same as in Example 1.
[0071] Comparative Example 5
[0072] The structural formula of the electrolyte additive used in the preparation of the comparative example electrolyte is as follows:
[0073] Except that the mass fractions of the two electrolyte additives in the electrolyte are 1.67% and 1.33% respectively, the rest is the same as in Example 1.
[0074] Preparation of lithium-ion batteries
[0075] (1) Preparation of positive electrode sheet
[0076] The positive electrode active material LiNi 0.8 Co 0.1 Mn 0.1 O2, conductive agent acetylene black and binder polyvinylidene fluoride (PVDF) are mixed in a mass ratio of 94:3:3 and added to a solvent N-methylpyrrolidone (NMP). The mixture is evenly mixed to obtain a positive electrode slurry with a solid content of 45%. The positive electrode slurry is coated on both surfaces of the positive electrode current collector aluminum foil to form a positive electrode active coating. After vacuum drying, a positive electrode sheet is obtained.
[0077] (2) Preparation of negative electrode sheet
[0078] Silicon-carbon negative electrode material (SiC), conductive agent conductive carbon black (SP), single-walled carbon nanotubes (SWCNT) and binder polyacrylic acid (PAA) are mixed in a mass ratio of 80:9:1:10 and added to a solvent deionized water, mixed evenly, to prepare a negative electrode slurry with a solid content of 25%, and the negative electrode slurry is coated on both surfaces of the negative electrode current collector copper foil to form a negative electrode active coating, and after vacuum drying, a negative electrode sheet is prepared.
[0079] (3) Selection of electrolyte
[0080] The electrolytes obtained in the above-mentioned embodiments and comparative examples and the common electrolyte of the control group (EC:DMC:DEC mass ratio of 30:40:30, LiPF6 1 mol / L) were selected to prepare lithium-ion batteries.
[0081] (4) Selection of isolation membrane
[0082] The isolation film includes a polyethylene (PE) film and ceramic layers respectively arranged on two surfaces of the PE film, wherein the total thickness of the two ceramic layers is 3 μm, the thickness of the PE film is 9 μm, and the total thickness of the isolation film is 12 μm.
[0083] (5) Preparation of lithium-ion batteries
[0084] The positive electrode sheet, the isolation film, and the negative electrode sheet are stacked in order, and the isolation film is placed between the positive electrode sheet and the negative electrode sheet to play an isolating role, so as to prepare a bare battery cell; the bare battery cell is placed in an outer packaging shell, and after drying, an electrolyte is injected, and a lithium-ion battery is obtained through vacuum packaging, standing, forming, shaping and other processes.
[0085] Performance Testing
[0086] The rate performance of the battery was tested under lithium-ion battery test conditions. The test was conducted on the LAND battery test system of Wuhan Jinnuo Electronics Co., Ltd. at room temperature (25°C). The conventional charge and discharge voltage was limited to 2.5V to 4.2V, and a high voltage cycle of 2.5 to 4.4V was designed. The cycle performance and rate performance are shown in Table 1 below.
[0087] 1) 2.5~4.2V at room temperature, 1C / 1C cycle 900 weeks capacity retention rate
[0088] At 25°C, the lithium-ion battery is charged to 4.2V at a constant current and constant voltage rate of 1C, with a cut-off current of 0.05C, and allowed to stand for 10 minutes. Then, the lithium-ion battery is discharged to 2.5V at a constant current rate of 1C and allowed to stand for 10 minutes. This is considered one charge and discharge cycle. The lithium-ion battery is charged and discharged for 900 cycles according to the above method, and the capacity retention rate of the lithium-ion battery after 900 cycles of charge and discharge at 1C / 1C is calculated.
[0089] The capacity retention rate (%) of a lithium-ion battery after N cycles = (discharge capacity at the Nth cycle / initial discharge capacity) × 100%, where N is the number of cycles of the lithium-ion battery.
[0090] 2) Room temperature 2.5 ~ 4.4V, 1C / 1C cycle 900 weeks capacity retention rate
[0091] At 25°C, the lithium-ion battery is charged to 4.4V at a constant current and constant voltage rate of 1C, with a cut-off current of 0.05C, and allowed to stand for 10 minutes. Then, the lithium-ion battery is discharged to 2.5V at a constant current rate of 1C and allowed to stand for 10 minutes. This is considered one charge and discharge cycle. The lithium-ion battery is charged and discharged for 900 cycles according to the above method, and the capacity retention rate of the lithium-ion battery after 900 cycles of charge and discharge at 1C / 1C is calculated.
[0092] The capacity retention rate (%) of a lithium-ion battery after N cycles = (discharge capacity at the Nth cycle / initial discharge capacity) × 100%, where N is the number of cycles of the lithium-ion battery.
[0093] 3) Room temperature 6C rate performance - constant current charging ratio
[0094] At 25°C, the lithium-ion battery was discharged at a constant current rate of 1C to 2.5V and allowed to stand for 10 minutes. Then, the lithium-ion battery was charged at a constant current and constant voltage rate of 6C to 4.2V, with a cut-off current of 0.05C. The battery was allowed to stand for 10 minutes. The constant current charging capacity Q1 and the constant current and constant voltage charging total capacity Q2 of the lithium-ion battery were recorded. The 6C rate charging constant current charging ratio was calculated according to the following formula: 6C rate charging constant current charging ratio = constant current charging capacity Q1 / constant current and constant voltage charging total capacity Q2 × 100%.
[0095] 4) 1C discharge capacity retention rate at low temperature (-20℃)
[0096] At 25°C, the lithium ion battery is charged to 4.2V at a constant current and constant voltage rate of 1C, with a cut-off current of 0.05C, and allowed to stand for 10 minutes. The discharge capacity at this time is measured as the discharge capacity at 25°C, recorded as q1. Then, at 25°C, the lithium ion battery is charged to 4.2V at a constant current and constant voltage rate of 1C, with a cut-off current of 0.05C, and allowed to stand for 10 minutes. After the lithium ion battery is placed at -20°C for 2 hours, the lithium ion battery is discharged to 2.5V at a constant current rate of 1C at -20°C. The discharge capacity at this time is measured as the discharge capacity at -20°C, recorded as q2. The 1C discharge capacity retention rate at low temperature (-20°C) is calculated according to the following formula: 1C discharge capacity retention rate at -20°C = discharge capacity at -20°C q2 / discharge capacity at 25°C q1×100%.
[0097] 5) Battery thermal runaway ARC (adiabatic accelerated calorimeter) test
[0098] The lithium-ion battery is heated from room temperature to 45±2℃ in the chamber. After being left for 90 minutes, the temperature rise rate of the battery is detected. If the temperature rise exceeds 0.2℃ within 10 minutes (i.e., the self-heating temperature rise rate SHR>0.02℃ / min), it is considered that a self-exothermic reaction occurs inside the lithium-ion battery, and the adiabatic environment is maintained until the lithium-ion battery has thermal runaway; if the temperature rise does not exceed 0.2℃ within 10 minutes (i.e., the self-heating temperature rise rate SHR≤0.02℃ / min), continue to the next step temperature rise test; each temperature step is 5℃, and the steps are repeated on each step. The ARC test temperature range is 45-300℃, the self-heating starting temperature is T1 (temperature rise rate SHR>0.02℃ / min), and the thermal runaway starting temperature is T2 (temperature rise rate SHR>1℃ / min).
[0099] Table 1
[0100]
[0101]
[0102] From the analysis of Table 1, we can see that:
[0103] After the electrolytes of Examples 1 to 9 of the present invention are used to prepare lithium-ion batteries, they show good performance in terms of cycle capacity retention rate (including 2.5 to 4.2V cycles and high voltage cycles 2.5 to 4.4V), high rate performance-constant current charging ratio (fast charging), low temperature discharge capacity retention rate and battery thermal runaway ARC test (self-heating starting temperature T1 and thermal runaway starting temperature T2), while Comparative Examples 1 to 5 and the control group do not belong to the technical scheme of the present invention, so the performance in the above four aspects is significantly deteriorated, which fully demonstrates that the electrolyte prepared by the technical scheme of the present invention is applied to lithium batteries, which can effectively improve the cycle performance and rate performance of lithium-ion batteries, and improve the low temperature and high voltage performance of the electrolyte, while making the electrolyte have a flame retardant effect, thereby improving the safety performance of lithium-ion batteries.
[0104] The electrolyte additives of Examples 2 and 3 are other electrolyte additives that meet the general structural formula of the electrolyte additive of the technical solution of the present invention. Compared with the electrolyte additive in Example 1, the electrolyte additive structural formula of Example 2 contains 2 F atoms and the substitution sites of the F atoms on the phenyl group are also different. The phenyl group in the electrolyte additive structural formula of Example 3 contains other non-F substituents - amino groups. From the test results in Table 1, the lithium-ion batteries prepared using the electrolytes of Examples 2 and 3 also show good technical effects in the cycle capacity retention rate, high rate performance-constant current charging ratio, low temperature discharge capacity retention rate and battery thermal runaway ARC test.
[0105] Compared with Example 1, the electrolyte in Example 4 uses more electrolyte additives - the mass fraction of the electrolyte additives in the electrolyte is 6%, and the electrolyte in Example 5 uses less electrolyte additives - the mass fraction of the electrolyte additives in the electrolyte is 0.7%. The electrolyte additives used in the electrolytes of Example 4 and Example 5 are not within the further preferred range of the mass fraction of the electrolyte additives of 1% to 4%. From the test results in Table 1, the technical effects of the lithium-ion battery prepared using the electrolyte of Example 4 in terms of cycle capacity retention rate, high rate performance-constant current charging ratio, low temperature discharge capacity retention rate and battery thermal runaway ARC test are reduced. The amount of electrolyte additives used in Example 5 is relatively small, which promotes the formation of rich inorganic lithium salts on the surface of the positive and negative electrodes - Li2S, Li3N and LiF are relatively small, and the ability to protect the positive and negative electrode interfaces is weakened; the inhibition of the dehydrogenation reaction of ethylene carbonate (EC) occurring on the surface of the positive electrode NCM is weakened; ensuring Li + The good complexing ability and efficient desolvation ability are weakened, the improvement of the low temperature and high voltage performance of the electrolyte is weakened, the molecular structure stability of the electrolyte additive is reduced, the flame retardant performance of the electrolyte is reduced, and the technical effects of the lithium ion battery prepared using the electrolyte of Example 5 in the cycle capacity retention rate, high rate performance-constant current charging ratio, low temperature discharge capacity retention rate and battery thermal runaway ARC test are reduced.
[0106] Compared with Example 1, no sulfur-containing additive is added to the electrolyte of Example 6, no lithium salt additive is added to the electrolyte of Example 7, and the mass fractions of the sulfur-containing additive and the lithium salt additive in the electrolytes of Examples 8 and 9 are not within a further preferred range - the mass fraction of the sulfur-containing additive is 1% to 3%, and the mass fraction of the lithium salt additive is 0.5 to 1%, that is, the mass fractions of the sulfur-containing additive and the lithium salt additive in the electrolyte of Example 8 are both greater than the preferred range, and the mass fractions of the sulfur-containing additive and the lithium salt additive in the electrolyte of Example 9 are both less than the preferred range. From the test results in Table 1, the lithium-ion battery prepared using the electrolyte of Example 6 has better technical effects than Example 8 in terms of cycle capacity retention rate, high rate performance-constant current charging ratio, low temperature discharge capacity retention rate and battery thermal runaway ARC test. The mass fractions of the sulfur-containing additive and the lithium salt additive in the electrolyte of Example 8 are not within the preferred range, and the technical effect is not as good as that of Example 6 (the sulfur-containing additive 1,3-propane sultone is not added). This shows that an unexpected synergistic technical effect can be achieved by satisfying the combination of the sulfur-containing additive and the lithium salt additive and their respective mass fractions being within the preferred range.
[0107] Compared with Example 1, Comparative Example 1 does not use electrolyte additives. Therefore, from the test results in Table 1, compared with Example 1, the technical effects of the lithium ion battery prepared using the electrolyte of Comparative Example 1 in terms of cycle capacity retention rate, high rate performance-constant current charging ratio, low temperature discharge capacity retention rate and battery thermal runaway ARC test are significantly reduced.
[0108] The electrolyte additives used in Comparative Example 2 are 2-methyltetrahydrofuran, methyl trifluoroethyl carbonate and trifluoromethanesulfonamide. The combination of 2-methyltetrahydrofuran, methyl trifluoroethyl carbonate and trifluoromethanesulfonamide satisfies the electrolyte additive structural formula of Example 1 and has multiple functional groups of furan, fluorine and sulfonamide. From the test results in Table 1, the lithium ion battery prepared using the electrolyte of Comparative Example 2 has significantly reduced technical effects in terms of cycle capacity retention rate, high rate performance-constant current charging ratio, low temperature discharge capacity retention rate and battery thermal runaway ARC test. This shows that even if the electrolyte additive used simultaneously satisfies the functional group characteristics of the general structural formula of the electrolyte additive in the technical scheme of the present invention, replacing it with the electrolyte additive in the technical scheme of the present invention cannot simultaneously achieve the above four technical effects.
[0109] Compared with Example 1, the structural formula of the electrolyte additive used in Comparative Example 3 has one less F atom on the phenyl group, that is, the electrolyte additive does not contain fluorine. From the test results in Table 1, the lithium ion battery prepared using the electrolyte of Comparative Example 3 has significantly reduced technical effects in terms of cycle capacity retention rate, high rate performance-constant current charging ratio, low temperature discharge capacity retention rate and battery thermal runaway ARC test.
[0110] Compared with Example 1, the structural formula of the electrolyte additive used in Comparative Example 4 lacks a furan structure. From the test results in Table 1, the technical effects of the lithium ion battery prepared using the electrolyte of Comparative Example 4 in terms of cycle capacity retention rate, high rate performance-constant current charging ratio, low temperature discharge capacity retention rate and battery thermal runaway ARC test are significantly reduced.
[0111] The electrolyte additive used in Comparative Example 5 is a combination of the additives in Comparative Example 3 and Comparative Example 4, that is, the combination thereof satisfies the functional group characteristics in the general structural formula of the electrolyte additive of the present invention in Example 1. From the test results in Table 1, the technical effects of the lithium ion battery prepared using the electrolyte of Comparative Example 5 in terms of cycle capacity retention rate, high rate performance-constant current charging ratio, low temperature discharge capacity retention rate and battery thermal runaway ARC test are significantly reduced, which shows that even if the electrolyte additive used simultaneously satisfies the functional group characteristics of the general structural formula of the electrolyte additive of the technical scheme of the present invention, replacing it with the electrolyte additive in the technical scheme of the present invention cannot simultaneously achieve the technical effects of the above four aspects.
[0112] The above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the protection scope of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. An electrolyte, characterized in that: The electrolyte includes an electrolyte additive, and the general structural formula of the electrolyte additive is shown in the following formula (I): Among them, at least one of R1 to R5 is a F atom, and R1 to R5 are each independently a H atom, a methyl group or an amino group.
2. The electrolyte according to claim 1, characterized in that: The electrolyte additive includes at least one of the following structural formulas:
3. The electrolyte according to claim 1, characterized in that: In the electrolyte, the mass fraction of the electrolyte additive is 1% to 4%.
4. The electrolyte according to claim 1, characterized in that: The electrolyte also includes linear carbonates and cyclic carbonates.
5. The electrolyte according to claim 4, characterized in that: The linear carbonate includes at least one of dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate and methyl propyl carbonate.
6. The electrolyte according to claim 4, characterized in that: The cyclic carbonate includes at least one of ethylene carbonate, fluoroethylene carbonate and propylene carbonate.
7. The electrolyte according to claim 1, characterized in that: The electrolyte further comprises a sulfur-containing additive and a lithium salt additive; in the electrolyte, the mass fraction of the sulfur-containing additive is 1% to 3%, and the mass fraction of the lithium salt additive is 0.5 to 1%.
8. The electrolyte according to claim 7, characterized in that: The sulfur-containing additive includes at least one of 1,3-propane sultone, vinyl sulfate, propylene sulfite, and propenyl-1,3-sultone.
9. The electrolyte according to claim 7, characterized in that: The lithium salt additive includes at least one of LiPO2F2, LiODFB, LiODFP, and LiBOB.
10. A lithium ion battery, characterized in that: Comprising the electrolyte as claimed in any one of claims 1 to 9.
Citation Information
Patent Citations
Electrolyte and preparation method and application thereof
CN116454378A
Non-aqueous electrolyte, lithium ion battery, battery module, battery pack and electric device
CN116487696A
Positive electrode film-forming additive and preparation method thereof, electrolyte and lithium ion battery
CN116613380A
Electrolyte for high-voltage lithium ion battery as well as preparation method and application of electrolyte
CN118198498A
Electrolyte for rechargeable lithium battery, method of preparing same and rechargeable lithium battery comprising same