Component made of cmc material having thermally mechanically adaptable
By forming a pre-existing environmental barrier layer of the thermally mechanical adaptable crack network on the surface of the CMC material, the problem of uncontrolled cracking and peeling of CMC materials in high temperature environments is solved, and more stable anti-oxidation and corrosion protection is achieved, and the use is extended. life.
Patent Information
- Application Number
- CN202380034901.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-25
- Filing Date
- 2023-03-23
- Publication Date
- 2024-12-06
AI Technical Summary
Existing CMC materials have uncontrolled cracking problems in high-temperature oxidation and corrosion environments, resulting in instability and peeling of the protective silica layer, affecting its service life.
The pre-existing thermomechanical adaptation to the environmental barrier layer of the crack network is adopted to adapt to the thermomechanical stress by controlling the distance and depth of the cracks, preventing uncontrolled cracking of the barrier, and controlling the growth and peeling of the protective silica layer.
Effectively improve the stability and service life of CMC materials in high temperature environments, dissipate energy through the pre-existing crack network, prevent uncontrolled cracking, maintain internal areas sealing, and provide optimal anti-oxidation and corrosion protection.
Smart Images

Figure CN119095811A_ABST
Abstract
Description
Technical Field
[0001] One particular field of application of the invention is the protection of composite materials having a matrix at least partially made of ceramic (“CMC material”) forming hot parts of gas turbines for aircraft engines or industrial turbines, such as combustion chamber walls, turbine rings, turbine nozzles or turbine blades. Background Art
[0002] Increasing efficiency and reducing pollutant emissions require consideration of ever-higher temperatures in gas turbines.
[0003] Therefore, it has been proposed to replace metal materials with CMC materials, in particular for combustion chamber walls or turbine rings. In fact, it is known that CMC materials have both good mechanical properties that allow them to be used in structural elements and the ability to maintain these properties at high temperatures. CMC materials require less cooling due to their improved resistance to high temperatures. Since this cooling is traditionally a result of extraction in the compressor, which affects the efficiency of the turbine equipment, CMC materials improve engine efficiency, which reduces fuel consumption. In addition, their use helps to optimize the performance of the turbine equipment, in particular by reducing the total mass of the turbine equipment, which further helps to reduce fuel consumption and thus significantly reduce polluting emissions.
[0004] CMC materials may include a fiber reinforcement made of refractory fibers, typically carbon fibers or ceramic fibers, densified by a ceramic matrix, for example made of silicon carbide.
[0005] Under the operating conditions of aircraft turbines, i.e. at high temperatures, in an oxidizing and humid environment, CMC materials are very sensitive to corrosion phenomena. The corrosion of CMC is caused by the oxidation of silicon carbide to silicon dioxide, which volatilizes in the form of silicon hydroxide Si(OH)4 in the presence of water vapor. Corrosion causes the CMC to deteriorate and affects its service life. In order to limit this degradation in operation, it has been considered to form an environmental barrier coating (EBC) on the surface of the CMC material. The environmental barrier can include a silicon bonding coating and a rare earth silicate layer located on the bonding coating. The bonding coating can, on the one hand, improve the adhesion of the rare earth silicate layer and, on the other hand, form a protective silicon dioxide layer, the low oxygen permeability of which helps to protect the CMC from oxidation. The rare earth silicate layer limits the diffusion of water vapor into the silicon dioxide layer formed by the oxidation of silicon and thus limits its degradation.
[0006] However, it remains desirable to further improve the protection of CMC materials in oxidative and corrosive environments at high temperatures, particularly at or above 800°C. Summary of the invention
[0007] The invention relates to a coated component intended to be installed in a turbine device, comprising:
[0008] - a substrate of a composite material having a matrix at least partly made of ceramic, and
[0009] - An environmental barrier on the substrate, comprising: (i) a silicon-containing bonding coating present on the surface of the substrate; and (ii) an environmental barrier layer covering the bonding coating, the environmental barrier layer comprising an inner region that is not cracked and is located on the side of the bonding coating and an outer region opposite to the bonding coating and covering the inner region, wherein the inner region has an environmental barrier against oxidation and corrosive substances, and the outer region has a network of thermomechanically adapted cracks, the distance between adjacent cracks is comprised between 10 μm and 50 μm, and the depth of crack extension is comprised between 50% and 95% of the thickness of the environmental barrier layer.
[0010] The inventors have discovered that prior art environmental barriers may experience uncontrolled cracking during operation due to the fact that the barriers are initially in a state of compression when manufactured. When subjected to the high temperatures encountered in operation, this compressive stress relaxes by creep and then causes cracking during cooling due to the return to a tensile field. This cracking can reach the bond coat, which causes uncontrolled growth of the protective silica layer, which in turn causes the environmental barrier layer to peel off by increasing local stresses at the interface between the bond coat and the environmental barrier layer. Notably, the inventors have discovered that the use of an environmental barrier that is pre-cracked in a controlled manner (with a controlled distance between adjacent cracks and with a controlled crack depth) prior to first use can advantageously accommodate the thermomechanical stresses in operation. The thermomechanically adapted crack network prevents uncontrolled cracking of the barrier by dissipating energy through the pre-existing crack network while maintaining a crack-free internal area, thereby providing the desired seal against oxidative and corrosive substances so as to control the growth of the protective silica layer and avoid peeling.
[0011] In one embodiment, the distance between adjacent cracks of the thermomechanically adapted crack network is comprised between 15 μm and 30 μm.
[0012] Such properties help to further improve the adaptation to thermomechanical stresses during operation.
[0013] In an exemplary embodiment, the crack extension depth of the thermomechanically adapted crack network is comprised between 75% and 90% of the thickness of the environmental barrier layer.
[0014] Such properties help to further improve the adaptability to thermomechanical stresses in operation while giving the inner area an optimal sealing against oxidation and corrosive substances.
[0015] In an exemplary embodiment, the environmental barrier layer comprises at least one rare earth silicate, in particular, the environmental barrier layer may comprise yttrium disilicate, ytterbium disilicate or a mixture of these two compounds. According to a variant, the environmental barrier layer comprises mullite.
[0016] In an exemplary embodiment, the component further comprises an additional coating on the outer region of the environmental barrier layer, the additional coating being a thermal barrier with a thickness greater than or equal to 100 μm, or a protective layer against calcium and magnesium aluminum silicates with a thickness greater than or equal to 50 μm.
[0017] Such properties advantageously enable further functionalization of the protective coating and thereby improve the protection imparted.
[0018] In one exemplary embodiment, the inner region and the outer region of the environmental barrier are made of the same material.
[0019] Such a property advantageously optimizes the thermomechanical compatibility between the two regions and thereby optimizes the control of the pre-cracking of the environmental barrier.
[0020] In particular, the inner and outer regions of the environmental barrier layer may be yttrium disilicate, ytterbium disilicate or a mixture of these two compounds. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 An example of a coated component according to the invention is shown schematically and partially.
[0022] Figure 2 Schematically and partially shown Figure 1 Precursor deposition of an environmental barrier layer of a component.
[0023] Figure 3 Schematic and partial view of the cracking heat treatment in Figure 2 on the precursor sediments.
[0024] Figure 4 is an image of one example of an environmental barrier layer useful in the context of the present invention obtained after a cracking process of a precursor deposit. DETAILED DESCRIPTION
[0025] Figure 1An example of a component 1 is shown, which includes a CMC material 3 and is provided with an environmental barrier 12. The CMC material 3 may include a fiber reinforcement, which may be carbon (C) fibers or ceramic fibers, for example silicon carbide (SiC) fibers or essentially formed of SiC, including Si-CO or Si-CON fibers, i.e. also containing oxygen and possibly nitrogen. Such fibers are produced by NGS under the name "Nicalon" or "Hi-Nicalon" or "Hi-Nicalon Type-S", or by UBE Industries under the name "Tyranno ZMI". The ceramic fibers may be coated with a thin intermediate phase layer of pyrolytic carbon (PyC), boron nitride (BN) or boron-doped carbon (BC, containing 5% to 20% B, the remainder being C). The fiber reinforcement is densified by at least part of a ceramic matrix, for example mainly ceramic by volume. The ceramic matrix may include silicon carbide or a ternary Si-BC system. The matrix may be formed at least partly of CVI in a manner known per se. Alternatively, the matrix can be formed at least partially by liquid means (impregnation with a matrix precursor resin and conversion by crosslinking and pyrolysis, the process being repeatable) or by infiltration of silicon in a molten state (melt infiltration method). In the latter case, a powder is introduced into an optionally partially densified fiber reinforcement, which powder can be a carbon powder, a ceramic powder (e.g., silicon carbide) or a mixture of these powders, and then infiltrates a silicon-based metal composition in a molten state to form a SiC-Si type matrix. The fiber reinforcement can be woven or not; when the fiber reinforcement is in the form of short fibers dispersed in the material 3, it does not exceed the scope of the present invention. Alternatively, a particle reinforcement in the form of particles dispersed in the material 3 can be used.
[0026] The environmental barrier 12 can be formed on the entire outer surface S of the CMC material 3, or only on a portion of this surface S, for example when only a certain portion of the surface S needs to be protected. The environmental barrier 12 comprises an adhesive coating 5 and an environmental barrier layer 7 covering the adhesive coating 5. In the example shown, the adhesive coating 5 is in contact with the surface S of the composite material 3. Furthermore, in this example, the layer 7 is in contact with the adhesive coating 5. In operation, the adhesive coating 5 can form a silicon dioxide layer that prevents oxidation, a so-called thermally grown oxide (TGO) layer, in a manner known per se. The adhesive coating 5 can be made of silicon.
[0027] The layer 7 provides oxidation and corrosion protection at high temperatures, in particular by limiting the diffusion of water vapor and oxygen to the bond coat 5 and the CMC material 3. The layer 7 may comprise a rare earth silicate, for example a rare earth monosilicate and / or a rare earth disilicate. The layer 7 may comprise at least one rare earth element selected from yttrium Y, scandium Sc and lanthanides. In particular, the rare earth element may be selected from yttrium Y and ytterbium Yb. It should be noted that it would not go beyond the scope of the invention if the layer 7 comprised several rare earth elements, for example yttrium and ytterbium.
[0028] Figure 1An environmental barrier layer 7 is shown, which includes an inner region 73 without cracks and located on the side of the bonding coating 5. The inner region 73 provides a seal against oxidation and corrosive substances. The region 73 can be located at a position in contact with the bonding coating 5. The layer 7 also includes an outer region 71 arranged opposite the bonding coating 5 and having a network of cracks 75 for thermomechanical adaptation. The region 73 and the region 71 can be made of the same material, such as yttrium disilicate, ytterbium disilicate or a mixture of these two compounds. The details of the formation of the environmental barrier 12 will be described below. The outer region 71 covers the inner region 73. The cracks 75 extend over the entire thickness of the region 71 to the region 73 without cracks. The network of cracks 75 can extend over the entire area of the region 71. The controlled distance d between adjacent cracks of the network of cracks 75 is contained between 10μm and 50μm, preferably between 15μm and 30μm. In particular, the average distance between adjacent cracks 75 is comprised between 10 μm and 50 μm, preferably between 15 μm and 30 μm. In general, the distance d between adjacent cracks may be regular on the layer 7 and correspond to the cracking increment. Alternatively, for all cracks 75, this distance d may vary between different pairs of adjacent cracks while still being comprised between 10 μm and 50 μm, preferably between 15 μm and 30 μm. According to an example, the set of distances d between adjacent cracks may be comprised between m / 2 and 2m, where m represents the average distance between adjacent cracks 75. Each crack 75 may extend over a depth p75 between 50% and 95%, preferably between 75% and 90%, of the thickness e7 of the environmental barrier layer 7. The cracks 75 do not reach the bonding coating 5, and thus the inner sealing area 73 may be maintained in order to control the growth of the protective silica layer in operation and prevent chipping. The thickness e7 of layer 7 may be greater than or equal to 50 μm, for example, greater than or equal to 200 μm, for example greater than or equal to 250 μm. The thickness e7 may be comprised between 50 μm and 1000 μm, for example between 200 μm and 1000 μm or between 250 μm and 1000 μm, for example between 200 μm and 700 μm or between 250 μm and 700 μm. In general, the thickness e73 of the inner sealing area 73 may be comprised between 1 μm and 10 μm, for example between 2 μm and 5 μm. If desired, an additional thermal barrier or CMAS protective coating may be deposited on the area 71 in a manner known per se, or the area 71 may define the outer surface of the coated component 1.
[0029] Details relating to the manufacture of the coatings on the CMC material 3 , and in particular to the formation of the bond coating 5 and the environmental barrier layer 7 , will now be described.
[0030] The adhesion coating 5 may be formed by chemical vapor deposition from a precursor containing silicon (including, for example, silane, monochlorosilane, dichlorosilane and / or trichlorosilane). Two examples of forming the adhesion coating 5 by chemical vapor deposition are described below.
[0031] According to a first example, the temperature applied during the deposition of the bonding coating 5 may be comprised between 900° C. and 1150° C., for example between 1100° C. and 1150° C., and the pressure applied during the deposition may be comprised between 15.3 kPa and 20 kPa, for example between 16.7 kPa and 18 kPa. During the deposition, a precursor containing silicon may be introduced into the reaction chamber where the CMC material 3 is located at a flow rate between 0.05 g / min and 0.3 g / min, for example between 0.1 g / min and 0.2 g / min. According to this first example, the obtained bonding coating 5 has a crystalline microstructure. In particular, the bonding coating 5 may be made of silicon, the bonding coating 5 comprising, for example, columnar grains of crystalline silicon. Alternatively, the bonding coating 5 may be made of a silicon alloy, for example a eutectic silicon alloy or a silicide.
[0032] According to a second example, the bonding coating 5 comprises an amorphous silicon phase, inside which crystalline silicon grains are distributed, and the average size of these grains may be comprised between 0.03 μm and 3 μm. The amorphous silicon phase may be formed of pure silicon or silicon in which boron, oxygen and / or nitrogen are distributed. According to this second example, the bonding coating 5 may be formed at a deposition temperature that prevents crystallization of the deposited silicon, and then the bonding coating is heat treated at a treatment temperature higher than the temperature applied during deposition, so as to form crystalline silicon grains distributed in the amorphous silicon phase. The temperature applied during deposition may be comprised between 300° C. and 700° C. or between 700° C. and 1000° C., and the pressure applied during deposition may be comprised between 1.2 kPa and 1013 hPa. The operating conditions are selected according to the precursor used. The treatment temperature may be comprised between 1000° C. and 1400° C., for example between 1200° C. and 1350° C. During deposition, a precursor comprising silicon may be introduced into the reaction chamber where the CMC material 3 is located at a flow rate of 0.1 g / min to 2 g / min. Those skilled in the art will recognize that the bond coating 5 may be formed by other techniques.
[0033] Generally speaking, the environmental barrier layer 7 can be formed by implementing the following steps:
[0034] (a) depositing a precursor layer by metal organic chemical vapor deposition (MOCVD), optionally by direct liquid injection metal organic chemical vapor deposition (DLI-MOCVD), and then
[0035] (b) cracking the precursor layer deposited in step (a) by subjecting it to a temperature comprised between 1250° C. and 1350° C. for a time comprised between 5 hours and 50 hours, such as between 10 hours and 50 hours.
[0036] According to one example, the deposition of the precursor layer performed during step (a) may include at least one rare earth silicate and be formed by at least an alkoxysilane silicon oxide precursor and a rare earth β-diketonate rare earth oxide precursor in the presence of an oxygen supply gas source. In particular, the silicon oxide precursor may be di-tert-butoxydiacetoxysilane and a rare earth oxide precursor RE(thd)3, wherein RE represents a rare earth element and the (thd) group represents 2,2,6,6-tetramethyl-3,5-heptanedioate, and the rare earth oxide precursor is, for example, Y(thd)3 (CAS No.15632-39-0). The oxygen supply gas source may contain at least one of the following gases: O2, N2O, H2O, CO2, O3. The temperature applied during step (a) may be included between 1000°C and 1250°C. The cracking treatment of step (b) may be performed in an oxidizing atmosphere, for example, in air.
[0037] Figure 2 and Figure 3 The deposits obtained after steps (a) and (b) are schematically shown respectively. After step (a), the deposit 700 has a microstructure of growth cones, wherein the growth cones have a first portion 701 formed by first continuous growth cones having a first average size and located on the bonding coating 5 side, and a second portion 702 formed by second growth cones having a second average size larger than the first average size and less dense than the first growth cones. According to one example, the deposit 700 of yttrium disilicate α phase can be obtained during step (a). During step (b), the deposit 700 is obtained. Figure 3 The structure shown, wherein the junction of the growth cone 702 is preferentially cracked while the sealing of the coating at the junction with the bonding coating 5 is ensured by the presence of the crack-free inner region 73 obtained from the cone 701. The heat treatment of step (b) can cause sintering of the coating, which leads to the agglomeration of the growth cones 701, which are smaller in size but more numerous in the region close to the junction with the bonding coating 5, thus resulting in the formation of the sealed region 73. The heat treatment of step (b) can also cause volume shrinkage - for example due to the transformation between the α phase and the β phase of yttrium disilicate in the case used, which leads to preferential cracking at the junction of the growth cones 702.
[0038] The component 1 thus manufactured may be a component for aviation or aerospace applications. The component 1 may be a hot component of an industrial turbine or a gas turbine of an aviation or aerospace engine. The component 1 may be a turbine equipment component. The component 1 may constitute at least a portion of a distributor, at least a portion of a nozzle or a thermal protection coating, a wall of a combustion chamber, a turbine ring sector or a turbine equipment blade.
[0039] Once obtained, component 1 is mounted and assembled to other components of a turbine installation in order to be used in oxidizing and corrosive environments at high temperatures (greater than or equal to 800° C.). In particular, it can be used at temperatures comprised between 800° C. and 1500° C. or between 800° C. and 1300° C. Component 1 can in particular be used in humid air.
[0040] Example
[0041] The precursor deposition was carried out from a solution of di-tert-butoxydiacetoxysilane (DADBS) and yttrium tris(2,2,6,6-tetramethyl-3,5-heptanedione) (Y(thd)3) diluted in toluene in a reactor with hot walls for chemical vapor deposition of organometallic compounds by direct liquid injection (DLI-MOCVD). The precursors were injected and vaporized using a thermostatically controlled direct liquid injection system sold under the name Vapbox 300 by the company KEMSTREAM, using an automotive engine type injector to form an aerosol. After preparation, the precursor deposit was heat treated at 1350°C in air for 5 hours. During this heat treatment, the deposit transforms from the alpha phase in the precursor deposit to the beta phase, resulting in regular microcracking in the upper part of the coating.
[0042] Details of the growth conditions are provided below:
[0043] -Deposition temperature: 1030℃,
[0044] -Deposition pressure: 5 mbar,
[0045] -DADBS concentration: 0.1 mol / L,
[0046] -Y(thd)3 concentration: 0.15mol / L,
[0047] - Precursor solution flow rate: 0.1 g / min,
[0048] -O2 flow rate: 54 standard cubic centimeters per minute (sccm),
[0049] -N2 flow rate: 200 standard cubic centimeters per minute,
[0050] - Injector frequency: 2Hz,
[0051] -Precursor evaporation temperature: 210℃.
[0052] The deposits obtained after cracking heat treatment are as follows Figure 4 shown.
[0053] The obtained coating passed the 1500 hours of corrosion test without degradation. During the corrosion test, the bond with the bond coating did not change. This result confirms that the small thickness of the sealing part of the environmental barrier is sufficient to ensure chipping resistance. In addition, the pre-cracking network is largely reproducible.
[0054] More generally, the following range of conditions can be used to deposit the precursor layer:
[0055] -Deposition temperature: 1000℃ to 1250℃,
[0056] -Deposition pressure: 5 mbar,
[0057] -DADBS concentration: 0.01mol / L to 0.1mol / L,
[0058] -Y(thd)3 concentration: 0.015mol / L to 0.15mol / L,
[0059] - Precursor solution flow rate: 0.1 g / min to 2 g / min,
[0060] -O2 flow rate: 25 to 200 standard cubic centimeters per minute,
[0061] -N2 flow rate: 100 to 400 standard cubic centimeters per minute,
[0062] - Injector frequency: 0.5Hz to 3Hz,
[0063] - Precursor evaporation temperature: 170°C to 250°C,
[0064] - Also applicable to reactors with cold wall construction.
[0065] The expression "comprising between ... and ..." should be understood as including the boundary values.
Claims
1. A coated component (1) for installation in a turbine device, comprising: - a substrate (3) of a composite material having an at least partially ceramic matrix, and - An environmental barrier (12) on the substrate, comprising: (i) a silicon-containing bonding coating (5) present on the surface of the substrate, and (ii) an environmental barrier layer (7) covering the bonding coating, the environmental barrier layer comprising an inner region (73) that is uncracked and located on the side of the bonding coating and provides a barrier to oxidizing and corrosive substances, and an outer region (71) arranged opposite to the bonding coating and covering the inner region, the outer region (71) having a network of thermomechanically adapted cracks (75), the distance (d) between adjacent cracks being comprised between 10 μm and 50 μm, and the depth (p75) to which the cracks extend being comprised between 50% and 95% of the thickness (e7) of the environmental barrier layer.
2. The component (1) according to claim 1, wherein The distance (d) between adjacent cracks (75) of the network of thermomechanically adapted cracks is comprised between 15 μm and 30 μm.
3. A component (1) according to claim 1 or 2, wherein: The cracks (75) of the network of thermomechanically adapted cracks extend to a depth (p75) of protection between 75% and 90% of the thickness (e7) of the environmental barrier layer.
4. A component (1) according to any one of claims 1 to 3, wherein: The environmental barrier layer (7) comprises at least one rare earth silicate.
5. The component (1) according to claim 4, wherein The environmental barrier layer (7) comprises yttrium disilicate, ytterbium disilicate or a mixture of these two compounds.
6. A component according to any one of claims 1 to 5, wherein The component also comprises an additional coating on the outer area of the environmental barrier layer, the additional coating being a thermal barrier with a thickness greater than or equal to 100 μm, or a protective layer against calcium and magnesium aluminum silicates with a thickness greater than or equal to 50 μm.
7. A component according to any one of claims 1 to 6, wherein The inner region (73) and the outer region (71) of the environmental barrier layer (7) are made of the same material.
8. The component according to claim 7, wherein The inner region (73) and the outer region (71) of the environmental barrier layer (7) are yttrium disilicate, ytterbium disilicate or a mixture of these two compounds.