Shaving board and manufacturing method thereof

By grinding composite materials and mixing them with synthetic resin and organic particles, high-performance particle board is formed, which solves the problems of insufficient waterproofness, thermal insulation and electrical insulation in the prior art, and achieves more efficient resource utilization and performance improvement.

CN119095704APending Publication Date: 2024-12-06安杰伊·阿达姆西奥
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202380032287.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-01
Filing Date
2023-03-30
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The prior art cannot provide sufficient waterproofness, thermal insulation and electrical insulation, and requires the use of a large number of epoxy resins and polyester resins as adhesives.

Method used

Using particleboard composed of synthetic resin, composite materials and organic particles, the composite materials are ground into 1D or 2D forms, mixed and pressed in the mold for two stages, reducing the use of adhesive and improving the performance of the sheet.

Benefits of technology

The waterproofness, insulation and flame retardancy of the board are improved, the consumption of adhesives and dependence on natural resources are reduced, and the hardness and water resistance of the board are enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119095704A_ABST
    Figure CN119095704A_ABST
Patent Text Reader

Abstract

The invention relates to a shaving board consisting of organic particles of a synthetic resin composite material containing, by weight, 10% to 60% of a ground composite material, 5% to 60% of a synthetic resin and 10% to 85% of organic particles, in particular wood and plant particles or fibers or a composition of these components. The invention further aims to provide a manufacturing method of the shaving board.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The object of the present invention is a particleboard consisting of organic particles, a composite material and a synthetic resin and a method for its manufacture.

[0002] Document CN107206734A discloses a composite board at least partially composed of a non-woven composite material, wherein the non-woven composite material contains: natural fibers and / or dispersed glass fibers, ductile optical fibers and 0 to 50% (by weight) of a thermal hardener. The present invention also relates to particleboard (PB), medium density fiber board (MDF) and high density fiber board (MDF-HDF), oriented strand board (OSB), laminated veneer lumber (LVL), plywood (PLW) and related materials.

[0003] Currently known solutions do not provide adequate waterproofing, thermal and electrical insulation of the panels or electrical conductivity. Previous solutions required the use of 50%-60% adhesives in the form of epoxy and polyester resins.

[0004] According to the invention, a particleboard consisting of organic particles of a synthetic resin composite material comprises, by weight, 10 to 60% of a particle composite material, 5 to 60% of a synthetic resin and 10 to 85% of organic particles, in particular wood and plant particles or fibers or a combination of these components.

[0005] Preferably, the composite material is ground into a 1D form, in which the size of the particle mixture is: 1 mm-4 mm in length and not more than 1 mm in thickness.

[0006] Preferably, the composite material is ground into a 2D form, in which the composite material particles have dimensions of 5 mm to 200 mm in length, 1 mm to 30 mm in width, and 0.2 mm to 2 mm in thickness.

[0007] Preferably, the composite material comprises 10% to 40% by weight of the particle board.

[0008] Preferably, the synthetic resin comprises 5 to 20% by weight of the particleboard.

[0009] In another aspect, the invention relates to a method for producing a particleboard:

[0010] 1) grinding the composite material;

[0011] 2) mixing together, by weight, 10% to 60% of a ground composite material, 5% to 60% of a synthetic resin, and 10% to 85% of organic particles;

[0012] 3) placing the mixture in a mold or on a molding plate or a molding belt at a temperature of 18°C ​​to 250°C;

[0013] 4) performing two-stage pressing at a temperature of 18°C ​​to 250°C, wherein the first step comprises arranging or arranging the filler and matrix particles and degassing the composite material, and the second step comprises providing the final thickness at a temperature of 18°C ​​to 250°C and a pressure of 0.02 MPa to 5 MPa.

[0014] Preferably, in order to manufacture a multilayer board, it is necessary to form a cushion layer, the outer layer of the cushion layer is 0% to 60% of the grinding composite material, and then form a middle layer containing 10% to 70% of the grinding composite material, and finally form an upper outer layer containing 0% to 60% of the grinding composite material, wherein the proportion of the middle layer is 50% to 90% of the manufactured board.

[0015] Preferably, the composite material is ground into a 1D form in which the particle mixture has a size of 1 mm to 4 mm in length and a thickness of no more than 1 mm.

[0016] Preferably, the composite material is ground into a 2D form in which the composite material particles have dimensions of 5 mm to 200 mm in length, 1 mm to 30 mm in width and 0.2 mm to 2 mm in thickness.

[0017] Preferably, the composite material comprises from 10% to 40% by weight of the particleboard.

[0018] Preferably, the synthetic resin comprises 5 to 20% by weight of the particleboard.

[0019] The following is an embodiment of the present invention.

[0020] According to the present invention, the manufacturing method of particleboard is as follows:

[0021] 1) grinding the composite material;

[0022] 2) mixing together, by weight, 0% to 60% of a ground composite material, 10% to 60% of a synthetic resin, and 0% to 90% of organic particles;

[0023] 3) placing the mixture in a mold or on a molding plate or a molding belt at a temperature of 18°C ​​to 250°C;

[0024] 4) performing two-stage pressing at a temperature of 18°C ​​to 250°C, wherein the first step comprises arranging or arranging the filler and matrix particles and degassing the composite material, and the second step comprises providing the final thickness at a temperature of 18°C ​​to 250°C and a pressure of 0.02 MPa to 5 MPa.

[0025] The abrasive composite material used may be a glass-epoxy composite material, a glass-polyester composite material, a carbon-epoxy composite material or a carbon-polyester composite material, and both glass fibers and carbon fibers may be present in the abrasive composite material bonded with synthetic resins. The abrasive composite material may be derived from the recycling of wind turbines or yacht and boat composite propellers or composite panels or other composite structures and articles, or may be a mixture of composite materials from the above or other sources.

[0026] In the case of a multilayer board, the formation of the cushion layer is as follows: by weight, an outer layer containing 0% to 60% of abrasive composite material is formed, then an intermediate layer containing 10% to 70% of abrasive composite material is formed, and finally an upper outer layer containing 0% to 60% of abrasive composite material is formed, wherein the proportion of the intermediate layer is 50% to 75%, or even up to 90%, of the manufactured board.

[0027] According to the present invention, the composite material used to manufacture the board can be ground into a 1D form, in which the particle mixture has a size of: 1 mm in length and a thickness not exceeding 1 mm; or ground into a 2D form, in which the particle mixture has a size of: 5 mm-200 mm in length, 5 mm-30 mm in width and 0.2 mm-2 mm in thickness.

[0028] Milled 2D and 1D composites are used to make OSB-type particleboards, while milled 1D composites are used to make particleboards, fiberboards and MDF.

[0029] The ground composite material does not absorb the binder, so using it reduces the amount of binder (resin) consumed - the resin applied to the particles does not penetrate into the particles, making the amount less than that required to cover the same amount of wood or plant particles. Therefore, due to the lack of absorption, the amount of resin required to bind the composite board particles is less than the amount required to bind the same amount of wood chips.

[0030] Due to grinding, the composite material has an uneven, rough / porous surface, which can easily get tangled with wood or plant debris.

[0031] Since the specific weight of the composite material is an average of 1800 kg / m 3 , therefore, it is best to add 10% to 40% (by weight) of composite materials to the particleboard.

[0032] The composite material content of the particleboard is not more than 60% by weight.

[0033] Using ground composite materials increases the hardness of the board, i.e. the more composite materials, the harder the board.

[0034] Using a higher content of abrasive composite in the outer layer of the mixture can improve its water resistance.

[0035] Commonly available synthetic resins are used to bond cut-out panels and composite materials. 5% to 20% of the weight of each panel is sufficient to bond the cut-out panels and composite materials.

[0036] Depending on the resin type, resin consumption can also be less than 5% when using expensive resins.

[0037] The pressing temperature of particleboard is 18℃-250℃, and the pressure is 0.2MPa-5.0MPa.

[0038] The particleboards of the present invention have been tested to determine the physical and mechanical properties.

[0039] 1. Test subjects

[0040] The purpose of the tests was to evaluate the physical and mechanical properties of particleboards with a thickness of 16 mm containing composite material additives derived from turboprop debris. The particleboards were irregular in shape and had cuts and holes from many other tests. As mentioned above, the proportion of turboprop debris on the provided boards was 10%, 20%, 30% and 40%. All variants were evaluated together.

[0041] 2. Basis for particleboard performance evaluation

[0042] The evaluation of the properties of the provided particleboard sheets is based on the relevant standards:

[0043] -Static bending strength-PN-EN310

[0044] -Elastic modulus-PN-EN310

[0045] -Tensile strength perpendicular to the board surface-PN-EN319

[0046] -Expansion thickness after immersion in water-PN-EN317

[0047] -Water content-PN-EN322

[0048] -Density-PN-EN323

[0049] -The flammability is determined based on a method that allows the determination of the degree of flammability of wood and wood-based panels. Samples of panels with a size of approximately 15x15 cm are dried at a temperature of 102±3°C for 24 hours. After cooling, the sample is placed on a stand so that the sample is positioned at 45° relative to the substrate. A burner is placed under the stand so that the distance between the wick and the sample is 5 cm. The flame under the sample is maintained for 3.5 minutes. After this period, if the burner is burning vigorously, the burner and the sample are extinguished. The test sample is weighed before the measurement, 5 minutes after the measurement, and 60 minutes after the measurement. The mass loss of the test sample is calculated based on the mass difference. The burning or glowing of the sample is observed during the burning of the sample, and the ignition time is recorded. After cooling, the size of the area destroyed by the flame is also determined using a planimeter. A thickness of not more than 18 mm and a density of 650 kg / m is used. 3 The furniture board (PB) is used as the reference board.

[0050] 3. Summary of test results

[0051] The test results of the test plate are shown in Table 1. According to the data presented therein, the average static bending strength of the test plate is 9.4 N / mm 2 , the average elastic modulus is 1910N / mm 2 , the tensile strength perpendicular to the test plane is 0.21N / mm 2 The tested board aged due to damage, delamination of the outer layers. By default, this type of board will age in the middle layers, so the delivered boards were tested with an additional density distribution. From the data in scenario 1, it can be seen that the maximum density is shifted closer to the center of the board, so the weaker layers are closer to the outer layers, causing the board to age in the particulate layer.

[0052] Table 1

[0053] Testing the properties of particleboard

[0054]

[0055]

[0056] *- Requirements for unfinished particleboards - Type P2 - Panels for interior use (including furniture) in dry conditions (thickness range > 13 mm to 20 mm),

[0057] **-Standard Deviation

[0058] The water absorption of the particleboards not treated with additional hydrophobic agents was at a level of 27%-33%, and the absorption was from 60% up to 100%, so the expansion and absorption values ​​of the tested boards were considered satisfactory. It can be seen that the tested boards reacted better to fire. All the evaluated properties of the evaluated boards were lower (better) than the control boards. Therefore, the evaluated boards are less prone to fire than the control boards, as shown in Figure 2. Figure 1 .

[0059] 4. Conclusions and comments

[0060] The particleboards used for the tests have good physical and mechanical properties. The values ​​obtained indicate a high potential for industrial production. The slightly lower values ​​of static bending strength and tensile strength perpendicular to the plane are not due to the use of additives, but result from the way they were manufactured in the laboratory. The experience of the Department of Mechanical Wood Technology (pol. Katedra Mechanicznej Technologii Drewna) shows that the quality of particle layers manufactured under laboratory conditions is usually much lower than that manufactured under industrial conditions. Due to the addition of propeller chips to the intermediate layer, it must be taken into account that the mechanical properties of the boards formed under industrial conditions are even higher than those of the benchmark boards manufactured completely from sawdust.

[0061] 5. Summary

[0062] Panels based on cut-outs and pellets or made from chips from propeller grinding represent a new solution to the current trend of reducing natural resources and phasing out raw materials over the entire life cycle. Composite materials derived from ground propeller parts can serve as an important alternative to wood chip parts.

[0063] The use of ground composite materials improves the waterproofing and thermal insulation properties of particleboard. The use of ground composite materials improves the flame retardancy of particleboard due to the non-combustible fibers contained in the composite materials. The use of ground GFK composite materials improves the electrical insulation of particleboard. The use of ground CFK composite materials can improve the electrical conductivity of particleboard.

[0064] The use of ground composites reduces the emission of organic matter (volatile organic compounds), especially from softwood.

[0065] The use of ground composite reduces the need for chemicals, thereby reducing VOC emissions in the finished board. The use of ground composite reduces the amount of water required to prepare the wood chips. Ground composite does not emit VOCs. With the addition of ground composite, the board swells in response to moisture to the same extent as the proportion of composite in the board.

Claims

1. A particleboard consisting of organic particles of a synthetic resin composite material, It is characterized in that Contains by weight 10% to 60% of ground composite material, 5% to 60% of synthetic resin and 10% to 85% of organic particles, especially wood and plant particles or fibers or a combination of these components.

2. The particle board according to claim 1, It is characterized in that The composite material is ground into a 1D form, wherein the particle mixture in this form has a size of 1 mm to 4 mm in length and a thickness not exceeding 1 mm.

3. The particleboard according to any one of claims 1 to 2, It is characterized in that The composite material is ground into a 2D form, wherein the particle mixture in this form has dimensions of 5 mm to 200 mm in length, 1 mm to 30 mm in width, and 0.2 mm to 2 mm in thickness.

4. The particleboard according to any one of claims 1 to 3, It is characterized in that The composite material comprises 10% to 40% by weight of the particle board.

5. The particleboard according to any one of claims 1 to 3, It is characterized in that Synthetic resins make up 5%-20% of particleboard by weight.

6. A method for manufacturing a particle board, Features: 1) grinding the composite material; 2) mixing together, by weight, 10% to 60% of a ground composite material, 5% to 60% of a synthetic resin, and 10% to 85% of organic particles; 3) placing the mixture in a mold or on a molding plate or a molding belt at a temperature of 18°C ​​to 250°C; 4) performing two-stage pressing at a temperature of 18°C ​​to 250°C, wherein the first step comprises arranging or arranging the filler and matrix particles and degassing the composite material, and the second step comprises providing the final thickness at a temperature of 18°C ​​to 250°C and a pressure of 0.02 MPa to 5 MPa.

7. The method according to claim 6, It is characterized in that In order to manufacture a multilayer board, it is necessary to form a cushion layer so as to form an outer layer containing 0% to 60% grinding composite material by weight, then form an intermediate layer containing 10% to 70% grinding composite material, and finally form an upper outer layer containing 0% to 60% grinding composite material, wherein the proportion of the intermediate layer is 50% to 90% of the manufactured board.

8. The method according to any one of claims 6 to 7, It is characterized in that The composite material is ground into a 1D form, wherein the particle size of this form is: 1mm-4mm in length and no more than 1mm in thickness.

9. The method according to any one of claims 6 to 8, It is characterized in that The composite material is ground into a 2D form, wherein the particle size of the composite material in this form is: 5mm-200mm in length, 1mm-30mm in width, and 0.2mm-2mm in thickness.

10. The method according to any one of claims 6 to 9, It is characterized in that The composite material comprises 10% to 40% by weight of the particle board.

11. The method according to claims 6-10, It is characterized in that The synthetic resin accounts for 5 to 20% by weight of the particle board.

Citation Information

Patent Citations

  • A composite board made from recycled and recyclable materials

    CN107206734A

  • Method for producing fiberboard by utilizing cementing property of straw fibers

    CN103203790A

  • Method for manufacturing glue-less fiber board by leak-free type hot pressing technology

    CN1654180A

  • Waterproof board

    JP2009067008A

  • Fire retardant ligno-cellulosic composite materials and a method for making the same