Method for manufacturing semiconductor device

By using the photodevelopment technology of the photosensitive resin layer in semiconductor chip manufacturing, the fragments generated by laser processing are avoided, and the problem of laser processing residue affecting hybrid bonding is solved, and the connection reliability of semiconductor chips is improved.

CN119096330APending Publication Date: 2024-12-06RESONAC CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202480002341.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-28
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

During semiconductor chip manufacturing, fragment residues generated by laser processing will affect the connectivity of hybrid bonds, resulting in reduced reliability.

Method used

An opening is formed by using a photosensitive resin layer through light irradiation and developing the developer for plasma cutting without laser processing, thereby reducing fragment residue. The method includes forming a photosensitive resin layer on the semiconductor wafer, forming an opening by light irradiation and developing the developer, and dividing the wafer with plasma cleavage, and then removing the photosensitive resin layer to reduce residue.

Benefits of technology

It effectively reduces the impact of fragment residue in hybrid bonding, improves the connection reliability of semiconductor chips, and avoids the fragmentation problems caused by laser processing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119096330A_ABST
    Figure CN119096330A_ABST
Patent Text Reader

Abstract

This method for manufacturing a semiconductor device is provided with: a step for forming a photosensitive resin layer on one main surface of a semiconductor wafer; a step for forming an opening through which the semiconductor wafer is exposed by removing a portion of the photosensitive resin layer by light irradiation and development using a developer; dividing the semiconductor wafer along the opening by plasma dicing to form a semiconductor chip having a first main surface and a second main surface on the opposite side to the first main surface, the semiconductor chip having a photosensitive resin layer on the first main surface; a step for removing the photosensitive resin layer on the semiconductor chip; and a step for hybrid bonding the semiconductor chip and another semiconductor component such that the first main surface of the semiconductor chip and the semiconductor component are in contact with each other.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for manufacturing a semiconductor device. Background Art

[0002] In the manufacturing process of semiconductor devices, semiconductor wafers are sometimes singulated into semiconductor chips by plasma dicing. In plasma dicing, for example, after a mask partially covering the semiconductor wafer is formed on the semiconductor wafer, plasma is irradiated from above the mask to selectively etch the portion of the semiconductor wafer not covered by the mask, thereby dividing the semiconductor wafer.

[0003] As a method for forming a mask as described above, there is a method of removing a portion of the layer by laser processing after forming a layer covering the entire surface of a semiconductor wafer. However, during laser processing, debris (processing debris) is scattered around the processing portion and sometimes adheres to the manufactured semiconductor chip. In the case where a semiconductor chip with debris attached is used in a semiconductor device, reliability may be reduced, etc. Therefore, when manufacturing semiconductor chips, a method of suppressing the residue of debris accompanying laser processing in the semiconductor chip is being studied (for example, Patent Document 1).

[0004] Previous technical literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2019-50237 Summary of the invention

[0007] Technical issues to be solved by the invention

[0008] As a bonding technology for semiconductor chips and other semiconductor components (semiconductor chips, semiconductor wafers, etc.), there is hybrid bonding. In hybrid bonding, the semiconductor chip and other semiconductor components respectively have bonding surfaces composed of electrodes and insulating films, and the bonding surfaces are directly bonded to each other. Therefore, when hybrid bonding is used to manufacture semiconductor devices, even if a small amount of debris adheres to the surface of the semiconductor chip, it is particularly susceptible to its influence, which may lead to problems such as connectivity.

[0009] The present invention relates to a method for manufacturing a semiconductor device by plasma dicing, which can reduce the influence of debris and the like in hybrid bonding.

[0010] Means for solving technical problems

[0011] One aspect of the present invention relates to a method for manufacturing a semiconductor device, which comprises: a process of forming a photosensitive resin layer on a main surface of a semiconductor wafer; a process of removing a portion of the photosensitive resin layer by light irradiation and development using a developer to form an opening exposing the semiconductor wafer; a process of dividing the semiconductor wafer along the opening by plasma cutting to form a semiconductor chip having a first main surface and a second main surface on the opposite side thereof, and a photosensitive resin layer is provided on the first main surface; a process of removing the photosensitive resin layer on the semiconductor chip; and a process of hybrid bonding the semiconductor chip and other semiconductor components in a manner in which the first main surface of the semiconductor chip is connected to the semiconductor component.

[0012] In the above manufacturing method, the photosensitive resin layer with the opening formed therein is used as a mask in plasma cutting. The photosensitive resin layer is not laser processed, but the opening can be formed by light irradiation and development using a developer. In this way, in the above manufacturing method, in order to form a mask in plasma cutting, it is not necessary to perform laser processing that causes the generation of fragments, so the influence of fragments in hybrid bonding can be reduced.

[0013] In the above manufacturing method, the developer may be a developer containing water. Also, the pH of the developer may be 11 or less. In these cases, it is possible to suppress the degradation of parts (dicing tape, dicing ring, etc.) used in manufacturing semiconductor devices.

[0014] In the above manufacturing method, the photosensitive resin layer may be a positive photosensitive resin layer. In the case where the photosensitive resin layer is a positive photosensitive resin layer, the photosensitive resin layer on the semiconductor chip can be easily removed by light irradiation and dissolution in a cleaning solution after plasma dicing.

[0015] The manufacturing method may further include a step of irradiating the photosensitive resin layer on the semiconductor chip with light. The photosensitive resin layer on the semiconductor chip may be removed by dissolving it in a cleaning solution. In this case, the cleaning solution may be a cleaning solution containing water. Furthermore, the pH of the cleaning solution may be 11 or less.

[0016] In the above production method, the photosensitive resin layer may contain a reaction product of a polythiol compound having a disulfide bond and a cyclic ether compound having a polyether chain and two or more cyclic ether groups, and a photoradical generator.

[0017] Effects of the Invention

[0018] According to an aspect of the present invention, there is provided a method of manufacturing a semiconductor device by plasma dicing, capable of reducing the influence of debris and the like in hybrid bonding. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 This is a schematic diagram showing an example of a method for manufacturing a semiconductor device.

[0020] Figure 2 This is a schematic diagram showing an example of a method for manufacturing a semiconductor device. DETAILED DESCRIPTION

[0021] The present invention is not limited to the following examples.

[0022] Figure 1 and Figure 2 This is a schematic diagram showing an example of a method for manufacturing a semiconductor device. Figure 1 and Figure 2 The method shown in the figure comprises: as shown in (a), a step of forming a photosensitive resin layer 30 on a main surface of a semiconductor wafer 10 (hereinafter also referred to as "step (a)"); as shown in (b), a step of removing a portion of the photosensitive resin layer 30 by light irradiation and development using a developer to form an opening 30a in which the semiconductor wafer 10 is exposed (hereinafter also referred to as "step (b)"); as shown in (c), dividing the semiconductor wafer 10 along the opening 30a by plasma cutting to form a first main surface 20a and a second main surface 20a opposite thereto. A process of preparing a semiconductor chip 20 having a second principal surface 20b on one side and a photosensitive resin layer 30 on the first principal surface 20a (hereinafter also referred to as “process (c)”); a process of removing the photosensitive resin layer 30 on the semiconductor chip 20 as shown in (d) (hereinafter also referred to as “process (d)”); and a process of hybrid bonding the semiconductor chip 20 and other semiconductor components 70 in a manner such that the first principal surface 20a of the semiconductor chip 20 is in contact with the semiconductor component 70 as shown in (e) (hereinafter also referred to as “process (e)”).

[0023] In step (a), a photosensitive resin layer 30 is formed on one main surface of a semiconductor wafer 10. The semiconductor wafer 10 may be, for example, a silicon wafer. An integrated circuit may be formed on one main surface side of the semiconductor wafer 10. The thickness of the semiconductor wafer 10 may be, for example, greater than 10 μm and less than 1000 μm. Such a semiconductor wafer 10 may be produced, for example, by forming an integrated circuit on one main surface side of the semiconductor wafer 10 and then grinding the back side of the surface on which the integrated circuit is formed.

[0024] An example of a semiconductor wafer 10 may include a wafer body and electrodes and an insulating film disposed on one main surface of the wafer body, and one main surface of the photosensitive resin layer 30 side of the semiconductor wafer 10 may be composed of an insulating film having an opening and electrodes disposed in the opening of the insulating film. By dividing such a semiconductor wafer 10 in the step (c) described later, a semiconductor chip 20 having a first main surface 20a composed of electrodes and an insulating film can be formed. The electrodes disposed on the semiconductor wafer 10 may include through electrodes penetrating the wafer body.

[0025] like Figure 1 As shown in (a), the semiconductor wafer 10 can be fixed on the dicing tape 50. A dicing ring can also be attached to the dicing tape 50. Examples of the constituent materials of the dicing tape 50 include acrylic adhesive materials, unsaturated polyester adhesive materials, rubber adhesive materials, and urethane adhesive materials. In addition, examples of the constituent materials of the dicing ring include SUS, aluminum, ABS resin, and PSS resin.

[0026] The photosensitive resin layer 30 may be formed to cover the entirety of one main surface of the semiconductor wafer 10 or may be formed to cover a portion thereof. The photosensitive resin layer 30 may be formed to cover the entirety of the portion of the semiconductor wafer 10 where the integrated circuit is formed. The photosensitive resin layer 30 may be a positive photosensitive resin layer or a negative photosensitive resin layer. In the case where the photosensitive resin layer 30 is a positive photosensitive resin layer, in the step of removing the photosensitive resin layer on the semiconductor chip 20 described later, the photosensitive resin layer 30 on the semiconductor chip 20 can be easily removed by light irradiation and dissolution in a cleaning solution.

[0027] In step (b), a portion of the photosensitive resin layer 30 is removed by light irradiation and development using a developer. As a result, an opening 30a is formed in the photosensitive resin layer 30, and the semiconductor wafer 10 is exposed in the opening 30a. In the case where the photosensitive resin layer 30 is a positive photosensitive resin layer, the portion of the photosensitive resin layer 30 corresponding to the opening 30a is irradiated with light and removed by dissolving the portion in the developer.

[0028] The light source used for light irradiation may be, for example, an LED lamp, a mercury lamp (e.g., a low-pressure mercury lamp, a medium-pressure mercury lamp, and a high-pressure mercury lamp), a metal halide lamp, an excimer lamp, or a xenon lamp. Light irradiation may be performed directly on the photosensitive resin layer 30 or through glass or the like. Examples of irradiated light include visible light and ultraviolet light. The irradiated light may be, for example, light having a wavelength of 365 nm. The wavelength of the irradiated light may be, for example, 150 to 550 nm.

[0029] The exposure dose of light irradiation can be, for example, 1000 mJ / cm 2Above, and can be 2000mJ / cm 2 In this specification, exposure refers to illuminance (mW / cm 2 ) multiplied by the irradiation time (seconds).

[0030] The developer for development can be, for example, a developer comprising water. As water, for example, tap water, natural water, purified water, distilled water, ion exchanged water, pure water and ultrapure water (Milli-Q water, etc.) can be cited. Milli-Q water refers to the ultrapure water obtained by the Milli-Q water manufacturing device of Merck Millipore (Merck KGaA). From the viewpoint of impurity reduction, water can be purified water, distilled water, ion exchanged water, pure water or ultrapure water. The ratio of the water contained in the developer is based on the developer total amount, for example, can be more than 80 mass %.

[0031] The pH of the developer may be 14 or less, 12 or less, 11 or less, 10 or less, or 8 or less, and may be 1 or more, 2 or more, 4 or more, or 6 or more. When the developer is neutral or nearly neutral, deterioration of parts such as the dicing tape and the dicing ring can be suppressed.

[0032] The developer may contain a hydrophilic organic solvent. Examples of the hydrophilic organic solvent include alcohols such as methanol, ethanol, 2-propanol, and 1,2-propylene glycol; and glycol ethers such as ethylene glycol monomethyl ether, propylene glycol monomethyl ether, ethyl cellosolve, propylene glycol monopropyl ether, propylene glycol monoisopropyl ether, butyl cellosolve, ethylene glycol monoisobutyl ether, propylene glycol monobutyl ether, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, and dipropylene glycol monomethyl ether.

[0033] The developer may contain a pH adjuster. Examples of the pH adjuster include inorganic acids, inorganic bases, organic acids, and organic bases. Examples of inorganic acids include nitric acid, sulfuric acid, hydrochloric acid, phosphoric acid, and boric acid. Examples of inorganic bases include sodium hydroxide, potassium hydroxide, and calcium hydroxide. Examples of organic acids include formic acid, acetic acid, propionic acid, butyric acid, acrylic acid, benzoic acid, and picolinic acid. Examples of organic bases include primary amines, secondary amines, tertiary amines, tetramethylammonium hydroxide, tetraethylammonium hydroxide, and imidazole compounds.

[0034] A positive photosensitive resin layer that can be developed by a developer containing water and being neutral or nearly neutral can be, for example, a layer containing a chemical bond (e.g., a disulfide bond) that is cleaved by light irradiation and a polymer having a hydrophilic group. An example of such a positive photosensitive resin layer contains a reaction product (polymer) of a polythiol compound having a disulfide bond (hereinafter, also referred to as "compound (A)") and a cyclic ether compound having a polyether chain as a hydrophilic group and having two or more cyclic ether groups (hereinafter, also referred to as "compound (B)") and a photoradical generator. In this case, the photosensitive resin layer has the property of melting by light irradiation. If the photosensitive resin layer containing the reaction product of compound (A) and compound (B) and the photoradical generator is irradiated with light, the photoradical generator cleaves the disulfide bond (-SS-) in the reaction product of compound (A) and compound (B). As a result, the reaction product of compound (A) and compound (B) is reduced in molecular weight and can become a liquid (liquid).

[0035] The resin component produced by the low molecular weight of the reaction product of compound (A) and compound (B) has a large number of polyether chains or hydroxyl groups and tends to be hydrophilic, so the resin component dissolves in a developer containing water. Therefore, when such a photosensitive resin layer is used, it can be removed by development using a developer containing water.

[0036] Specifically, the reaction product of compound (A) and compound (B) may be a product of a curing reaction of compound (A) and compound (B). The photosensitive resin layer 30 containing the reaction product of compound (A) and compound (B) and a photoradical generator can be formed, for example, by a method comprising the following steps: a step of preparing a thermosetting composition containing compound (A), compound (B), a curing accelerator and a photoradical generator; and a step of further curing the thermosetting composition by heating the thermosetting composition. In this case, it can also be said that the photosensitive resin layer 30 contains a cured product of the above-mentioned thermosetting composition.

[0037] The thermosetting composition containing the compound (A), the compound (B), the curing accelerator and the photoradical generator can be prepared by, for example, mixing the compound (A), the compound (B), the curing accelerator and the photoradical generator.

[0038] Compound (A) is a compound having a disulfide bond (-SS-) and having two or more thiol groups (-SH). The upper limit of the number of thiol groups of compound (A) may be, for example, 5 or less. Compound (A) may be, for example, a dithiol compound, which is a compound having two thiol groups (-SH). Compound (A) may be a high molecular weight component of a polymer or oligomer. A compound having two thiol groups (-SH) may be considered to be a compound formed by two thiol groups and a group (the first connecting group) comprising a disulfide bond and connecting the two thiol groups.

[0039] The molecular weight or number average molecular weight of compound (A) may be, for example, 100 to 10,000,000, 200 to 3,000,000, 300 to 1,000,000, 400 to 10,000, or 500 to 5,000. The number average molecular weight is a polystyrene conversion value obtained by gel permeation chromatography (GPC) using a calibration curve based on standard polystyrene.

[0040] Compound (A) has one or more (two or more) disulfide bonds in the molecule. The number of disulfide bonds in compound (A) may be, for example, 1 to 1000 or 4 to 50.

[0041] Compound (A) may be a compound (e.g., a polymer or oligomer) having a linear or branched molecular chain and an end group, and having a disulfide bond in the molecular chain. In this case, the end group in compound (A) may be a thiol group. If compound (A) is such a compound, it has a tendency to further easily form a cured product having excellent photofusibility. The molecular chain in compound (A) may contain a disulfide bond and a polyether chain, or may consist of a disulfide bond and a polyether chain.

[0042] Compound (A) can be, for example, represented by formula (1): HS-(XSS) n1 -X-SH (compound (1)). In the formula, X represents a polyether chain. Multiple Xs may be the same or different. n1 represents an integer greater than 1. n1 may be, for example, 1 or more or 4 or more, and may be 1000 or less. In the case where compound (A) is a compound represented by formula (1), -(XSS) n1 The group represented by -X- is the first linking group. The compound for extending the chain of compound (1) may be, for example, a Michael adduct of compound (1) or a thiocarbamate of compound (1).

[0043] The polyether chain as X may be, for example, a polyoxyalkylene chain. The polyether chain as X may be, for example, a 1 -OX 2 -OX 3- represents a group. 1 ~X 3 Each of them independently may be an alkylene group, or may be an alkylene group having 1 to 2 carbon atoms (for example, a methylene group or an ethylene group). As for the polyether chain as X, for example, -CH2CH2-O-CH2-O-CH2CH2- can be mentioned.

[0044] As commercially available products of compound (A), for example, THIOKOL LP series (dithiol having a disulfide bond, manufactured by TORAY FINE CHEMICALS CO., LTD.) can be cited. Compound (A) can be obtained by converting the reactive functional group of a compound having a reactive functional group (e.g., carboxyl or hydroxyl group) and a disulfide bond at the terminal into a thiol group. Examples of compounds having a reactive functional group and a disulfide bond at the terminal include 3,3'-dithiodipropionic acid (manufactured by Tokyo Chemical Industry Co., Ltd.), dithiodiethanol and cystamine.

[0045] The content of compound (A) in the thermosetting composition may be 15 mass % or more, 25 mass % or more, or 35 mass % or more, and may be 80 mass % or less, 70 mass % or less, or 60 mass % or less, based on the total amount of the thermosetting composition.

[0046] Compound (B) is a compound having a polyether chain and having more than two cyclic ether groups. If the photosensitive resin layer 30 containing a cured product of a thermosetting composition containing compound (B) (specifically, a reaction product of compound (A) and compound (B)) is irradiated with light, the reaction product of compound (A) and compound (B) is reduced in molecular weight, and a resin component having a structure derived from compound (B) is generated. Here, since compound (B) is a compound having a polyether chain and having more than two cyclic ether groups, a large number of resin components having more polyether chains or (derived from cyclic ether groups) hydroxyl groups and having a tendency to show hydrophilicity are generated. Therefore, by using such a compound (B), in steps (b) and step (d), a developer or cleaning solution containing water can be used to remove the photosensitive resin layer 30. Compound (B) can be a high molecular weight component of a polymer or an oligomer.

[0047] The cyclic ether group of compound (B) can be a group that removes one hydrogen atom from a cyclic ether compound. As a specific example of the cyclic ether group of compound (B), ethylene oxide (for example, oxiranyl and epoxy), oxetane (for example, oxetane), tetrahydrofuranyl and tetrahydropyranyl can be cited. Wherein, from the viewpoint of reactivity and easy availability, the cyclic ether group can be an ethylene oxide group. That is, compound (B) can be an ethylene oxide compound (epoxy compound) having a polyether chain and having more than two ethylene oxides (for example, oxiranyl or epoxy). In addition, in this specification, in the cyclic ether group, a group having a cyclic ether structure (including a structure of a cyclic ether group) is included. For example, in the cyclic ether group, a group having an ethylene oxide structure (including a structure of an ethylene oxide (for example, an oxiranyl or epoxy)) such as a glycidyl group, a glycidyl ether group, an epoxycyclohexyl group is included.

[0048] The molecular weight or number average molecular weight of compound (B) may be, for example, 100 to 1,000,000, 100 to 500,000, 100 to 10,000, 150 to 5,000, or 200 to 2,000. The number average molecular weight is a polystyrene conversion value obtained by gel permeation chromatography (GPC) using a calibration curve based on standard polystyrene.

[0049] When the cyclic ether group of the compound (B) is an oxyethylene group (eg, an oxirane group or an epoxy group), the epoxy equivalent of the compound (B) may be 50 to 2000 g / eq, 80 to 1500 g / eq, or 100 to 1000 g / eq.

[0050] Compound (B) may be a compound having two cyclic ether groups (hereinafter, also referred to as "compound (B1)"), or a compound having three or more cyclic ether groups (hereinafter, also referred to as "compound (B2)"). Compound (B1) can be regarded as a compound formed by two cyclic ether groups and a group (second connecting group) comprising a polyether chain and connecting the two cyclic ether groups. Compound (B2) may be a compound having one or more cyclic ether groups as a side chain or substituent of the second connecting group in compound (B1). Compound (B) can further shorten the curing time of the thermosetting composition, and can further improve the photosensitivity of the photosensitive resin layer 30 and its solubility in a developer or a cleaning solution comprising water, and therefore may include compound (B1) and compound (B2).

[0051] Compound (B1) may be a compound (e.g., a polymer or oligomer) having a linear molecular chain and an end group, and having a polyether chain in the molecular chain. In this case, the end group in compound (B1) may be a cyclic ether group. When compound (B) is compound (B1), there is a tendency to easily remove the resin component produced by light irradiation of the photosensitive resin layer 30 with a developer or cleaning solution containing water. The polyether chain as a molecular chain may have a hydroxyl group, an alkyl group having a hydroxyl group, or other substituents. The molecular chain in compound (B1) may contain a polyether chain or may be formed by a polyether chain.

[0052] Compound (B1) can be, for example, a compound represented by formula (2): Z-(Y) n2 -Z represented by compound (compound (2)). In the formula, Y represents a polyether chain, and Z represents a cyclic ether group. Multiple Zs may be the same or different. n2 represents an integer greater than 1. n2 may be, for example, greater than 1 or greater than 2, and may be less than 1000. In the case where compound (B1) is a compound represented by formula (2), -(Y) n2 The group represented by - is the second connecting group.

[0053] The polyether chain as Y may be, for example, a polyoxyalkylene chain. The polyether chain as Y may be, for example, a polyoxyalkylene chain. 1 -OY 2 -OY 3 -represented by a group. 1 ~Y 3 Each of them independently may be an alkylene group, or may be an alkylene group having 1 to 3 carbon atoms (for example, a methylene group, an ethylene group, or a propylene group). As for the polyether chain as Y, for example, -CH2CH2-O-CH2-CH2-O-CH2CH2- can be mentioned.

[0054] Examples of commercially available products of the compound (B1) include DENACOL EX series (EX-850, EX-851, EX-821, EX-830, EX-832, EX-841, EX-861, and EX-920, manufactured by Nagase ChemteX Corporation).

[0055] The compound (B2) may be a compound having one or more cyclic ether groups as a side chain of the second linking group (polyether chain as Y) in the compound (B1).

[0056] As a commercial item of compound (B2), DENACOL EX series (EX-614B, EX-313, EX-512 and EX-521, manufactured by Nagase ChemteX Corporation) is mentioned, for example.

[0057] The content of compound (B) (the total of compound (B1) and compound (B2)) in the thermosetting composition can be 15% by mass or more, 25% by mass or more, or 35% by mass or more, and can be 80% by mass or less, 70% by mass or less, or 60% by mass or less, based on the total amount of the thermosetting composition.

[0058] The mass ratio of the content of the compound (B2) to the content of the compound (B) (the total of the compound (B1) and the compound (B2)) in the thermosetting composition (the content (mass) of the compound (B2) / the content (mass) of the compound (B) (the total of the compound (B1) and the compound (B2))) may be 0.01 to 0.40. If the mass ratio is 0.01 or more, there is a tendency that the curing time of the thermosetting composition can be further shortened, and if the mass ratio is 0.40 or less, there is a tendency that the photosensitivity of the photosensitive resin layer 30 and the solubility of the resin component generated by light irradiation of the photosensitive resin layer 30 in a developer or a cleaning solution containing water can be further improved. The mass ratio may be 0.02 or 0.03 or more, and may be 0.35 or less, 0.30 or less, 0.25 or less, 0.20 or less, 0.15 or less, 0.10 or less, or 0.05 or less.

[0059] The equivalent ratio of the cyclic ether group of the compound (B) to the thiol group of the compound (A) (cyclic ether group of the compound (B) / thiol group of the compound (A)) can be, for example, 0.5 to 2.5. If the equivalent ratio is 0.5 or more, there is a tendency to further improve the solubility of the resin component generated by light irradiation of the photosensitive resin layer 30 in a developer or a cleaning solution containing water, and if the equivalent ratio is 2.5 or less, there is a tendency to further improve the photofusibility of the photosensitive resin layer 30. The equivalent ratio can be 0.8 or more, 1.0 or more, 1.2 or more, or 1.5 or more, and can be 2.2 or less or 2.0 or less.

[0060] The curing accelerator is a component for accelerating the (curing) reaction of compound (A) and compound (B), and includes a component that acts as a catalyst for the curing reaction (catalyst-type curing agent). Examples of curing accelerators include amine compounds, imidazole derivatives, quaternary ammonium salts, organic metal salts, and phosphorus compounds.

[0061] Examples of the amine compound include dicyandiamide, trimethylamine, triethylamine, tripropylamine, tributylamine, tri-n-octylamine, dimethylethylamine, dimethylpropylamine, dimethylbutylamine, dimethyl-n-octylamine, 1,4-diazabicyclo[2.2.2]octane, 1,8-diazabicyclo[5.4.0]undec-7-ene, benzyldimethylamine, 4-methyl-N,N-dimethylbenzylamine, 2,4,6-tris(dimethylaminomethyl)phenol and 4-dimethylaminopyridine.

[0062] Examples of imidazole derivatives include 1-(1-cyanomethyl)-2-ethyl-4-methyl-1H-imidazole, 2-ethyl-4-methylimidazole, 2-methylimidazole, 2-phenylimidazole, 1-cyanoethyl-2-phenylimidazole, 2-phenyl-4,5-dihydroxymethylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, 2,4,5-triphenylimidazole, 1-benzyl-2-imidazole, 1,2-dimethylimidazole and 1-benzyl-2-phenylimidazole.

[0063] Examples of the quaternary ammonium salt include tetramethylammonium chloride, tetraethylammonium chloride, tetrabutylammonium chloride, benzyltrimethylammonium chloride, benzyltriethylammonium chloride, benzyltributylammonium chloride, tetramethylammonium bromide, tetraethylammonium bromide, tetrabutylammonium bromide, benzyltrimethylammonium bromide, benzyltriethylammonium bromide, tetramethylammonium iodide, tetraethylammonium iodide, tetrabutylammonium iodide, and benzyltributylammonium iodide.

[0064] Examples of the organic metal salt include bis(2,4-pentanedione)zinc(II), zinc octoate, zinc naphthenate, cobalt naphthenate, copper naphthenate, iron acetylacetonate, nickel octoate, and manganese octoate.

[0065] Examples of the phosphorus compound include tetraphenylphosphonium tetra-p-tolylborate, tetraphenylphosphonium tetraphenylboron, triphenylphosphine, tri-p-tolylphosphine, tri(4-chlorophenyl)phosphine, tri(4-methoxyphenyl)phosphine, tri(2,6-dimethoxyphenyl)phosphine, triphenylphosphine triphenylborane, tetraphenylphosphonium dicyanamide, and tetraphenylphosphonium tetra(4-methylphenyl)borate.

[0066] The content of the curing accelerator may be 0.01 mass % or more, 0.1 mass % or more, or 0.5 mass % or more, and may be 10 mass % or less, 5 mass % or less, or 2 mass % or less, based on the total amount of the thermosetting composition.

[0067] The photoradical generator is a component that generates free radicals by light irradiation. Examples of the photoradical generator include a hydrogen-abstracting photoradical polymerization initiator that generates free radicals by extracting hydrogen from other molecules by light irradiation, and an intramolecular cleavage photoradical polymerization initiator that generates two free radicals by photolysis by light irradiation. From the perspective of facilitating the (photomelting) reaction of the photosensitive resin layer 30, the photoradical generator may be an intramolecular cleavage photoradical polymerization initiator.

[0068] Examples of the hydrogen abstraction type photo-radical generator include hexaarylbiimidazole (HABI) compounds, benzophenone compounds, thioxanthone compounds, fluorenone compounds, and α-diketone compounds.

[0069] Examples of HABI compounds include 2,2'-bis(o-chlorophenyl)-4,4',5,5'-tetraphenylbiimidazole (e.g., 2,2'-bis(2-chlorophenyl)-4,4',5,5'-tetraphenyl-1,2'-biimidazole), 2,2'-bis(o-bromophenyl)-4,4',5,5'-tetraphenylbiimidazole, 2,2'-bis(o-,p-dichlorophenyl)-4,4',5,5 '-Tetraphenylbiimidazole, 2,2'-bis(o-chlorophenyl)-4,4',5,5'-tetra(m-methoxyphenyl)biimidazole, 2,2'-bis(o-,o-dichlorophenyl)-4,4',5,5'-tetraphenylbiimidazole, 2,2'-bis(o-nitrophenyl)-4,4',5,5'-tetraphenylbiimidazole and 2,2'-bis(o-methylphenyl)-4,4',5,5'-tetraphenylbiimidazole.

[0070] Examples of the benzophenone compound include 4,4'-bis(dimethylamino)benzophenone and 4,4'-bis(diethylamino)benzophenone.

[0071] Examples of thioxanthone compounds include thioxanthone, 2-isopropylthioxanthone, 2-dodecylthioxanthone, 2-cyclohexylthioxanthone, 2,4-diethylthioxanthone, 2,4-dimethylthioxanthone, 1-phenoxythioxanthone, 1-methoxycarbonylthioxanthone, 2-ethoxycarbonylthioxanthone, 3-(2-methoxyethoxycarbonyl)thioxanthone,

[0072] -thioxanthone, 4-butoxycarbonyl thioxanthone, 3-butoxycarbonyl-7-methyl thioxanthone, 3,4-di-[2-(2-methoxyethoxy)-ethoxycarbonyl]-thioxanthone, 2-chlorothioxanthone, 1-ethoxycarbonyl-3-ethoxythioxanthone, 1-ethoxycarbonyl-3-chlorothioxanthone, 1-chloro-4-n-propoxythioxanthone, 2-methyl-6-dimethoxymethyl-thioxanthone, 2-methyl-6-(1,1-dimethoxybenzyl)-thioxanthone, 6-ethoxycarbonyl-2-methoxy-thioxanthone, 6-ethoxycarbonyl-2-methylthioxanthone, 1-ethoxycarbonyl-3-(1-methyl-1-morpholinylethyl)-thioxanthone, 2-morpholinylmethylthioxanthone, 2-methyl-6-morpholinylmethylthioxanthone, and thioxanthone-2-carboxylic acid polyethylene glycol ester.

[0073] Examples of the fluorenone compound include 9-fluorenone, 3,4-benzo-9-fluorenone, 2-dimethylamino-9-fluorenone, 2-methoxy-9-fluorenone, 2-chloro-9-fluorenone, 2,7-dichloro-9-fluorenone, 2-bromo-9-fluorenone, 2,7-dibromo-9-fluorenone, 2-nitro-9-fluorenone and 2-acetyl-9-fluorenone.

[0074] Examples of α-diketone compounds include benzyl (also referred to as diphenylethanedione or dibenzoyl).

[0075] Examples of the intramolecular cleavage type photoradical generator include benzyl ketal photoradical generators, α-aminoalkylphenone photoradical generators, α-hydroxyalkylphenone photoradical generators, α-hydroxyacetophenone photoradical generators, and acylphosphine oxide photoradical generators.

[0076] Examples of the benzyl ketal-based photoradical generator include 2,2-dimethoxy-1,2-diphenylethane-1-one (Omnirad 651).

[0077] Examples of α-aminoalkylphenone-based photoradical generators include 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1 (Omnirad369), 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropane-1-one (Omnirad907), and 2-dimethylamino-2-(4-methyl-benzyl)-1-(4-morpholin-4-yl-phenyl)-butan-1-one (Omnirad379EG).

[0078] Examples of the α-hydroxyalkylphenone-based photoradical generator include 1-hydroxy-cyclohexyl-phenyl-ketone (Omnirad 184).

[0079] Examples of α-hydroxyacetophenone-based photoradical generators include 2-hydroxy-1-{4-[4-(2-hydroxy-2-methyl-propionyl)-benzyl]-phenyl}-2-methyl-propane-1-one (Omnirad 127) and 2-hydroxy-2-methyl-1-phenyl-propane-1-one (Omnirad 1173).

[0080] Examples of the acylphosphine oxide-based photoradical generator include 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide (Omnirad TPO H) and bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide (Omnirad 819).

[0081] The content of the photo radical generator in the thermosetting composition may be 1 mass % or more, 5 mass % or more, or 10 mass % or more, and may be 30 mass % or less, 20 mass % or less, or 15 mass % or less, based on the total amount of the thermosetting composition.

[0082] The thermosetting composition may further contain other ingredients except compound (A), compound (B), curing accelerator and light free radical generator. As other ingredients, for example, adhesive imparting agents such as plasticizers and tackifiers, antioxidants, leuco dyes, sensitizers, adhesion improvers such as coupling agents, polymerization inhibitors, light stabilizers, defoamers, fillers, chain transfer agents, thixotropy imparting agents, flame retardants, release agents, surfactants, lubricants, antistatic agents and other additives can be cited. These additives can use known additives. The content of other ingredients in the thermosetting composition is based on the total amount of the thermosetting composition, and can be 0 to 95% by mass, 0.01 to 50% by mass or 0.1 to 10% by mass.

[0083] The thermosetting composition described above is heated to carry out a (curing) reaction with compound (A) and compound (B) (for example, a compound having a glycidyl ether group as a cyclic ether group) to generate a cured product of the thermosetting composition. Here, the cured product of the thermosetting composition includes a reaction product of compound (A) and compound (B) and a photoradical generator. The reaction product of compound (A) and compound (B) can be, for example, a compound (polymer) having a structure represented by the following formula.

[0084]

[0085] In the formula, X represents a first linking group comprising a disulfide bond, and Y represents a second linking group comprising a polyether chain. m represents an integer greater than 1. For example, m may be greater than 50, greater than 100, greater than 500, or greater than 1000. * represents a bonding hand.

[0086] The heating temperature of the thermosetting composition may be, for example, 0 to 200° C., 30 to 150° C., or 60 to 100° C. The heating time of the thermosetting composition may be, for example, 0.1 to 168 hours, or 72 hours or less, 24 hours or less, 12 hours or less, 6 hours or less, 4 hours or less, 3 hours or less, or 2 hours or less.

[0087] The method for forming the photosensitive resin layer 30 containing the reaction product of the above-mentioned compound (A) and compound (B) and a photo radical generator may further include a step of disposing the above-mentioned thermosetting composition on one main surface of the semiconductor wafer 10. In this case, after disposing the thermosetting composition on one main surface of the semiconductor wafer 10, the thermosetting composition is heated.

[0088] As an example of a method for disposing the thermosetting composition on one main surface of the semiconductor wafer 10, the following method can be cited: a varnish of the thermosetting composition is prepared by diluting the thermosetting composition with a solvent, and the prepared varnish is applied to one main surface of the semiconductor wafer 10. Examples of the solvent include aromatic hydrocarbons such as toluene, xylene, mesitylene, cumene, and p-isopropylbenzene; aliphatic hydrocarbons such as hexane and heptane; cycloalkanes such as methylcyclohexane; cyclic ethers such as tetrahydrofuran and 1,4-dioxane; ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, and 4-hydroxy-4-methyl-2-pentanone; esters such as methyl acetate, ethyl acetate, butyl acetate, methyl lactate, ethyl lactate, and γ-butyrolactone; carbonates such as ethylene carbonate and propylene carbonate; and amides (NMP) such as N,N-dimethylformamide, N,N-dimethylacetamide, and N-methyl-2-pyrrolidone. The solid content in the varnish, that is, the total content of the varnish other than the solvent, may be 10 to 95% by mass, 15 to 70% by mass, or 20 to 50% by mass based on the total amount of the varnish.

[0089] In another embodiment, the method for forming the photosensitive resin layer 30 containing the reaction product of the above-mentioned compound (A) and compound (B) and the photo radical generator may further include the step of disposing a cured product of the thermosetting composition on one main surface of the semiconductor wafer 10. In this case, after heating the thermosetting composition, the cured product of the thermosetting composition is disposed on one main surface of the semiconductor wafer 10. The cured product of the thermosetting composition may be, for example, in the form of a film. The cured product of the film-like thermosetting composition may be produced, for example, by injecting the above-mentioned thermosetting composition into a mold and heating it.

[0090] The photosensitive resin layer 30 is not limited to the above examples, and may be a positive or negative photosensitive resin layer containing any photosensitive material used for photolithography. For example, the photosensitive resin layer 30 may contain any one of a positive or negative liquid photoresist, a photosensitive film, a photosensitive solder resist, and a photosensitive polyimide.

[0091] In step (c), the semiconductor wafer 10 is divided along the openings 30a by plasma dicing, thereby forming semiconductor chips 20 having a first main surface 20a and a second main surface 20b opposite thereto, and having a photosensitive resin layer 30 provided on the first main surface 20a.

[0092] Plasma cutting refers to cutting based on plasma etching. The conditions of plasma cutting can be appropriately set according to the type and thickness of the semiconductor wafer 10. In plasma cutting, for example, a dry etching device can be used. Regarding the generation of plasma, for example, C4F6 gas, C4F8 gas, etc. can be used.

[0093] Plasma dicing can be performed, for example, by the BOSCH method. In the BOSCH method, plasma for forming a protective film and plasma for etching are alternately generated to cut the semiconductor wafer 10. The BOSCH method enables etching with a high aspect ratio.

[0094] In step (d), the photosensitive resin layer 30 on the semiconductor chip 20 is removed.

[0095] The photosensitive resin layer 30 on the semiconductor chip 20 can be removed by, for example, irradiating light or dissolving in a cleaning solution. In this case, the manufacturing method further includes a step of irradiating the photosensitive resin layer 30 on the semiconductor chip 20 with light.

[0096] The light source for light irradiation can use the above-mentioned light source without particular limitation as the light source for light irradiation in step (b). Regarding light irradiation, the photosensitive resin layer 30 on a plurality of semiconductor chips 20 (for example, all semiconductor chips 20 present on the same dicing tape 50) can be collectively performed. In this case, examples of light sources for light irradiation include mercury lamps (low-pressure mercury lamps, medium-pressure mercury lamps, high-pressure mercury lamps), metal halide lamps, and LED lamps. Light irradiation can be performed directly on the photosensitive resin layer 30 or through glass or the like. Examples of irradiated light include visible light and ultraviolet light. The irradiated light can be, for example, light containing a wavelength of 365 nm. The wavelength of the irradiated light can be, for example, a wavelength of 150 to 550 nm.

[0097] The exposure amount of light irradiation in the step (b) can be within the above-mentioned numerical range.

[0098] As the cleaning liquid, the above-mentioned cleaning liquids can be used as the developing liquid in step (b) without particular limitation. The pH of the cleaning liquid can be within the above-mentioned numerical range as the pH of the developing liquid in step (b).

[0099] In another embodiment, the photosensitive resin layer 30 on the semiconductor chip 20 may be removed by ashing. The ashing is performed, for example, by a method including irradiating the photosensitive resin layer 30 on the semiconductor chip 20 with plasma generated using oxygen.

[0100] In step (e), the semiconductor chip 20 and the other semiconductor component 70 are hybrid-bonded in such a manner that the first main surface 20a of the semiconductor chip 20 is in contact with the semiconductor component 70. Figure 2 (e) shows the semiconductor device 100.

[0101] Figure 2 The semiconductor chip 20 shown in (e) includes a main body 20A, an electrode 21 and an insulating film 22 provided on one main surface of the main body 20A. The first main surface 20a of the semiconductor chip 20 is a bonding surface for hybrid bonding composed of the electrode 21 and the insulating film 22. Here, the first main surface 20a of the semiconductor chip 20 corresponds to the surface provided with the photosensitive resin layer 30 removed in the step (d). In addition, the semiconductor component 70 includes an electrode 71 and an insulating film 72, and the surface of the semiconductor component 70 that is in contact with the first main surface 20a of the semiconductor chip 20 (hereinafter, also referred to as "the first main surface of the semiconductor component 70") 70a is a bonding surface composed of the electrode 71 and the insulating film 72. The semiconductor component 70 may be, for example, a semiconductor wafer or a semiconductor chip. The second main surface 20b of the semiconductor chip 20 may also be a bonding surface composed of an electrode and an insulating film. In this case, a plurality of semiconductor chips 20 may be stacked by hybrid bonding.

[0102] The electrode 21 and the electrode 71 may each independently include Cu as a constituent material. The insulating film 22 and the insulating film 72 may each independently include an inorganic insulator such as SiO 2 or an organic insulator (including a dielectric) as a constituent material.

[0103] like Figure 2 As shown in (e), the hybrid bonding of the semiconductor chip 20 and other semiconductor components 70 can be implemented by a method comprising the following steps: a step of picking up the semiconductor chip 20 from the cutting tape 50; a step of aligning the semiconductor chip 20 and the semiconductor component 70 in such a way that the first main surface 20a of the semiconductor chip 20 is in contact with the semiconductor component 70; and a step of joining the semiconductor chip 20 and the semiconductor component 70.

[0104] In the process of picking up the semiconductor chip 20 from the dicing tape 50, for example, the dicing tape 50 is bent by pressing the ejector pin from the lower part of the dicing tape 50, and the semiconductor chip 20 is picked up from the dicing tape 50 by the suction chuck. In the case of an ultraviolet curing dicing tape whose adhesive strength is reduced by ultraviolet irradiation, the adhesive strength of the dicing tape 50 may be reduced by ultraviolet irradiation before this process.

[0105] In the process of aligning the semiconductor chip 20 and the semiconductor component 70 in such a way that the first main surface 20a of the semiconductor chip 20 is connected to the semiconductor component 70, the first main surface 20a of the semiconductor chip 20 and the first main surface 70a of the semiconductor component 70 are arranged in such a way that the electrodes 21 and the electrode 71, and the insulating film 22 and the insulating film 72 are respectively opposite to each other.

[0106] In the step of bonding the semiconductor chip 20 and the semiconductor component 70, the first main surface 20a of the semiconductor chip 20 is brought into contact with the first main surface 70a of the semiconductor component 70. More specifically, the electrodes 21 and 71, and the insulating films 22 and 72 are brought into contact with each other.

[0107] In the process of bonding the semiconductor chip 20 and the semiconductor component 70, at least one of heating and pressurization may be performed. The heating temperature may be, for example, 20°C or more or 200°C or more, and 500°C or less or 400°C or less. The pressurization pressure may be, for example, 0.1 MPa or more and 1.0 MPa or less.

[0108] The manufacturing method may include the following step: before the first main surface 20a of the semiconductor chip 20 is brought into contact with the first main surface 70a of the semiconductor component 70, a step of activating the bonding surface of at least one side of the first main surface 20a of the semiconductor chip 20 and the first main surface 70a of the semiconductor component 70. When the step of activating the bonding surface is included, bonding of the semiconductor chip 20 and the semiconductor component 70 becomes easy.

[0109] As a method for activating the bonding surface, there can be cited a method for hydrophilizing the bonding surface, a method for removing inactive substances (oxide film, etc.) on the bonding surface, etc. As an example of a method for hydrophilizing the bonding surface, there can be cited a method for irradiating the bonding surface with oxygen plasma. Furthermore, as an example of a method for removing inactive substances on the bonding surface, there can be cited a method for irradiating the bonding surface with an ion beam (e.g., an Ar ion beam) under high vacuum.

[0110] The step of activating the bonding surface may be performed, for example, after the step of removing the photosensitive resin layer 30 on the semiconductor chip 20 . Furthermore, the step of activating the bonding surface may be performed before the step of picking up the semiconductor chip 20 from the dicing tape 50 during the step of bonding the semiconductor chip 20 and the semiconductor component 70 .

[0111] Explanation of symbols

[0112] 10-semiconductor wafer, 20-semiconductor chip, 20a-first main surface, 20b-second main surface, 20A-main body, 21-electrode, 22-insulating film, 30-photosensitive resin layer, 30a-opening, 50-dicing tape, 70-semiconductor component, 70a-first main surface, 71-electrode, 72-insulating film, 100-semiconductor device.

Claims

1. A method for manufacturing a semiconductor device, comprising: A step of forming a photosensitive resin layer on one main surface of a semiconductor wafer; A step of removing a portion of the photosensitive resin layer by light irradiation and development using a developer to form an opening through which the semiconductor wafer is exposed; The semiconductor wafer is divided along the opening by plasma dicing to form semiconductor chips having a first main surface and a second main surface opposite thereto, and the photosensitive resin layer is provided on the first main surface; A step of removing the photosensitive resin layer on the semiconductor chip; and A step of hybrid bonding the semiconductor chip and other semiconductor components so that the first main surface of the semiconductor chip is in contact with the semiconductor component.

2. The manufacturing method according to claim 1, wherein: The developer contains water.

3. The manufacturing method according to claim 2, wherein: The pH of the developer is 11 or less.

4. The manufacturing method according to claim 1, wherein: The photosensitive resin layer is a positive photosensitive resin layer.

5. The manufacturing method according to claim 4, wherein: The method further comprises the step of irradiating the photosensitive resin layer on the semiconductor chip with light. The photosensitive resin layer on the semiconductor chip is removed by dissolving it in a cleaning solution.

6. The manufacturing method according to claim 5, wherein: The cleaning liquid is a cleaning liquid containing water.

7. The manufacturing method according to claim 6, wherein: The pH of the cleaning solution is 11 or less.

8. The manufacturing method according to any one of claims 4 to 7, wherein: The developer contains water.

9. The manufacturing method according to claim 8, wherein: The pH of the developer is 11 or less.