Photoactivated chlorine dioxide-releasing powder and method for producing same
By spray-drying the formed photoactivated powder at high temperature, chlorine dioxide is generated when exposed to visible light, the problem of toxic by-products in the prior art is solved, and an environmentally friendly disinfection and sterilization of ethylene oxide is provided. method.
Patent Information
- Application Number
- CN202280092373.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-02-22
- Filing Date
- 2022-04-18
- Publication Date
- 2024-12-06
AI Technical Summary
Detectable amounts of toxic by-products such as chlorine, chlorate and chlorite are present in existing chlorine dioxide generation methods, and ethylene oxide sterilization is potentially threatening to the environment and public health, requiring a An alternative process to reduce the use of ethylene oxide.
The photo-activated catalyst, alkali and sodium chlorite are mixed to form an aqueous suspension and spray-dried at high temperatures to form a solid powder, which produces chlorine dioxide when exposed to visible light without releasing a detectable amount of toxic by-products. The method involves mixing and spray drying in the dark, using high purity sodium chlorite and appropriate dispersant to stabilize the suspension, and controlling gas release by adjusting the pH and additives.
Achieves effective generation and release of chlorine dioxide by solid powder without releasing detectable amounts of toxic by-products, providing an alternative, environmentally friendly disinfection and sterilization method for ethylene oxide. .
Abstract
Description
Technical Field
[0001] Photoactivated powders for generating and releasing chlorine dioxide and methods for making the same are provided. More specifically, photoactivated powders are provided that are capable of solid-state generation and release of chlorine dioxide without detectable amounts of any toxic byproducts and are prepared under conditions that maximize the activity of the powder for use in disinfection, sanitation, sterilization, and control of biological or pathogenic contamination. Background Art
[0002] Currently, ethylene oxide is used to sterilize medical devices and other products. The U.S. Food and Drug Administration recognizes that ethylene oxide has potential adverse effects on the environment and public health. The FDA is encouraging changes to ethylene oxide sterilization processes and equipment that will reduce the amount of ethylene oxide on medical devices.
[0003] When chlorine dioxide is generated from some conventional chlorine dioxide generating products, detectable amounts of toxic byproducts including chlorine gas, chlorate, and / or chlorite have been observed. Summary of the invention
[0004] One option for reducing ethylene oxide concentrations on medical devices is to replace ethylene oxide entirely with a different gas produced by a process that has less impact on the environment and public health.
[0005] In a first aspect of the invention, there is provided a method for preparing a light-activated powder for providing a solid state controlled release of chlorine dioxide, the method comprising: mixing a light-activated catalyst, a base, sodium chlorite and water to form an aqueous suspension; and spray drying the suspension at an inlet temperature in the range of about 482°C to about 537°C (900°F to 1000°F) and an outlet temperature not exceeding 143°C (290°F) to form a powder. The mixing and spray drying steps are performed in the dark. When exposed to visible light, the powder is capable of generating a disinfecting, sanitizing, sterilizing effective amount of chlorine dioxide from the powder in a solid state controlled release without releasing detectable amounts of chlorine, chlorate and / or chlorite.
[0006] The aqueous suspension may include sodium chlorite in an amount of 85% to 99% purity.
[0007] When exposed to visible light, the powder is capable of generating a disinfecting, sanitizing, sterilizing effective amount of chlorine dioxide controlled release from the solid state of the powder without releasing detectable amounts of toxic byproducts such as chlorine gas and / or chlorites, chlorates.
[0008] The powder prepared by this method is capable of generating a controlled release of chlorine dioxide from the solid state of the powder without exposing the powder to moisture, relative humidity, or an acid-releasing agent prior to or during exposure of the powder to visible light. The acid-releasing agent is an acid, a substance that is hydrolyzable to an acid (i.e., a substance that reacts with water diffused into the powder to form an acid), or a mixture thereof. The hydronium ions (if present) generated by the acid hydrolysis will diffuse through the powder and react with the chlorite anions to generate chlorine dioxide.
[0009] As a second aspect of the present invention, a photoactivated powder is provided. The photoactivated powder is prepared by the method described in the first aspect and examples of the present invention. When exposed to visible light, the powder is capable of generating a disinfection, sanitation, and sterilization effective amount of chlorine dioxide to be controlledly released from the solid state of the powder without releasing detectable amounts of toxic byproducts such as chlorine gas and / or chlorite and chlorate.
[0010] Other objects and features will be in part apparent and in part pointed out hereinafter. BRIEF DESCRIPTION OF THE DRAWINGS
[0011] not applicable. DETAILED DESCRIPTION
[0012] A method of making a light-activated powder has been discovered that provides solid-state generation and release of chlorine dioxide without detectable amounts of any toxic byproducts, such as chlorine, chlorate and / or chlorite. The method includes an inlet spray drying temperature that is much higher than the 180°C decomposition temperature of sodium chlorite. Chlorine dioxide is generated and released from a "solid-state" powder, meaning that the powder does not include a source of moisture, such as unbound water or acid, that would trigger the release of chlorine dioxide. The powder does not need to be exposed to moisture, relative humidity or acid before or during exposure of the powder to visible light to generate the gas. When exposed to light, the powder is able to generate and release the gas after activation of the catalyst by oxidation or reaction of light and sodium chlorite.
[0013] The powder may be prepared under conditions that minimize or prevent decomposition or oxidation of the sodium chlorite or premature photoactivation of the powder during the manufacturing process to maximize its activity.
[0014] As a first aspect of the present invention, there is provided a method for preparing a photoactivated powder for providing a solid controlled release of chlorine dioxide, the method comprising: mixing a photoactivated catalyst, a base, sodium chlorite and water to form an aqueous suspension; and spray drying the suspension at an inlet temperature in the range of about 482°C to about 537°C (900°F to 1000°F) and at an outlet temperature in the range of about 121°C (250°F) to about 143°C (290°F) to form a powder. The aqueous suspension comprises sodium chlorite of 85% to 99% purity. The mixing and spray drying steps are performed in the dark.
[0015] When exposed to visible light, the powder is capable of generating a controlled release of a disinfecting effective amount of chlorine dioxide from the solid state of the powder without releasing detectable amounts of chlorine gas, chlorite, or chlorate.
[0016] When the powder is exposed to light, such as visible light, the catalyst is activated and the chlorite anions are oxidized or reacted to generate and release chlorine dioxide.
[0017] The powder prepared by this method is capable of generating a controlled release of chlorine dioxide from the solid state of the powder without exposing the powder to moisture, relative humidity, or acid prior to or during exposure of the powder to visible light.
[0018] When preparing the aqueous suspension in the method of the present invention, a dispersant can be mixed with a catalyst, an alkali, sodium chlorite and water. The dispersant can reduce agglomeration in the suspension. The dispersant can include a nonionic surfactant. Examples of nonionic surfactants include, but are not limited to, secondary alcohol ethoxylates, alkylphenol ethoxylates, alkyl ethoxylates, alkylaryl ethoxylates, polyethylene oxide-polypropylene oxide block copolymers, polyethylene glycol ethers of linear alcohols, reaction products of fatty acids with ethylene oxide and / or propylene oxide, polyvinyl alcohol, polyvinyl pyrrolidone, copolymers of polyvinyl alcohol and polyvinyl pyrrolidone, copolymers of (meth) acrylic acid and (meth) acrylic esters, or combinations thereof.
[0019] The aqueous suspension is also preferably maintained at an alkaline pH of about 9 to about 14, preferably about 9 to about 11. The pH can be maintained by adjusting the concentration of the base added when forming the aqueous suspension.
[0020] It is believed that the base in the aqueous suspension stabilizes the chlorite anion during processing and participates in electron transfer by generating hydroxyl radicals that aid in the oxidation of the anion. The amount of base in the powder can be adjusted to change the time period of gas release and to improve thermal stability. Up to about 50% by weight of the base can be included based on the total weight of the powder. Suitable bases include, but are not limited to, alkali metal hydroxides such as lithium hydroxide, sodium hydroxide, or potassium hydroxide; alkaline earth metal hydroxides such as calcium hydroxide or magnesium hydroxide; hydroxide salts of transition metal ions; protonated primary, secondary, or tertiary amines, or quaternary amines such as ammonium hydroxide. Sodium hydroxide is preferred.
[0021] In the process of the present invention, the aqueous suspension may be an azeotrope. When the aqueous suspension is an azeotrope, the spray drying inlet temperature may be as high as 537°C (1000°F) while still avoiding decomposition of sodium chlorite. The azeotrope may include a mixture of solvents including, but not limited to, acetone, acetonitrile, acrylonitrile, alcohols (e.g., ethanol, methanol, isopropanol, tert-butyl alcohol), enols, alkanes (e.g., hexane, 2-methylpentane), alkenals, halogenated alkanes (e.g., dichloromethane, trichlorotrifluoroethane), nitroalkanes (e.g., nitromethane), aniline, cycloalkanes (e.g., cyclopentane, cyclohexane), benzene, alkylbenzenes, halogenated benzenes, carbon disulfide, carbon tetrachloride, chloroform, epichlorohydrin, alkylamines, dialkylamines, alkyl halides (e.g., methyl iodide, ethyl iodide), alkyl ethers (e.g., isopropyl ether), alkyl acetates (e.g., methyl acetate), halogenated alkenes, alkenyl chlorides, trifluoroacetic acid, toluene, xylene, or any combination thereof.
[0022] For example, the aqueous suspension may include an azeotrope comprising acetone and one or more solvents comprising ethanol, methanol, isopropanol, tert-butanol, hexane, 2-methylpentane, dichloromethane, trichlorotrifluoroethane, nitromethane, cyclopentane, cyclohexane, carbon disulfide, carbon tetrachloride, chloroform, methyl iodide, ethyl iodide, isopropyl ether, methyl acetate, or trifluoroacetic acid.
[0023] The light used to activate the photoactivated catalyst of the powder can be sunlight, fluorescence, incandescent light or ultraviolet light. Visible light (such as blue light) is a preferred light source. If it is desired to limit the wavelength range transmitted to the catalyst, additives such as UV blockers may also be included in the powder. Photosensitizers may be added to change the absorption wavelength of the powder, particularly to change the ultraviolet absorption wavelength to a visible absorption wavelength to improve activation of indoor lighting. UV absorbers may be added to the composition to slow down the rate of gas generation and release.
[0024] Photoactivated catalysts are commonly used to catalyze oxidation and reduction reactions. When photons are absorbed by the catalyst, electrons are promoted from the valence band to the conduction band, generating valence band holes. The holes and electrons diffuse to the surface of the catalyst particles, where each can undergo a chemical reaction. The valence band holes oxidize water molecules adsorbed at the catalyst surface to generate hydroxyl radicals.
[0025] Any semiconductor activated by light or particles or other materials incorporating such semiconductors can be used as photoactivated catalysts. Such semiconductors are typically metals, ceramics, inorganic or polymeric materials prepared by various processes known in the art (such as sintering). The catalysts used in the present invention are commercially available in a wide range of particle sizes from nanoparticles to granules.
[0026] The photoactivated catalyst in the aqueous suspension may include metal oxides, metal sulfides, metal chalcogenides, metal phosphides, metal arsenides, non-metallic semiconductors, polymer semiconductors, photosensitive isopolyanions, photosensitive heteropolyions, or combinations thereof. Preferably, the photoactivated catalyst includes metal oxides.
[0027] When the photoactivated catalyst is a metal oxide, the metal oxide may include, but is not limited to, titanium dioxide, zinc oxide, tungsten trioxide, ruthenium dioxide, iridium dioxide, tin dioxide, strontium titanate, barium titanate, tantalum oxide, calcium titanate, iron (III) oxide, molybdenum trioxide, niobium pentoxide, indium trioxide, cadmium oxide, hafnium oxide, zirconium oxide, manganese dioxide, copper oxide, vanadium pentoxide, chromium trioxide, yttrium trioxide, silver oxide, or Ti. x Zr 1-x O2, wherein x is between 0 and 1. Transition metal oxides such as titanium dioxide and zinc oxide are preferred because they are chemically stable, non-toxic, inexpensive, exhibit high photocatalytic activity, and are available as nanoparticles for the preparation of transparent molded or extruded plastic products. Preferably, the photoactivated catalyst comprises titanium dioxide, and more preferably, comprises rutile titanium dioxide.
[0028] Without being bound by any particular theory, it is believed that when the powder produced as described herein includes rutile titanium dioxide, the titanium dioxide has a high electron density flat surface that adsorbs atmospheric water. The adsorbed water can be, for example, associated water molecules, dissociated hydroxyls in direct contact with the surface, or water molecules hydrogen bonded to associated water and structural oxygen atoms at the surface. The amount of adsorbed water can be determined by differential scanning calorimetry. It is also believed that the dispersant, if present, can bind to the titanium dioxide and provide a source of hydronium ions. The water adsorbed at the titanium dioxide surface can then be used to generate chlorine dioxide for release from the solid state of the powder.
[0029] When the catalyst is a metal sulfide, the metal sulfide may include cadmium sulfide, zinc sulfide, indium sulfide, copper sulfide, tungsten disulfide, bismuth trisulfide, or cadmium zinc disulfide.
[0030] When the catalyst is a metal chalcogenide, the metal chalcogenide may include zinc selenide, cadmium selenide, indium selenide, tungsten selenide, or cadmium telluride.
[0031] When the catalyst is a non-metallic semiconductor, the non-metallic semiconductor may include silicon, silicon carbide, diamond, germanium, germanium dioxide, or germanium telluride.
[0032] Other representative catalysts include indium phosphide; gallium arsenide; polyacetylene; including W 10 O 32 -4 or including XM 12 O 40-n or X2M 18 O 62 -7 The photosensitive heteropoly ion is a photosensitive heteropoly ion, wherein x is Bi, Si, Ge, P or As, M is Mo or W, and n is an integer from 1 to 12.
[0033] An inert atmosphere, such as a nitrogen blanket, may be used during the process. An inert atmosphere may be present during the entire process, or during the mixing step, the spray drying step, when collecting the spray dried product and / or when storing the spray dried product.
[0034] Aqueous suspensions can be prepared by mixing their ingredients in any order of addition. For example, sodium chlorite can be mixed with water and a base to form a solution, a solvent can be added to the solution to form an azeotrope, and a photoactivated catalyst can be mixed with the solution or azeotrope to form a suspension. Alternatively, the catalyst and solvent can be mixed to form a slurry, and sodium chlorite can be added to the slurry to form a suspension, or both the catalyst and sodium chlorite can be mixed with a solvent prior to mixing to form a suspension. When preparing the suspension, ultrasonic mixing, high shear mixing, or any conventional homogenization method can be used.
[0035] Once the suspension is formed, it can be spray dried to form a powder by any method known in the art, including, for example, any known atomization method, such as a nozzle or a rotating disk. Typically, the inlet temperature is maintained at about 482°C to about 537°C (900°F to 1000°F), and the outlet temperature is maintained in the range of about 121°C (250°F) to about 143°C (290°F). The spray drying process usually occurs quickly (e.g., within about 60 seconds at most). If desired, the powder can then be further dried by any conventional method.
[0036] After spray drying to form a powder, the powder can be mixed with a desiccant to further protect the powder from moisture activation. The desiccant can include, but is not limited to, silicon dioxide, silicates such as sodium silicate, sodium metasilicate, sodium sesquisilicate, sodium orthosilicate, borosilicates, aluminosilicates, zeolites, sodium sulfide, or a combination thereof.
[0037] The powder can then be packaged in a container that blocks wavelengths of light that can activate the catalyst.
[0038] The powder produced by the method of the present invention may include about 50 wt % to about 99.99 wt % photocatalyst and about 0.01 wt % to about 50 wt % sodium chlorite; about 70 wt % to about 97 wt % photoactivated catalyst and about 3 wt % to about 30 wt % sodium chlorite; or about 80 wt % to about 95 wt % photoactivated catalyst and about 5 wt % to about 20 wt % sodium chlorite.
[0039] The chlorine dioxide release rate effective for disinfection may be in the range of, for example, about 0.08 ppm / minute to about 8.0 ppm / minute for a period of about 2 hours to about 72 hours.
[0040] As a second aspect of the present invention, a photoactivated powder is provided. The photoactivated powder is prepared by the method described in the first aspect and examples of the present invention. When exposed to visible light, the powder is capable of generating a disinfection effective amount of chlorine dioxide to be controlledly released from the solid state of the powder without releasing a detectable amount of chlorine gas and / or chlorite or chlorate.
[0041] The application of powder is very extensive. They can be used in most any environment that may be exposed to light. Powder can be formed into solid by molding or sintering. Powder can also be impregnated, melt processed, sintered, blended with other powders, or otherwise incorporated into various materials to provide films, fibers, coatings, tablets, resins, polymers, plastics, tubing, films, engineering materials, paints, coatings and adhesives, thereby being used for a wide range of end-use applications. Powder is particularly useful for preparing any injection molded product, compression molded product, thermoforming (thermoforming) product or extrusion molded product, such as cast or blown film. The thermal stability of powder allows them to be used in injection molding processes.
[0042] The powder of the present invention is preferably incorporated into the plastic product of injection molding, compression molding, thermoforming or extrusion molding, which is by compounding and granulating the powder via conventional means, and mixing the pellets with the material before conventional molding or molding process. Suitable materials for forming these products include any polymer, multi-component polymer (such as copolymer, terpolymer or oligomer) and their polymer alloys or blends or any wax. Representative polymers include polyolefins, such as polyethylene and polypropylene, polyethylene terephthalate, polyvinyl chloride, polyurethane, metallocene polymers, polyesters, polyacrylates, acrylic acid, polystyrene, polycarbonate, polyamide, polyesteramide, ethylene-vinyl acetate copolymer, ethylene-methacrylate copolymer and polyacetal. Suitable wax includes microcrystalline wax, paraffin and synthetic wax, such as chlorinated wax, polyethylene wax, polyethylene glycol and polypropylene glycol. Preferably, polymer is biodegradable.
[0043] The shaped or molded product preferably comprises from about 0.1 wt % to about 70 wt % of the powder of the present invention and from about 30 wt % to about 99.9 wt % of the material, and more preferably, from about 1 wt % to about 50 wt % of the powder of the present invention and from about 50 wt % to about 99 wt % of the material, and most preferably, from about 2 wt % to about 50 wt % of the powder of the present invention and from about 50 wt % to about 98 wt % of the material.
[0044] The shaped or molded product can be prepared by any conventional polymer processing method. For example, the powder or powder pellets of the present invention and the material can be mixed together in a mixer such as a Henschel mixer and fed to an extruder or molding equipment operating at a temperature not exceeding about 200° C. to form a melt. The melt can be extruded as a film cast, cooled on a vibrating conveyor using dry air to form pellets, or formed into a desired shape by conventional injection molding, thermoforming or compression molding methods.
[0045] The melt can be applied as a thin film on a surface using well-known hot melt, dip coating, spray coating, curtain coating, dry wax, wet wax and lamination processes. When the powder is in nanoparticle form (eg, 5 to 20 micrometers in diameter), a transparent film can be formed.
[0046] Conventional film-forming additives may be added to the material as desired. Such additives include crosslinkers, UV stabilizers, flame retardants, emulsifiers, compatibilizers, lubricants, antioxidants, colorants and dyes.
[0047] A multilayer composite material can be formed to generate gas within a housing formed by the composite material. Such a composite material includes a gas generating layer and a barrier layer. The gas generating layer includes a powder. The barrier layer is adjacent to a surface of the gas generating layer. The barrier layer is light transmissive so that it transmits light to the gas generating layer. However, the barrier layer is impermeable, or only semi-permeable, to the gas generated and released by the gas generating layer. After activation of the catalyst and oxidation or reaction of the chlorite anion, the gas generating layer is capable of generating and releasing chlorine dioxide when exposed to light.
[0048] The gas-releasing powders, films or other compositions of the present invention can be used to retard, kill, prevent or control microbial contamination or biochemical decomposition on the surface of a material, in the material or in the atmosphere surrounding the material by placing the material adjacent to the composition of the present invention and exposing the composition to light to release chlorine dioxide from the composition into the atmosphere surrounding the material. Microbial contaminants may include bacteria, viruses, molds and fungi.
[0049] The composition may also be used to retard, prevent or control biological contamination of the atmosphere by exposing the composition to light to generate chlorine dioxide and release it from the composition into the atmosphere surrounding the composition.
[0050] As used herein, delaying, preventing or controlling biocontamination is also referred to as "sanitization," "disinfection," or "sterilization." Biocontamination can include bacteria, viruses such as coronaviruses (e.g., SARS-COV-2 and variants thereof such as Delta or Omicron variants), molds, and fungi.
[0051] The composition can also be used to delay, prevent or control biological contamination of a material by placing the material adjacent to the composition and exposing the composition to light to generate chlorine dioxide and release it from the composition into the atmosphere surrounding the material. For example, chlorine dioxide is used to inactivate biological contaminants (e.g., anthrax) after biological warfare or for other military decontamination.
[0052] For example, the powder or any composition containing the powder (such as a film) can be placed in a sealable bag or other container for sterilizing medical devices, or in a "red bag" for decontaminating or disinfecting medical waste or personal protective equipment (such as masks, gowns and pants). Alternatively, the bag or container can be made of a film containing the powder of the present invention. The chlorine dioxide released by the powder or composition can be effective against SARS-COV-2 and its variants, such as Delta or Omicron variants.
[0053] Since the chlorine dioxide generated by the powder of the present invention is dry and non-humid, the powder can also effectively sterilize electronic devices without corroding the electronic devices. This can be beneficial in resisting the effects of pathogens on electronic devices in battlefield contamination caused by the use of biological warfare.
[0054] The composition may also be used to deodorize the surface of a material or the atmosphere surrounding the material, or to enhance the freshness of a material by placing the material adjacent to the composition and exposing the composition to light to generate and release chlorine dioxide from the composition into the atmosphere surrounding the material.
[0055] The composition can also be used to delay, prevent, inhibit or control the chemotactic attraction of an organism to a material by placing the material adjacent to the composition and exposing the composition to light to generate and release chlorine dioxide from the composition into the atmosphere surrounding the material.
[0056] In the above method, the surface of the material or the entire material can be impregnated with the powder of the present invention or coated with the composition, the composition can be mixed with the material, the composition can be enclosed in a gas-permeable container, or the material and the composition can be enclosed in a container. When the composition is enclosed in a container, the container can be hermetically sealed, or partially sealed so that some gas leaks from the container.
[0057] The chlorine dioxide-releasing powder can be impregnated into containers for storing food, soap, laundry detergent, documents, clothing, paint, seeds, medical equipment, devices and supplies (such as catheters and sutures), personal care products, medical or biological waste, sports shoes, ostomy bags, footwear and garbage, for example. Such powders can also be impregnated into covers for medical, hospital, household or commercial equipment or covers for storage. Pouches, pouches, "tea bags" or other breathable containers of powder can be included in the storage container to provide a chlorine dioxide micro-atmosphere when activated. The chlorine dioxide-releasing powder can also be impregnated into paper or polymeric materials (e.g., shower mats, shoe insoles or shoe insoles, bandage materials, cutting boards, food packaging materials, food packaging trays, seed packets, or air filters); incorporated into wax or polymer coatings applied to cardboard containers or other surfaces; incorporated into films, such as packaging films or coverings for storage or medical, hospital, household, or commercial equipment; formed into porous portions to sterilize water; mixed with materials to create a micro-atmosphere of chlorine dioxide around materials (e.g., soil); or mixed with other powders to kill microorganisms, enhance freshness, or deodorize (e.g., foot powders, bath powders, powders for treating soft surfaces such as carpet powders, desiccants for removing moisture).
[0058] These powders may also be used to: neutralize odors, delay, prevent, inhibit or control chemotaxis (ie, the attraction of living organisms to chemicals); or reduce or eliminate bacteria in animal feed and potentially reduce the bacterial load in the intestines of animals consuming the feed.
[0059] The compositions of the present invention effectively release gas at temperatures (including refrigeration temperatures) commonly encountered in the above-mentioned applications. Compositions that release chlorine dioxide can be used, for example, to package medical supplies, food, or other materials that require refrigeration to sterilize or deodorize the material. Multilayer films including barrier layers can also be used to form packages, such as for medical supplies or food. The barrier layer retains the generated gas in the package, for example, to increase shelf life and prevent mold growth in food or to improve the sterilization of medical supplies.
[0060] Having now described the invention in detail, it will be apparent that modifications and variations are possible without departing from the scope of the invention defined in the appended claims.
[0061] Example
[0062] The following non-limiting examples are provided to illustrate the invention.
[0063] Example 1
[0064] A liquid slurry was prepared in a blending tank, which was spray dried to form a light activated powder. The blending tank had an agitator that was on during the addition of all ingredients. The lighting in the manufacturing area was dimmed to less than 12 lumens.
[0065] First, fill a blending tank with deionized water. Sodium hydroxide (1.2 wt % of a 50% solution) is added to the water to form a solution. Sodium chlorite powder (3.0 wt %) is slowly added to the solution, followed by 26.4 wt % of titanium dioxide to form a slurry. The amounts listed are based on the total weight of the liquid slurry before spray drying. The slurry is then transferred to the feed tank of a spray dryer, which is also equipped with an agitator.
[0066] About 57 kg (125 lb) of a liquid slurry containing dissolved sodium chlorite, sodium hydroxide and suspended titanium dioxide was pumped into the spray dryer using a positive displacement pump. The absolute viscosity of the slurry ranged from 950 centipoise to 1750 centipoise at 29°C (85°F) and a pH of 12.3. The inlet temperature of the spray dryer ranged from 510°C (950°F) to 527°C (980°F) throughout the run. The outlet temperature ranged from 121°C (250°F) to 124°C (255°F). The slurry was spray dried to produce a powder.
[0067] The resulting fine white powder was screened through a 50 micron screen into a polymer drum lined with two opaque plastic bags. A perforated hose connected to a nitrogen bottle was inserted into the drum to facilitate cooling. Once the temperature dropped to 32°C (90°F), the bags and drums were sealed. Multiple samples of the finished powder were collected throughout the run and tested for chlorine dioxide production when exposed to an LED light strip. After exposing 5 grams of powder to an LED light source for 30 seconds, the production of more than 25 ppm of chlorine dioxide was consistently observed.
[0068] Example 2
[0069] Titanium dioxide (99.9% rutile (Aldrich Chemical)) was mixed with sodium chlorite solution (technical grade (Aldrich Chemical)), sodium hydroxide, acetone, a solvent that forms an azeotrope with acetone, and water to form a suspension and immediately spray dried in the dark (less than 12 lumens) and under a nitrogen blanket at an inlet temperature in the range of about 482°C to about 537°C (900°F to 1000°F) and an outlet temperature not exceeding 143°C (290°F) to form a white powder. The powder was placed in a wide-mouth bottle and monitored with a 0 ppm to 100 ppm chlorine dioxide electrochemical sensor. When the powder was exposed to visible light, chlorine dioxide was generated and released from the white powder within several hours of the test. Gas release was suspended when the powder was kept in the dark, and gas release resumed when the powder was exposed to visible light again.
[0070] Pellets Formation: The spray dried powder was compounded into pellets using 2 melt index linear low density polyethylene (LLDPE) resin (manufactured by Rexene) at a concentration of 20% powder and 80% resin. The manufacture of pellets was carried out in the dark under nitrogen. The pellets were stored in aluminum foil / plastic laminate containers to protect them from exposure to light.
[0071] Film Formation: The pellets were blown into films using 2 melt index Rexene LLDPE resin (50% dilution). The resulting film contained about 10% by weight of powder. The film was made in the dark under nitrogen. The film was stored in an aluminum foil / plastic laminate container to protect it from exposure to light.
[0072] Photoactivation of film under dry conditions: The film samples were placed in a jar with a 0 ppm to 10 ppm chlorine dioxide electrochemical detector attached to the lid (including desiccant to produce 0% relative humidity) and covered with aluminum foil for several days to avoid light. No chlorine dioxide was generated during this period. Illumination of the sample with ambient fluorescent room lighting resulted in immediate generation of chlorine dioxide.
[0073] Photoactivation of film under light cycle: 1g of film sample was placed in a 500ml wide mouth bottle with a 0ppm to 10ppm 15 chlorine dioxide electrochemical detector attached to the lid and covered with aluminum foil for about 10 minutes to avoid light. No chlorine dioxide was generated during this period. Irradiation of the sample with ambient fluorescent room lighting for about 10 minutes to 30 minutes resulted in immediate generation of chlorine dioxide. The film was covered with foil, during which no chlorine dioxide was generated. When the foil was removed and the film was exposed to room light, chlorine dioxide was generated.
[0074] definition
[0075] As used herein, the term "suitable substituent" is intended to mean a chemically acceptable functional group, preferably a part that does not counteract the activity of the compounds of the present invention. Such suitable substituents include, but are not limited to, halide groups, perfluoroalkyl groups, perfluoroalkoxy groups, alkyl groups, alkenyl groups, alkynyl groups, hydroxyl groups, oxo groups, sulfhydryl groups, alkylthio groups, alkoxy groups, aryl or heteroaryl groups, aryloxy or heteroaryloxy groups, aralkyl or heteroaralkyl groups, aralkyloxy or heteroaralkyloxy groups, HO-(C=O)-groups, heterocyclic groups, cycloalkyl groups, amino groups, alkylamino and dialkylamino groups, carbamoyl groups, alkylcarbonyl groups, alkoxycarbonyl groups, alkylaminocarbonyl groups, dialkylaminocarbonyl groups, arylcarbonyl groups, aryloxycarbonyl groups, alkylsulfonyl groups, and arylsulfonyl groups. It will be appreciated by those skilled in the art that many substituents may be substituted with additional substituents.
[0076] As used herein, the term "alkyl" refers to a straight chain, branched chain or cyclic hydrocarbon group, preferably having 1 to 32 carbon atoms (i.e., 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 39, 30, 31 or 32 carbons), and more preferably having 1 to 18 carbon atoms. Alkyl groups include, but are not limited to, methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl and tert-butyl. Alkyl groups can be unsubstituted or substituted with one or more suitable substituents.
[0077] As used herein, term "alkenyl" refers to a straight chain, branched or cyclic hydrocarbon group, preferably having 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 39, 30, 31 or 32 carbons, more preferably having 1 to 18 carbon atoms, and having one or more carbon-carbon double bonds. Alkenyl groups include but are not limited to vinyl, 1-propenyl, 2-propenyl (allyl), isopropenyl, 2-methyl-1-propenyl, 1-butenyl and 2-butenyl. Alkenyl groups can be unsubstituted or substituted by one or more suitable substituents, as defined above.
[0078] The term "alkynyl" as used herein refers to a straight chain, branched or cyclic hydrocarbon group, preferably having 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 39, 30, 31 or 32 carbons, more preferably having 1 to 18 carbon atoms, and having one or more carbon-carbon triple bonds. Alkynyl groups include, but are not limited to, ethynyl, propynyl and butynyl. Alkynyl groups can be unsubstituted or substituted with one or more suitable substituents, as defined above.
[0079] The term "aryl" or "ar" as used herein alone or as part of another group (e.g., aralkyl) means a monocyclic, bicyclic or tricyclic aromatic group such as phenyl, naphthyl, tetrahydronaphthyl, indanyl, etc., optionally substituted with one or more suitable substituents, preferably 1 to 5 suitable substituents, as defined above. The term "aryl" also includes heteroaryl.
[0080] "Arylalkyl" or "aralkyl" means an aryl group attached to a parent molecule through an alkylene group. The number of carbon atoms in the aryl group and the alkylene group is selected so that there are a total of about 6 to about 18 carbon atoms in the arylalkyl group. A preferred arylalkyl group is benzyl.
[0081] As used herein, the term "cycloalkyl" refers to a monocyclic, bicyclic or tricyclic carbocyclic group (e.g., cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, cycloheptyl, cyclooctyl, cyclononyl, cyclopentenyl, cyclohexenyl, bicyclo[2.2.1]heptyl, bicyclo[3.2.1]octyl and bicyclo[5.2.0]nonyl, etc.); optionally containing 1 or 2 double bonds. The cycloalkyl group may be unsubstituted or substituted with one or more suitable substituents, preferably 1 to 5 suitable substituents, as defined above.
[0082] As used herein, "darkness" refers to light intensities not exceeding about 129 lux (ie, 12 foot candles) to avoid photoactivation of the photoactivated catalyst.
[0083] The term "-ene" used as a suffix as part of another group represents a divalent group in which a hydrogen atom is removed from each of the two terminal carbons of the group, or if the group is cyclic, from each of two different carbon atoms in the ring. For example, alkylene represents a divalent alkyl group, such as ethylene (-CH2CH2-) or isopropylene (-CH2(CH3)CH2-). For clarity, the addition of the -ene suffix is not intended to change the definition of the main word, except for indicating a divalent group. Thus, continuing with the above example, alkylene represents an optionally substituted straight-chain saturated divalent hydrocarbon group.
[0084] As used herein, the term "ether" refers to a divalent (ie, difunctional) group that includes at least one ether linkage (ie, -O-).
[0085] As used herein, the term "heteroaryl" refers to a monocyclic, bicyclic or tricyclic aromatic heterocyclic group containing one or more heteroatoms (e.g., 1 to 3 heteroatoms) selected from O, S and N in the ring. Heteroaryl groups include, but are not limited to, pyridyl, pyrazinyl, pyrimidinyl, pyridazinyl, thienyl, furanyl, imidazolyl, pyrrolyl, oxazolyl (e.g., 1,3-oxazolyl, 1,2-oxazolyl), thiazolyl (e.g., 1,2-thiazolyl, 1,3-thiazolyl), pyrazolyl, tetrazolyl, triazolyl (e.g., 1,2,3-triazolyl, 1,2,4-triazolyl), oxadiazolyl (e.g., 1,2,3-oxadiazolyl), thiadiazolyl (e.g., 1,3,4-thiadiazolyl), quinolyl, isoquinolyl, benzothienyl, benzofuranyl and indolyl. A heteroaryl group may be unsubstituted or substituted by one or more suitable substituents, preferably 1 to 5 suitable substituents, as defined above.
[0086] The term "hydrocarbon" as used herein describes a compound or radical consisting solely of the elements carbon and hydrogen.
[0087] The term "substituted" means that in the group in question, at least one hydrogen atom bonded to a carbon atom is replaced by one or more substituents, such as hydroxyl (-OH), alkylthio, phosphino, amido (-CON(RA)(RB), wherein RA and RB are independently hydrogen, alkyl or aryl), amino (-N(RA)(RB), wherein RA and RB are independently hydrogen, alkyl or aryl), halide (fluorine, chlorine, bromine or iodine), silyl, nitro (-NO2), ether (-ORA, wherein RA is alkyl or aryl), ester (-OC(O)RA, wherein RA is alkyl or aryl), ketone (-C(O)RA, wherein RA is alkyl or aryl), heterocycle, etc. When the term "substituted" introduces or follows a list of possible substituent groups, the term is intended to apply to each member of the group. That is, the phrase "optionally substituted alkyl or aryl" should be interpreted as "optionally substituted alkyl or optionally substituted aryl". Likewise, the phrase "alkyl or aryl optionally substituted by fluorine" should be interpreted as "alkyl optionally substituted by fluorine or aryl optionally substituted by fluorine".
[0088] When introducing elements of the present invention or the preferred embodiments thereof, the articles "a", "an", "the" and "said" are intended to mean that there are one or more elements. The terms "comprising", "including" and "having" are intended to be inclusive and mean that there may be additional elements besides the listed elements.
[0089] From the above, it will be seen that the several objects of the invention are achieved and other advantageous results attained.
[0090] As various changes could be made in the above products and methods without departing from the scope of the invention, it is intended that all matter contained in the above description and shown in the accompanying drawings shall be interpreted as illustrative and not in a limiting sense.
Claims
1. A method for preparing a light-activated powder for providing solid-state controlled release of chlorine dioxide, the method comprising: mixing a photoactivated catalyst, a base, sodium chlorite, and water to form an aqueous suspension comprising 85% to 99% pure sodium chlorite; as well as spray drying the suspension at an inlet temperature in the range of about 482°C to about 537°C (900°F to 1000°F) and an outlet temperature not exceeding 143°C (290°F) to form a powder, in: The mixing and spray drying steps were performed in the dark, and When exposed to visible light, the powder is capable of generating a controlled release of a disinfecting effective amount of chlorine dioxide from the solid state of the powder without releasing detectable amounts of chlorine gas, chlorate, and / or chlorite.
2. The method of claim 1, further comprising mixing a dispersant with the catalyst, the base, the sodium chlorite and the water to form the aqueous suspension.
3. The method of claim 2, wherein the dispersant comprises a nonionic surfactant.
4. The method according to claim 3, wherein the nonionic surfactant comprises secondary alcohol ethoxylates, alkylphenol ethoxylates, alkyl ethoxylates, alkylaryl ethoxylates, polyethylene oxide-polypropylene oxide block copolymers, polyethylene glycol ethers of linear alcohols, reaction products of fatty acids with ethylene oxide and / or propylene oxide, polyvinyl alcohol, polyvinyl pyrrolidone, copolymers of polyvinyl alcohol and polyvinyl pyrrolidone, copolymers of (meth)acrylic acid and (meth)acrylates, or any combination thereof.
5. The method according to any one of claims 1 to 4, wherein the pH of the aqueous suspension is from about 9 to about 14.
6. The method of any one of claims 1 to 4, wherein the pH of the aqueous suspension is from about 9 to about 11.
7. The process according to any one of claims 1 to 6, wherein the aqueous suspension is an azeotrope.
8. The method of claim 7, wherein the azeotrope in the aqueous suspension comprises acetone, acetonitrile, acrylonitrile, alcohol, enol, alkane, alkenal, alkyl halide, aniline, cycloalkane, benzene, alkylbenzene, halogenated benzene, carbon disulfide, carbon tetrachloride, chloroform, epichlorohydrin, alkylamine, dialkylamine, alkyl halide, alkyl ether, alkyl acetate, alkyl halide, alkenyl chloride, toluene or xylene.
9. The method of claim 7, wherein the azeotrope comprises acetone and one or more solvents comprising ethanol, methanol, isopropanol, tert-butanol, hexane, 2-methylpentane, methylene chloride, trichlorotrifluoroethane, nitromethane, cyclopentane, cyclohexane, carbon disulfide, carbon tetrachloride, chloroform, methyl iodide, ethyl iodide, isopropyl ether, methyl acetate or trifluoroacetic acid.
10. The method according to any one of claims 1 to 9, further comprising mixing the powder with a desiccant.
11. The method of claim 10, wherein the desiccant comprises silica, a silicate, a borosilicate, an aluminosilicate, a zeolite, sodium sulfide, or any combination thereof.
12. The method according to any one of claims 1 to 11, wherein the catalyst comprises a metal oxide, a metal sulfide, a metal chalcogenide, a metal phosphide, a metal arsenide, a non-metallic semiconductor, a polymer semiconductor, a photosensitive isopolyanion, a photosensitive heteropolyion, or a combination thereof.
13. The method according to claim 12, wherein the metal oxide comprises titanium dioxide, zinc oxide, tungsten trioxide, ruthenium dioxide, iridium dioxide, tin dioxide, strontium titanate, barium titanate, tantalum oxide, calcium titanate, iron (III) oxide, molybdenum trioxide, niobium pentoxide, indium trioxide, cadmium oxide, hafnium oxide, zirconium oxide, manganese dioxide, copper oxide, vanadium pentoxide, chromium trioxide, yttrium trioxide, silver oxide or Ti x Zr 1-x O2, wherein x is between 0 and 1; the metal sulfide comprises cadmium sulfide, zinc sulfide, indium sulfide, copper sulfide, tungsten disulfide, bismuth trisulfide or cadmium zinc disulfide; the metal chalcogenide comprises zinc selenide, cadmium selenide, indium selenide, tungsten selenide or cadmium telluride; the metal phosphide comprises indium phosphide; the metal arsenide comprises gallium arsenide; the non-metallic semiconductor comprises silicon, silicon carbide, diamond, germanium, germanium dioxide or germanium telluride; the polymer semiconductor comprises polyacetylene; the photosensitive isopolyanion comprises W 10 O 32 -4 ; and the photosensitive heteropoly ions include XM 12 O 40 -n or X2M 18 O 62 -7 , wherein x is Bi, Si, Ge, P or As, M is Mo or W, and n is an integer from 1 to 12.
14. The method of claim 13, wherein the metal oxide comprises titanium dioxide.
15. The method of claim 14, wherein the titanium dioxide comprises rutile titanium dioxide.
16. The method of any one of claims 1 to 15, wherein the powder comprises from about 50% to about 99.99% by weight of the photoactivated catalyst and from about 0.01% to about 50% by weight of sodium chlorite.
17. The method of any one of claims 1 to 15, wherein the powder comprises from about 70% to about 97% by weight of the photoactivated catalyst and from about 3% to about 30% by weight of sodium chlorite.
18. The method of any one of claims 1 to 15, wherein the powder comprises from about 80% to about 95% by weight of the photoactivated catalyst and from about 5% to about 20% by weight of sodium chlorite.
19. The method of any one of claims 1 to 18, wherein the disinfecting effective amount is in the range of about 0.08 ppm / minute to about 8.0 ppm / minute for a period of about 2 hours to about 72 hours.
20. The method of any one of claims 1 to 19, wherein the powder is capable of generating a controlled release of the chlorine dioxide from the solid state of the powder without exposing the powder to moisture, relative humidity, or acid prior to or during exposure of the powder to visible light.
21. The process according to any one of claims 1 to 20, wherein the mixing and / or spray drying steps are performed under an inert atmosphere.
22. A light activated powder capable of generating a disinfecting effective amount of chlorine dioxide controlled release from the solid state of the powder when exposed to visible light without releasing detectable amounts of chlorine gas, chlorate and / or chlorite, said powder being prepared by the method of any one of claims 1 to 21.
23. A film comprising the photoactivated powder according to claim 22 and a biodegradable polymer.