Aqueous resin dispersion, aqueous coating material, and article coated with aqueous coating material

The aqueous resin dispersion, formed by radical polymerization of a specific (meth)acrylate in resin particles, addresses the limitations of existing water-based coatings by providing a film with superior performance in appearance, hardness, adhesion, alcohol resistance, and solvent resistance, suitable for automotive and household applications.

CN119095924APending Publication Date: 2024-12-06DIC CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202280095469.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2022-08-30
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Existing water-based coatings for automotive interiors face challenges in achieving high performance in terms of appearance, adhesion, alcohol resistance, hot water resistance, and solvent resistance, while solvent-based coatings remain the mainstream due to the limitations of two-component curing systems.

Method used

An aqueous resin dispersion is obtained through the radical polymerization of a specific (meth)acrylate in resin particles dispersed in an aqueous medium, formed by reacting an acrylic polymer with hydroxyl and carboxyl groups and a polyurethane (meth)acrylate having an isocyanate group, which is then neutralized and dispersed in an aqueous medium.

Benefits of technology

The resulting coating film exhibits excellent appearance, hardness, adhesion, alcohol resistance, hot water resistance, and solvent resistance, making it suitable for various applications including automotive interiors and household appliances.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005105359350000141
    Figure BDA0005105359350000141
Patent Text Reader

Abstract

Provided is an aqueous resin dispersion obtained by radical polymerization of a (meth) acrylate (X) dispersed in resin particles in an aqueous medium, wherein the (meth) acrylate (X) is a product of a reaction of an acrylic polymer (A) having a hydroxyl group and a carboxyl group and a polyurethane (meth) acrylate (B) having an isocyanate group. The aqueous resin dispersion can be used in an aqueous coating material because it provides a cured coating film having excellent appearance, hardness, adhesion, alcohol resistance, hot water resistance, and solvent resistance, and the aqueous coating material can be applied to a variety of articles.
Need to check novelty before this filing date? Find Prior Art

Description

Field of the Invention

[0001] The invention relates to an aqueous resin dispersion, an aqueous coating and a product coated with the aqueous coating. Background of the Invention

[0003] Under the background of VOC regulation, the use of water-based coatings is advancing in various applications. However, due to the high performance requirements for coating film appearance, adhesion and chemical resistance, automotive interior coatings face high barriers to water-based coatings, while solvent-based coatings are the mainstream.

[0004] Under such circumstances, an aqueous resin dispersion obtained by copolymerizing a urethane acrylate oligomer and another acrylic monomer has been proposed (see, for example, Patent Document 1). However, this material has problems such as workability because it is a two-component curing type using an amino resin as a curing agent.

[0005] Therefore, there is a need for a one-component water-based material that provides a cured coating film having excellent physical properties such as appearance, hardness, adhesion, alcohol resistance, hot water resistance, and solvent resistance.

[0006] Citations

[0007] Patent Literature

[0008] PTL 1: CN105601832B SUMMARY OF THE INVENTION

[0010] Technical issues

[0011] The problem to be solved by the present invention is to provide an aqueous resin dispersion which provides a cured coating film having excellent appearance, hardness, adhesion, alcohol resistance, hot water resistance and solvent resistance, an aqueous coating containing the aqueous dispersion, and an article coated with the coating.

[0012] Solutions to the problem

[0013] The inventors of the present invention have conducted intensive studies to solve the above problems. As a result, the inventors have found that obtaining an aqueous resin dispersion by radical polymerization of a specific (meth)acrylate in resin particles dispersed in an aqueous medium can solve the above problems, and have completed the present invention.

[0014] That is, the present invention relates to: an aqueous resin dispersion obtained by free radical polymerization of (meth)acrylate (X) in resin particles dispersed in an aqueous medium, wherein the (meth)acrylate (X) is a reaction product of an acrylic polymer (A) having hydroxyl and carboxyl groups and a polyurethane (meth)acrylate (B) having an isocyanate group; an aqueous coating containing the aqueous dispersion; and an article coated with the aqueous coating.

[0015] Advantageous Effects of the Invention

[0016] The aqueous resin dispersion of the present invention can be used for water-based coatings because it provides a cured coating film having excellent appearance, hardness, adhesion, alcohol resistance, hot water resistance and solvent resistance, and the aqueous coating can be applied to a variety of products. Therefore, the aqueous resin dispersion of the present invention can be appropriately used as an aqueous coating to coat products, such as the main bodies of household appliances such as refrigerators, televisions and air conditioners, the housings of information terminals such as mobile phones, smart phones and personal computers, automotive interior parts, cosmetic containers and highly designed packaging materials.

[0017] Implementation plan description

[0018] The aqueous resin dispersion of the present invention is an aqueous resin dispersion obtained by free radical polymerization of (meth)acrylate (X) in resin particles dispersed in an aqueous medium, wherein the (meth)acrylate (X) is a reaction product of an acrylic polymer (A) having a hydroxyl group and a carboxyl group and a polyurethane (meth)acrylate (B) having an isocyanate group.

[0019] First, the acrylic polymer (A) will be described. The acrylic polymer (A) is obtained by copolymerizing an unsaturated monomer (a1) having a hydroxyl group, an unsaturated monomer (a2) having a carboxyl group, and another unsaturated monomer (a3).

[0020] Examples of unsaturated monomers (a1) having a hydroxyl group include 2-hydroxyethyl (meth) acrylate, 3-hydroxypropyl (meth) acrylate, 4-hydroxy-n-butyl (meth) acrylate, 2-hydroxypropyl (meth) acrylate, 2-hydroxy-n-butyl (meth) acrylate, 3-hydroxy-n-butyl (meth) acrylate, 1,4-cyclohexanedimethanol mono (meth) acrylate, N-(2-hydroxyethyl) (meth) acrylamide, glycerol mono (meth) acrylate, polyethylene glycol mono (meth) acrylate, polypropylene glycol mono (meth) acrylate, 2-hydroxy-3-phenoxypropyl (meth) acrylate, 2-(meth) acryloyloxyethyl-2-hydroxyethyl phthalate, and lactone-modified (meth) acrylates having a terminal hydroxyl group. These unsaturated monomers (a1) can be used alone or in combination of two or more.

[0021] Examples of the unsaturated monomer (a2) having a carboxyl group include unsaturated monocarboxylic acids such as (meth) acrylic acid, crotonic acid, β-carboxyethyl (meth) acrylate, ω-carboxy-polycaprolactone mono(meth) acrylate, 2-(meth) acryloyloxyethyl succinate and 2-(meth) acryloyloxyethyl hexahydrophthalic acid; unsaturated dicarboxylic acids such as maleic acid, fumaric acid and itaconic acid, and half esters of these unsaturated dicarboxylic acids. Among them, (meth) acrylic acid is preferred because of its excellent dispersibility in water. These unsaturated monomers (a2) can be used alone or in combination of two or more.

[0022] In addition, examples of the unsaturated monomer (a3) ​​include aromatic vinyl monomers such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, n-heptyl (meth)acrylate, n-octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, dodecyl (meth)acrylate, hexadecyl (meth)acrylate, stearyl (meth)acrylate, behenyl (meth)acrylate, cyclohexyl (meth)acrylate , 4-tert-butylcyclohexyl(meth)acrylate, isobornyl(meth)acrylate, dicyclopentyl(meth)acrylate, benzyl(meth)acrylate, methoxypolyethylene glycol(meth)acrylate, ethoxypolyethylene glycol(meth)acrylate, phenoxypolyethylene glycol(meth)acrylate, (meth)acrylamide, N,N-dimethyl(meth)acrylamide, diacetone(meth)acrylamide, (meth)acrylonitrile, 3-(meth)acryloylpropyltrimethoxysilane, N,N-dimethylaminoethyl(meth)acrylate, glycidyl(meth)acrylate, styrene, α-methylstyrene, p-methylstyrene and p-methoxystyrene. Among them, from the perspective of water dispersibility, (meth)acrylates having ethylene oxide chains such as methoxypolyethylene glycol(meth)acrylate and ethoxypolyethylene glycol(meth)acrylate are preferred, and (meth)acrylic compounds having carbonyl groups such as diacetone(meth)acrylamide are preferred because they can form crosslinks with dihydrazine compounds. These unsaturated monomers (a3) ​​may be used alone or in combination of two or more.

[0023] The amount of the acrylic monomer (a1) in the monomer component as a raw material of the acrylic polymer (A) is preferably 3 to 50% by mass, more preferably 5 to 30% by mass, from the viewpoint of the reaction point with the urethane acrylate (B).

[0024] From the viewpoint of water dispersibility, the amount of the acrylic monomer (a2) in the monomer component as a raw material of the acrylic polymer (A) is preferably 1 to 20% by mass, more preferably 3 to 10% by mass.

[0025] The amount of the acrylic monomer (a3) ​​used is the remainder obtained by subtracting the proportions of the unsaturated monomers (a1) and (a2) used from the total 100 mass % of the monomer components as the raw material of the acrylic polymer (A).

[0026] Examples of the method for producing the acrylic polymer (A) include a method of copolymerizing an acrylic acid monomer (a1) and an unsaturated monomer (a2) in an organic solvent using a polymerization initiator. The organic solvent used herein is preferably an alcohol compound, a ketone compound, an ester compound, an ether compound, an amide compound, a sulfoxide compound, or a hydrocarbon compound, and specific examples thereof include methanol, ethanol, propanol, n-butanol, isobutanol, tert-butanol, 3-methoxybutanol, acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, ethyl acetate, butyl acetate, propylene glycol monomethyl ether acetate, diisopropyl ether, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dibutyl ether, propylene glycol monomethyl ether, propylene glycol monopropyl ether, propylene glycol monobutyl ether, propylene glycol dimethyl ether, dipropylene glycol monomethyl ether, dipropylene glycol dimethyl ether, dimethylformamide, dimethylacetamide, N-methylpyrrolidone, dimethyl sulfoxide, tetrahydrofuran, dioxane, toluene and xylene. Among them, dialkyl glycol dialkyl ethers such as diethylene glycol dimethyl ether, diethylene glycol diethyl ether and dipropylene glycol dimethyl ether are more preferred from the viewpoint of improving the storage stability of the obtained aqueous resin dispersion.

[0027] Examples of the polymerization initiator include ketone peroxide compounds such as cyclohexanone peroxide, 3,3,5-trimethylcyclohexanone peroxide and methylcyclohexanone peroxide; peroxyketal compounds such as 1,1-di(tert-butylperoxy)-3,3,5-trimethylcyclohexane, 1,1-di(tert-butylperoxy)cyclohexane, n-butyl-4,4-di(tert-butylperoxy)valerate, 2,2-di(4,4-di-tert-butylperoxycyclohexyl)propane, 2,2-di(4,4-di-tert-amylperoxycyclohexyl)propane, 2,2-di(4,4-di-tert-hexylperoxycyclohexyl)propane, 2,2-di(4,4-di-tert-octylperoxycyclohexyl)propane and 2,2-di(4,4-diisopropylperoxycyclohexyl)propane; hydroperoxides such as cumene hydroperoxide and 2,5-dimethylbenzene hydroperoxide. dialkyl peroxide compounds such as 1,3-di(tert-butylperoxy-m-isopropyl)benzene, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, diisopropylbenzene peroxide and tert-butylisopropylbenzene peroxide; diacyl peroxide compounds such as decanoyl peroxide, lauroyl peroxide, benzoyl peroxide and 2,4-dichlorobenzoyl peroxide; peroxide carbonate compounds such as bis(tert-butylcyclohexyl)peroxydicarbonate; organic peroxides such as peroxyester compounds such as tert-butylperoxy-2-ethylhexanoate, tert-butylperoxybenzoate and 2,5-dimethyl-2,5-di(benzoylperoxy)hexane; and azo compounds such as 2,2'-azobisisobutyronitrile and 1,1'-azobis(cyclohexane-1-carbonitrile).

[0028] In addition, when producing the acrylic polymer (A), a chain transfer agent such as dodecyl mercaptan, 2-mercaptoethanol, thioglycerol, ethylthioglycolic acid and octylthioglycolic acid may be used as necessary.

[0029] The hydroxyl value of the acrylic polymer (A) is preferably from 10 to 200 mgKOH / g, more preferably from 20 to 100 mgKOH / g, from the viewpoint of the reaction point with the urethane (meth)acrylate (B).

[0030] The acid value of the acrylic polymer (A) is preferably from 10 to 150 mgKOH / g, more preferably from 20 to 80 mgKOH / g, from the viewpoint of water dispersibility.

[0031] The hydroxyl value and acid value in the present invention are values ​​calculated from the raw materials used.

[0032] From the viewpoint of further improving the water dispersibility and storage stability of the obtained aqueous resin dispersion, the weight average molecular weight (Mw) of the acrylic polymer (A) is preferably 3,000 to 200,000, more preferably 5,000 to 150,000. Here, the weight average molecular weight (Mw) is a polystyrene equivalent value measured based on gel permeation chromatography (hereinafter referred to as "GPC").

[0033] The urethane (meth)acrylate (B) having an isocyanate group has an isocyanate group and a (meth)acryloyl group.

[0034] For example, urethane (meth)acrylate (B) can be obtained by a urethane reaction between polyisocyanate (b1) and (meth)acrylate (b2) having a hydroxyl group.

[0035] Examples of polyisocyanates (b1) include aromatic diisocyanate compounds such as toluene diisocyanate, diphenylmethane diisocyanate, m-xylene diisocyanate and m-phenylene bis(dimethylmethylene) diisocyanate; and aliphatic or alicyclic diisocyanate compounds such as hexamethylene diisocyanate, lysine diisocyanate, 1,3-bis(isocyanatomethyl)cyclohexane, 2-methyl-1,3-diisocyanatocyclohexane, 2-methyl-1,5-diisocyanatocyclohexane, 4,4'-dicyclohexylmethane diisocyanate and isophorone diisocyanate. Among them, aliphatic or alicyclic diisocyanate compounds are preferred because they have excellent yellowing resistance.

[0036] In addition, for the polyisocyanate (b1), there can also be used a prepolymer having an isocyanate group obtained by subjecting the above-mentioned diisocyanate compound to an addition reaction with a polyhydric alcohol; a compound having an isocyanate ring obtained by cyclotrimerizing the above-mentioned diisocyanate compound; a polyisocyanate compound having a urea bond or a burette bond obtained by reacting the above-mentioned diisocyanate compound with water; an acrylic monomer having an isocyanate group such as homopolymers of (meth)acrylate 2-isocyanatoethyl, 3-isopropylene-α,α-dimethylbenzyl isocyanate and (meth)acryloyl isocyanate; and a copolymer having an isocyanate group obtained by copolymerizing an acrylic monomer having an isocyanate group with other monomers such as an acrylic monomer, a vinyl ester compound, a vinyl ether compound, an aromatic vinyl monomer and a fluoroolefin.

[0037] The above polyisocyanates (b1) may be used alone or in combination of two or more.

[0038] Examples of (meth)acrylates (b2) having a hydroxyl group include 2-hydroxyethyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxy-n-butyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxy-n-butyl (meth)acrylate, 3-hydroxy-n-butyl (meth)acrylate, 1,4-cyclohexanedimethanol mono(meth)acrylate, N-(2-hydroxyethyl) (meth)acrylamide, glycerol mono(meth)acrylate, polyethylene glycol mono(meth)acrylate, polypropylene glycol mono(meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, 2-(meth)acryloyloxyethyl-2-hydroxyethyl phthalate, and lactone-modified (meth)acrylates having a terminal hydroxyl group. These (meth)acrylates (b2) having a hydroxyl group may be used alone or in combination of two or more.

[0039] In the present invention, the polyurethane reaction may be carried out in the absence of a catalyst or in the presence of a polyurethane forming catalyst to promote the reaction. Examples of polyurethane forming catalysts include: amine compounds such as pyridine, pyrrole, triethylamine, diethylamine and dibutylamine; phosphine compounds such as triphenylphosphine and triethylphosphine; organic tin compounds such as dibutyltin dilaurate, octyltin trilaurate, octyltin diacetate, dibutyltin diacetate and tin octoate; and organic metal compounds such as zinc octoate.

[0040] The content of the isocyanate group in the urethane (meth)acrylate (B) is preferably 3 to 20% by mass from the viewpoint of the reaction point with the acrylic polymer (A).

[0041] The urethane (meth)acrylate (B) preferably has a weight average molecular weight of 200 to 2,000.

[0042] The (meth)acrylate (X) is obtained by a urethane reaction between an acrylic polymer (A) having a hydroxyl group and a urethane (meth)acrylate (B) having an isocyanate group.

[0043] From the viewpoint of improving the water dispersibility of the resulting aqueous resin dispersion and improving the storage stability, the mass ratio (A / B) of the acrylic polymer (A) to the polyurethane (meth)acrylate (B) is preferably in the range of 0.25 to 4, more preferably in the range of 0.5 to 3.

[0044] From the viewpoint of improving the water dispersibility of the resulting aqueous resin dispersion and improving the storage stability, the molar ratio (A / B) of the hydroxyl group of the acrylic polymer (A) to the isocyanate group of the polyurethane (meth)acrylate (B) is preferably in the range of 0.8 to 1.2, more preferably in the range of 0.9 to 1.1.

[0045] From the viewpoint of further improving water dispersibility, the acid value of the (meth)acrylate (X) is preferably from 10 to 60 mgKOH / g.

[0046] (Meth)acrylate (X) is a product of a reaction between an acrylic polymer (A) having a hydroxyl group and a urethane (meth)acrylate (B) having an isocyanate group. However, it is preferred to further use a polymer polyol (P) as a reaction raw material.

[0047] Examples of the polymer polyol (P) include polycarbonate diols, polyester diols, and polyether diols. These polymer polyols (P) may be used alone or in combination of two or more.

[0048] The number average molecular weight of the polymer polyol (P) is preferably 500 to 3,000, more preferably 500 to 2,000, from the viewpoint of water dispersibility.

[0049] From the viewpoint of further improving chemical resistance and coating film hardness, the amount of the polymer polyol (P) is preferably 5 to 20 mass %, more preferably 5 to 10 mass %, based on the raw material of the (meth)acrylate (X).

[0050] Examples of the reaction method of the acrylic polymer (A), the polyurethane (meth)acrylate (B) and the polymer polyol (P) include: a method of reacting the acrylic polymer (A), the polyurethane (meth)acrylate (B) and the polymer polyol (P) at the same time, and a method of reacting the polyisocyanate (b1) and the polymer polyol (P) when the polyurethane (meth)acrylate (B) is obtained, and then reacting the (meth)acrylate (b2) having a hydroxyl group.

[0051] Preferred examples of the method of dispersing the (meth)acrylate (X) as resin particles in an aqueous medium include a method of neutralizing the carboxyl group of the (meth)acrylate (X) with a basic compound, followed by mixing with the aqueous medium.

[0052] Examples of alkaline compounds include organic amines such as methylamine, dimethylamine, trimethylamine, ethylamine, diethylamine, triethylamine, butylamine, dibutylamine, tributylamine, N,N-dimethylethanolamine, 2-aminoethanol and other monoalkanolamines, diethanolamine, diisopropanolamine and dibutanolamine; inorganic alkaline compounds such as ammonia, sodium hydroxide and potassium hydroxide; and quaternary ammonium hydroxides such as tetramethylammonium hydroxide, tetra-n-butylammonium hydroxide and trimethylbenzylammonium hydroxide. Among them, organic amines and ammonia (ammonia water can be used) are preferably used. These alkaline compounds can be used alone or in combination of two or more.

[0053] Furthermore, from the viewpoint of further improving the storage stability of the aqueous resin dispersion, the amount of the basic compound to be used is preferably such that the neutralization rate of the carboxyl group of the (meth)acrylate (X) is within a range of 50% to 100%.

[0054] Examples of aqueous media include water, hydrophilic organic solvents, and mixtures thereof. As the hydrophilic organic solvent, a water-miscible organic solvent that is miscible with water without separation is preferred, and among these solvents, an organic solvent having a solubility in water (the number of grams of the organic solvent dissolved in 100 g of water) of 3 g or more at 25° C. is preferred. The example of these water miscible organic solvents includes: alcohol solvents, such as methanol, ethanol, propanol, butanol, 3-methoxybutanol and 3-methyl-3-methoxybutanol; Ketone solvents, such as acetone and methyl ethyl ketone; and glycol ether-based solvents, such as ethylene glycol monomethyl ether, ethylene glycol dimethyl ether, ethylene glycol monoethyl ether, ethylene glycol diethyl ether, ethylene glycol monopropyl ether, ethylene glycol monoisopropyl ether, monobutyl ether, diethylene glycol monomethyl ether, diethylene glycol dimethyl ether, diethylene glycol monoethyl ether, diethylene glycol diethyl ether, diethylene glycol monoisopropyl ether, diethylene glycol monobutyl ether, triethylene glycol monomethyl ether, triethylene glycol dimethyl ether, propylene glycol monomethyl ether, propylene glycol dimethyl ether, propylene glycol monopropyl ether, propylene glycol monobutyl ether, diethylene glycol monomethyl ether and diethylene glycol dimethyl ether. These water miscible organic solvents can be used alone, or can be used in combination of two or more.

[0055] Although the aqueous resin dispersion of the present invention is obtained by radical polymerization of (meth)acrylic acid ester (X) in resin particles dispersed in an aqueous medium, it can also be obtained by copolymerization of other (meth)acrylic monomers (Y).

[0056] As the (meth)acrylic monomer (Y), the above-mentioned unsaturated monomers (a1) to (a3) ​​as a raw material for the acrylic polymer (A) may be used.

[0057] When the (meth)acrylic acid monomer (Y) is copolymerized, it is preferred to first mix the (meth)acrylic acid ester (X) with the (meth)acrylic acid monomer (Y) and then disperse the (meth)acrylic acid ester (X) in an aqueous medium.

[0058] Furthermore, in the radical polymerization of the (meth)acrylate (X), it is preferred to use a water-soluble polymerization initiator such as ammonium persulfate, potassium persulfate, and sodium persulfate.

[0059] The aqueous resin dispersion of the present invention may contain a dihydrazine compound because it can form a higher density of crosslinking.

[0060] The water-based paint of the present invention contains the above-mentioned water-based resin dispersion. However, as other compounds, additives such as antistatic agents, defoamers, viscosity modifiers, light stabilizers, weathering stabilizers, heat stabilizers, UV absorbers, antioxidants, leveling agents and pigment dispersants can be used.

[0061] In addition, the water-based paint of the present invention can be used as a paint for coating a variety of articles, and examples of articles that can be coated with the water-based paint of the present invention include the bodies of household appliances such as refrigerators, televisions and air conditioners, housings of information terminals such as mobile phones, smartphones and personal computers, automobile interior trims, cosmetic containers and highly designed packaging materials.

[0062] Examples of methods for applying the aqueous coating of the present invention include methods using a gravure coater, a roll coater, a comma coater, a knife coater, an air knife coater, a curtain coater, a kiss coater, a shower coater, a spin coater, dipping, screen printing, spraying, an applicator, a strip coater, or a brush. In addition, examples of methods for forming a coating film after coating include methods of drying at room temperature to 120°C. Example

[0063] The present invention will be described in more detail below using specific examples. In addition, under the following GPC measurement conditions, the weight average molecular weight (Mw) of the polymer was measured.

[0064] [GPC measurement conditions]

[0065] Measuring apparatus: High-speed GPC apparatus ("HLC-8220GPC" manufactured by Tosoh Corporation) Columns: The following columns manufactured by Tosoh Corporation were connected in series and used.

[0066] "TSKgel G5000" (7.8mm ID×30cm)×1

[0067] "TSKgel G4000" (7.8mm ID×30cm)×1

[0068] "TSKgel G3000" (7.8mm ID×30cm)×1

[0069] "TSKgel G2000" (7.8mm ID×30cm)×1

[0070] Detector: RI (differential refractometer)

[0071] Column temperature: 40°C

[0072] Eluent: Tetrahydrofuran (THF)

[0073] Flow rate: 1.0mL / min

[0074] Injection volume: 100 μL (tetrahydrofuran solution, sample concentration is 4 mg / mL)

[0075] Standard samples: Use the following monodisperse polystyrene to create a calibration curve.

[0076] (monodisperse polystyrene)

[0077] "TSKgel Standard Polystyrene A-500" manufactured by Tosoh Corporation

[0078] "TSKgel Standard Polystyrene A-1000" manufactured by Tosoh Corporation

[0079] "TSKgel Standard Polystyrene A-2500" manufactured by Tosoh Corporation

[0080] "TSKgel Standard Polystyrene A-55000" manufactured by Tosoh Corporation

[0081] "TSKgel Standard Polystyrene F-1" manufactured by Tosoh Corporation

[0082] "TSKgel Standard Polystyrene F-2" manufactured by Tosoh Corporation

[0083] "TSKgel Standard Polystyrene F-4" manufactured by Tosoh Corporation

[0084] "TSKgel Standard Polystyrene F-10" manufactured by Tosoh Corporation

[0085] "TSKgel Standard Polystyrene F-20" manufactured by Tosoh Corporation

[0086] "TSKgel Standard Polystyrene F-40" manufactured by Tosoh Corporation

[0087] "TSKgel Standard Polystyrene F-80" manufactured by Tosoh Corporation

[0088] "TSKgel Standard Polystyrene F-128" manufactured by Tosoh Corporation

[0089] "TSKgel Standard Polystyrene F-288" manufactured by Tosoh Corporation

[0090] "TSKgel Standard Polystyrene F-550" manufactured by Tosoh Corporation

[0091] (Synthesis Example 1: Synthesis of acrylic polymer (A-1))

[0092] In a reactor equipped with stirring, cooling and heating devices, 283 parts by mass of diethylene glycol dimethyl ether (hereinafter referred to as "MDM") was charged, and the mixture was heated to 135° C. Then, a monomer mixture of 70 parts by mass of methyl methacrylate (hereinafter referred to as "MMA"), 160 parts by mass of n-butyl methacrylate (hereinafter referred to as "nBMA"), 70 parts by mass of 2-hydroxyethyl methacrylate (hereinafter referred to as "HEMA") and 60 parts by mass of styrene (hereinafter referred to as "St"), and a solution prepared by dissolving 20 parts by mass of tert-butyl peroxy-2-ethylhexanoate (hereinafter referred to as "PO") in 20 parts by mass of MDM were added dropwise in two lines at a constant speed over 2 hours. Then, a monomer mixture of 210 parts by mass of MMA, 73 parts by mass of n-butyl acrylate (hereinafter referred to as "nBA"), 27 parts by mass of HEMA, 40 parts by mass of St, 40 parts by mass of acrylic acid (hereinafter referred to as "AA'"), 10 parts by mass of methoxypolyethylene glycol methacrylate (number of oxyethylene repeating units: 23) and 40 parts by mass of diacetone acrylamide (hereinafter referred to as "DAAM"), and a solution prepared by dissolving 10 parts by mass of PO in 10 parts by mass of MDM were added dropwise in two lines at a constant rate over 2 hours and 30 minutes. After maintaining the temperature at 135° C. for 60 minutes, the mixture was cooled to obtain a solution of an acrylic polymer (A-1) having a carboxyl group and a hydroxyl group. The solution had a solid content of 70.0% by mass, a hydroxyl value of 52, an acid value of 39, and a weight average molecular weight of 33,000. (Synthesis Example 2: Synthesis of polyurethane (meth) acrylate (B-1))

[0093] In a reactor equipped with a stirring, cooling and heating device, 222 parts by mass of isophorone diisocyanate, 0.07 parts by mass of 4-methoxyphenol (MEHQ) and dibutyltin dilaurate were charged and stirring was started. Then, the reaction temperature was maintained at 25 to 35° C., and 139 parts by mass of HEMA were added dropwise over 2 hours. Thirty minutes after the addition was completed, the reaction temperature was raised to 40° C. and maintained until the isocyanate group content became less than 11% to obtain a polyurethane (meth) acrylate (B-1) having an isocyanate group and a (meth) acryloyl group. The isocyanate group content of the polyurethane (meth) acrylate (B-1) was 10.8%.

[0094] (Example 1: Synthesis and evaluation of aqueous resin dispersion (1))

[0095] In a reactor equipped with a stirring, cooling and heating device, 890 parts by mass of the solution of the acrylic polymer (A-1) obtained in Synthesis Example 1, 200 parts by mass of the polyurethane (meth) acrylate (B-1) obtained in Synthesis Example 2 and 0.1 parts by mass of MEHQ were charged, and the mixture was heated to 80°C. The temperature was maintained for about 3 hours until the isocyanate content became less than 0.2% to obtain (meth) acrylate (X-1). Then, the mixture was cooled to 60°C, and 80 parts by mass of MMA and 28 parts by mass of triethylamine (TEA) were added. After being maintained for about 30 minutes, 1000 parts by mass of deionized water were added and stirred to obtain an aqueous dispersion containing (meth) acrylate (X-1) and MMA in the particles. Then, the mixture was heated to 60°C, an aqueous solution prepared by dissolving 0.45 parts by mass of ammonium persulfate in 40 parts by mass of deionized water was added, and the mixture was heated to 80°C and maintained for 1 hour. Then, the mixture was cooled to 60°C, and an aqueous solution prepared by dissolving 12 parts by mass of adipic acid hydrazide (ADH) in 50 parts by mass of deionized water was added over 30 minutes, followed by cooling to obtain an aqueous resin dispersion (1). The resin solid content of the aqueous resin dispersion (1) was 40.9% by mass.

[0096] (Example 2: Synthesis and evaluation of aqueous resin dispersion (2))

[0097] In a reactor equipped with stirring, cooling and heating devices, 860 parts by mass of the solution of the acrylic polymer (A-1) obtained in Synthesis Example 1, 150 parts by mass of polycarbonate diol ("DURANOL T5651" produced by Asahi Kasei Corporation), 280 parts by mass of polyurethane (meth) acrylate (B-1) and 0.1 parts by mass of MEHQ were charged, and the mixture was heated to 80°C. The temperature was maintained for about 4 hours until the isocyanate group content became less than 0.2%, to obtain (meth) acrylate (X-2). Then, the mixture was cooled to 60°C, and 27 parts by mass of TEA were added. After maintaining for about 30 minutes, 1200 parts by mass of deionized water were added and stirred to obtain an aqueous dispersion containing (meth) acrylate (X-2) in particles. The mixture was then heated to 60°C, an aqueous solution prepared by dissolving 0.5 parts by mass of ammonium persulfate in 28 parts by mass of deionized water was added, and the mixture was heated to 80°C and maintained for 1 hour. The mixture was then cooled to 60°C, and an aqueous solution prepared by dissolving 12 parts by mass of ADH in 70 parts by mass of deionized water was added over 30 minutes, followed by cooling to obtain an aqueous resin dispersion (2). The resin solid content of the aqueous resin dispersion (2) was 41.1% by mass.

[0098] (Comparative Example 1: Synthesis and Evaluation of Aqueous Resin Dispersion (R1))

[0099] In a reactor equipped with stirring, cooling and heating devices, 283 parts by mass of MDM were charged and the mixture was heated to 135°C. Then, a monomer mixture of 70 parts by mass of MMA, 160 parts by mass of nBMA, 70 parts by mass of HEMA and 60 parts by mass of St, and a solution prepared by dissolving 20 parts by mass of PO in 20 parts by mass of MDM were added dropwise in two lines at a constant rate over 2 hours. Then, a monomer mixture of 210 parts by mass of MMA, 73 parts by mass of nBA, 27 parts by mass of HEMA, 40 parts by mass of St, 40 parts by mass of AA, 10 parts by mass of methoxypolyethylene glycol methacrylate and 40 parts by mass of DAAM, and a solution prepared by dissolving 10 parts by mass of PO in 10 parts by mass of MDM were added dropwise in two lines at a constant rate over 2 hours and 30 minutes. After maintaining the temperature at 135°C for 60 minutes, the mixture was cooled to 60°C and 36 parts by mass of TEA were added. After holding for about 30 minutes, 810 parts by mass of deionized water was added under stirring to obtain an aqueous dispersion of an acrylic polymer having carboxyl and hydroxyl groups. The mixture was then cooled to 60°C, and an aqueous solution prepared by dissolving 16 parts by mass of ADH in 50 parts by mass of deionized water was added over 30 minutes. The mixture was cooled to obtain an aqueous resin dispersion (R1). The resin solid content in the aqueous resin dispersion (R1) was 40.0% by mass.

[0100] [Preparation of Cured Coating Film for Evaluation]

[0101] The aqueous resin dispersion obtained above was sprayed on ABS (acrylonitrile-butadiene-styrene copolymer) plates, PC (polycarbonate) plates and aluminum plates so that the film thickness after drying was 20 μm. After pre-drying at 80° C. for 30 minutes in a drying machine, the coating was cured at 25° C. for 1 week to obtain a cured coating film.

[0102] [Evaluation of coating film appearance]

[0103] The coating film appearance of the cured coating film prepared on the ABS plate was visually observed, and the coating film appearance was evaluated according to the following criteria.

[0104] A: No whitening occurs.

[0105] B: Slight whitening was observed.

[0106] C: Whitening occurs.

[0107] [Evaluation of coating film hardness]

[0108] For the cured coating film prepared on the aluminum plate, the hardness of the hardest pencil that does not produce a scar was measured as the pencil hardness using a pencil specified in JIS S 6006:2007 in accordance with JIS K5600-5-4:1999.

[0109] [Evaluation of coating film adhesion]

[0110] The measurement is carried out according to the JIS K-5600 cross-cut test method. On the cured coating film prepared on the PC board, a cutter is used to cut a 1 mm wide cut so that the number of grids is 100, and a cellophane tape is applied so that it covers all the grids and quickly peeled off. The judgment is made by counting the number of remaining grids. The evaluation criteria are as follows.

[0111] A: Not peeled off.

[0112] B: The peeling area is 1% or more and less than 65% of the total mesh area.

[0113] C: The peeling area is 65% or more of the total mesh area.

[0114] [Evaluation of alcohol resistance]

[0115] After the prepared cured coating film was reciprocated and rubbed 100 times on an ABS plate with a felt soaked in ethanol at a load of 500 g, the state of the cured coating film was evaluated by finger touch and visual observation. The evaluation criteria were as follows.

[0116] A: No softening or loss of gloss was observed.

[0117] B: Slight softening or loss of gloss was observed.

[0118] C: Remarkable softening or loss of gloss was observed.

[0119] [Evaluation of hot water resistance]

[0120] After the cured coating film prepared on the ABS plate was immersed in hot water at 80° C. for 4 hours, the appearance of the cured coating film immediately after being taken out of the hot water was visually observed and evaluated according to the following evaluation criteria.

[0121] A: No whitening or bubbling

[0122] B: Whitening or foaming was observed.

[0123] C: Peeling from the substrate was observed.

[0124] [Evaluation of solvent resistance]

[0125] After the prepared cured coating film was reciprocated and rubbed 50 times on an ABS plate with a felt soaked in methyl ethyl ketone at a load of 500 g, the state of the cured coating film was evaluated by finger touch and visual observation. The evaluation criteria were as follows.

[0126] A: No softening or loss of gloss was observed.

[0127] B: Slight softening or loss of gloss was observed.

[0128] C: Remarkable softening or loss of gloss was observed.

[0129] The evaluation results of Examples 1 to 2 and Comparative Example 1 are shown in Table 1.

[0130] [Table 1]

[0131]

[0132] The results show that the coating film obtained from the aqueous resin dispersion of the present invention is excellent in appearance, hardness, adhesion, alcohol resistance, hot water resistance and solvent resistance.

[0133] It was also found that hardness, adhesion, alcohol resistance, hot water resistance, and solvent resistance were insufficient in Comparative Example 1, which was an example in which urethane (meth)acrylate (B), which was an essential raw material of the present invention, was not used.

Claims

1. An aqueous resin dispersion obtained by free radical polymerization of (meth)acrylate (X) in resin particles dispersed in an aqueous medium, wherein the (meth)acrylate (X) is a reaction product of an acrylic polymer (A) having a hydroxyl group and a carboxyl group and a polyurethane (meth)acrylate (B) having an isocyanate group. 2 . The aqueous resin dispersion according to claim 1 , wherein the polyurethane (meth)acrylate (B) is a product of a reaction of a polyisocyanate (b1) and a (meth)acrylate (b2) having a hydroxyl group. 3 . The aqueous resin dispersion according to claim 1 , wherein the radical polymerization is copolymerization of the (meth)acrylate (X) and the (meth)acrylic acid monomer (Y).

4. The aqueous resin dispersion according to claim 1, wherein the reaction product contains a polymer polyol (P) as an essential raw material. 5 . A water-based paint comprising the water-based resin dispersion according to claim 1 .

6. An article coated with the water-based coating according to claim 5.

Citation Information

Patent Citations

  • Polyurethane modified acrylic secondary dispersion and preparation method thereof

    CN105601832B

  • Radiation-curable resin composition and multilayer structure using the same

    JP2006169412A

  • Water-borne clear coating composition and method of forming clear coating film

    WO2006137569A1