Aqueous separator slurry composition

By using anionic oxide nanoparticles and aqueous polymer binder, the environmental pollution and stability problems of traditional coating systems are solved, and a uniform and high porosity separator coating is achieved, and lithium electronic batteries are improved. security and performance.

CN119096407APending Publication Date: 2024-12-06阿科玛股份有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380034133.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-28
Filing Date
2023-04-24
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The non-aqueous coating systems used in existing electrochemical devices have environmental pollution, safety hazards and high cost problems. In addition, the charged alumina on the cationic surface in traditional aqueous systems leads to uneven coating and poor adhesive stability, which affects the membrane. performance.

Method used

Anionic oxide nanoparticles and aqueous polymer binders are used to prepare homogeneous aqueous slurries, avoid aggregation through surface charge regulation, and form a separator coating with high porosity and high mechanical strength, which is suitable for lithium electronic batteries.

Benefits of technology

A uniform and stable diaphragm coating is achieved, reducing the risk of short circuit of the battery at high temperatures, improving the cycle life and safety of the battery, while reducing the negative impact on the environment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005083585200000151
    Figure BDA0005083585200000151
  • Figure BDA0005083585200000161
    Figure BDA0005083585200000161
  • Figure BDA0005083585200000162
    Figure BDA0005083585200000162
Patent Text Reader

Abstract

The present invention relates to an aqueous slurry composition comprising a water-based polymer binder and anionic oxide nanoparticles, which aqueous slurry composition can be used, for example, in the coating of an electrode and / or a separator in an electrochemical device. The coating has high porosity and electronic isolation after being dried and shows high dimensional stability at high temperature.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an aqueous slurry composition for a separator coating in an electrochemical device.

[0002] background:

[0003] Separators play an important role in batteries. Compared with traditional polyolefin separators, the use of composite separators has been shown to improve the performance of lithium-ion batteries. This invention helps advance separator technology and improve the safety of lithium-ion batteries, promoting and accelerating the application of batteries in EVs (electric vehicles) and battery energy storage.

[0004] In the inorganic particle / polymer matrix or polymer binder coating composition, the polymer matrix or polymer binder can be used to provide: adhesion between inorganic particles, adhesion of the coating to the free-standing porous separator, and / or adhesion of the coated separator to one or more electrodes (adjacent or adjacent to the separator coating), and / or in-situ formation of the separator on the electrode to make an integrated electrode separator in a lithium electronic battery. Good contact between the separator and the electrode is important for the optimal cycle life of the lithium battery, because the presence of voids or spaces between the separator and the electrode may have an adverse effect on the long-term cycle life or battery performance.

[0005] Known inorganic nanoparticle / polyvinylidene fluoride (PVDF) coatings are typically based on non-aqueous slurries, solvent-based systems using solvents such as acetone, tetrahydrofuran (THF), dimethylformamide (DMF), N-methyl-2-pyrrolidone (NMP), dimethylacetamide (DMAC), combinations of these, and the like. PVDF has been used in such coatings because, for example, PVDF is inert and stable in lithium-ion battery systems. However, non-aqueous solvents for dissolving PVDF are typically hazardous and volatile, and may require careful use, disposal, and / or recycling because they may not be environmentally friendly and may produce undesirable emissions if improperly disposed of. Coating processes based on non-aqueous systems are costly, may have an unfavorable environmental footprint, and are difficult to handle due to safety issues associated with their flammability.

[0006] Therefore, there is a need for novel, optimized and / or improved self-supporting coated separators or cast separators (which are cast directly on the electrodes of electrochemical devices for application) having or produced using aqueous or water-based slurry systems, which may be preferred over non-aqueous or solvent-based coating systems due to, for example, performance, cost, environmental, safety and / or economic factors. The separators, cathodes and anodes coated with aqueous slurries of polymer binders and inorganic nanoparticles not only have good mechanical strength and good wet / dry adhesion, but also provide dimensional stability at high temperatures for the separators or electrodes, thereby reducing the possibility of short circuits in the battery when in use or at high temperatures. Prior art

[0007] http: / / dx.doi.org / 10.1016 / j.jpowsour.2015.11.067 The use of alumina of a few micrometers in size (Figure 2b) to cast an alumina-based ceramic paste to form a separator is demonstrated. The resulting separator coating on top of the electrode has limited flexibility and a thickness of 50 μm, which is thicker than commercial PE / PP separators. In addition, the SEM images (especially Figure 2b) show that the separator coating on the top is not uniform, which may be caused by the use of cationic surface charged alumina. In contrast, the present invention utilizes anionic oxide nanoparticles and is able to form a uniform coating and produce flexible thin separators, i.e., separators with a thickness of less than 25 μm, comparable to commercial PE / PP separators.

[0008] http: / / dx.doi.org / 10.1016 / j.memsci.2016.02.047 The fabrication of a free-standing membrane using micron-sized alumina and a pore former PEG is shown, as seen in the SEM shown in Figure 2(c). The resulting membrane thickness is 37 μm, which is thicker than commercially available PE / PP membranes. The PEG is removed by a time-consuming process that involves immersing the membrane in DI water and then drying. In contrast, the present invention uses anionic oxide nanoparticles to prepare a slurry that is able to produce a highly porous membrane without the need for a pore former.

[0009] "Entek" H-15 part DE-FC26-05NT42403 (report: https: / / www.osti.gov / servlets / purl / 1160224 ) demonstrates a separator made using a UHMWPE gel treatment combined with high loading levels of precipitated silica or fumed alumina as filler. The resulting filled separator has a large pore size with a thickness of >20 microns, which may compromise the performance and / or safety of the battery. In contrast, the present invention uses a high loading of cathode oxide nanoparticles, i.e., at least 20 weight percent cathode oxide nanoparticles, to produce a separator with high porosity without any organic solvent or gel treatment, so it is more environmentally sustainable and therefore desirable.

[0010] Patent publication number US20160164060A1 discloses an aqueous method for coating a separator. A method for producing a coated separator for a lithium battery, the method comprising the following steps: (a) providing a porous substrate, (b) applying a coating slurry on at least one surface of the porous substrate, wherein the coating slurry includes ceramic particles and a polymer binder in water or an aqueous solution or an aqueous suspension, and (c) drying the coating slurry to form a coating on the porous substrate. The choice of the type of ceramic used is not based on surface charge. Therefore, it is expected that the aqueous slurry coating will not be as uniform as shown in the SEM images of 1-5, which may be due to the use of cationic surface charged alumina. In contrast, in the SEM image of 8, the coating is uniform because it is solution cast, where the surface charge is weakened. In addition, the alumina particles used in the provided embodiments have a particle size of 0.65 μm and a BET surface area of ​​4.6 m 2 / g. In contrast to the patent, our invention is based on its surface charge characteristics (anionic), specific surface area (>15m 2 The inorganic particles are selected based on their wt. % to 30 wt. % (g) and their compatibility with the other components in the slurry to prevent agglomeration and thereby provide a uniform coating.

[0011] US9954211 patent relates to a separator, which includes a porous organic-inorganic coating composed of a mixture of inorganic particles and a polymer binder on a porous substrate, and an electrochemical device including the separator. "Inorganic particles are added to and dispersed in a first polymer binder solution. The solvent preferably has a solubility parameter similar to that of the first polymer binder and has a low boiling point, which is conducive to uniform mixing and easy removal of the solvent." The teachings and examples of the patent are all based on solution casting. Our invention uses water-based polymer binders and components to eliminate the use of the above-mentioned dangerous and environmentally harmful solvents.

[0012] In water-based slurries, cationic surface charged fumed alumina exhibits poor colloidal stability when mixed with conventional waterborne polymer binders including but not limited to polyvinylidene fluoride (PVDF), styrene-butadiene-rubber (SBR) and acrylic latex; or polyvinyl alcohol (PVA), carboxymethyl cellulose (CMC) or polyacrylic acid (PAA) or combinations thereof, causing severe aggregation, hindering homogenous mixing of slurries and uniform coatings. Surface functionalization is critical in determining its interaction with other components in waterborne slurry compositions.

[0013] We surprisingly found that by using anionic oxide nanoparticles (preferably alumina and / or silica) in an aqueous system, the slurry is stable in that it does not form visually visible aggregates or agglomerates. The cast slurry forms a smooth surface without visually visible defects (no agglomeration of anionic nanoparticles and binder), thus providing the desired slurry quality for coating applications. Summary of the invention

[0014] The present invention provides a homogenous slurry in which anionic particles and a binder are uniformly distributed (no agglomeration is observed visually and the Hegman fineness is less than 5), which can be used, for example, for coating electrodes and / or separators in electrochemical devices. The separator includes a porous composite having a microporous substrate and a coating formed on at least one surface of the porous substrate, wherein the coating is formed of particles and / or a mixture of particles and an aqueous or water-based polymer binder.

[0015] The present invention further provides a method for producing a separator for a lithium electronic battery, the method comprising providing a porous substrate (e.g., a polyolefin substrate or an electrode) to form a porous composite, and applying a coating to at least one surface of the porous substrate or electrode, wherein the coating comprises particles and / or a particle (inorganic) mixture and an aqueous or water-based polymer binder, wherein the aqueous or water-based polymer binder may include one or more generally water-insoluble polymers (e.g., PVDF, SBR, acrylic polymers) and may further include one or more generally water-soluble polymers (e.g., for example, PVA, CMC or PAA).

[0016] The present invention further provides the use of the self-supporting coated separator in a lithium electronic battery.

[0017] Also provided is a single operation use in which a slurry of conductive material (the slurry to form the electrode) and an aqueous slurry composition of the invention (to form the separator) are simultaneously cast onto a current collector and dried to form an integrated electrode / separator assembly.

[0018] The present invention discloses a method for preparing an aqueous slurry using anionic fumed oxide and an aqueous polymer binder, the slurry having a low Hegman fineness (less than 5), indicating excellent fluidity and fineness of grind. Preferably, the Hegman fineness is less than 3. In order to obtain a slurry without visually visible agglomeration and / or aggregation, it was surprisingly found that the surface charge of the nanoparticles is critical for dispersion uniformity and slurry stability. In addition, untreated fumed alumina can lead to severe aggregation, which hinders homogeneous mixing of the slurry and uniform coating, which is an unfavorable characteristic for achieving defect-free coatings.

[0019] The disclosed invention can be cast alone to produce a separator, membrane or film. It can also be cast simultaneously in a multilayer casting, such as disclosed in US 11,133,562, to produce an in-situ composite separator on an electrode for use in an electrochemical cell.

[0020] The present invention utilizes anionic surface charged oxides (e.g., fumed alumina or fumed silica) to prepare aqueous homogenous slurries. It has been found that the surface charge of the inorganic particles is critical because the aqueous slurry composition can aggregate depending on the surface charge of the oxide. Fewer additives or dispersants are required to address aggregation challenges, minimizing undesirable chemicals that compromise battery performance.

[0021] The embodiment of the present invention is to prepare water-based coatings using anionic oxide nanoparticles to obtain the necessary slurry quality for the coating. Using the present invention, aqueous deposition can be performed in different ways to obtain separators and / or separator coatings.

[0022] Other uses for the slurry compositions include applications requiring thin films that exhibit high porosity and electronic resistance.

[0023] The final aqueous slurry composition under dilute conditions (between 0.1 and 1% solids, preferably 1% solids) must have a negative zeta potential of less than -10 mV, preferably less than -20 mV, more preferably less than -30 mV.

[0024] Aspects of the Invention

[0025] Aspect 1: An aqueous slurry composition comprising

[0026] a) at least one polymer binder, and

[0027] b) at least one anionic oxide nanoparticle having a volume average particle size between 5 nm and 500 nm.

[0028] Aspect 2: The aqueous slurry composition according to aspect 1, wherein the anionic oxide nanoparticles comprise at least one of zinc oxide, aluminum oxide, zirconium oxide, or silicon dioxide.

[0029] Aspect 3: The aqueous slurry composition according to aspect 1 or 2, wherein the anionic oxide nanoparticles comprise anionic fumed aluminum oxide and have a volume average particle size of between 5 nm and 200 nm, preferably between 20 nm and 100 nm.

[0030] Aspect 4: The aqueous slurry composition according to any one of aspects 1 to 3, wherein the anionic oxide nanoparticles have a diameter of 15 to 600 m 2 / g, preferably 20 to 300 m 2 / g of surface area.

[0031] Aspect 5: The aqueous slurry composition according to any one of aspects 1 to 4, wherein the weight ratio of the anionic oxide nanoparticles to the polymer binder is between 5:95 and 95:5.

[0032] Aspect 6: The aqueous slurry composition according to any one of aspects 1 to 4, wherein the weight ratio of the anionic oxide nanoparticles to the polymer binder is between 15:85 and 85:15, preferably between 25:75 and 75:25.

[0033] Aspect 7: The aqueous slurry composition according to any one of aspects 1 to 6, wherein the solid content of the aqueous slurry is 10 wt % to 70 wt % based on the total weight of the aqueous slurry composition.

[0034] Aspect 8: The aqueous slurry composition according to any one of aspects 1 to 7, wherein the zeta potential of the aqueous slurry composition is anionic.

[0035] Aspect 9: The aqueous slurry composition according to any one of aspects 1 to 8, wherein the zeta potential of the aqueous slurry composition is a negative zeta potential of less than -10 mV, preferably less than -20 mV, and more preferably less than -30 mV.

[0036] Aspect 10: The aqueous slurry composition according to any one of aspects 1 to 9, wherein the viscosity is less than 20,000 cP, preferably less than 10,000 cP.

[0037] Aspect 11: The aqueous slurry composition according to any one of aspects 1 to 10, wherein the polymer binder comprises both a water-soluble polymer binder and a water-insoluble polymer binder.

[0038] Aspect 12: The aqueous slurry composition according to any one of aspects 1 to 11, wherein the polymer binder comprises at least one of SBR, an acrylic binder, a PVDF binder, or a mixture thereof.

[0039] Aspect 13: The aqueous slurry composition according to any one of aspects 1 to 12, wherein the polymer binder comprises at least one water-soluble binder selected from the group consisting of PAA, CMC, PVA, HASE and ASE, or a mixture thereof.

[0040] Aspect 14: The aqueous slurry composition of any one of aspects 1 to 13, wherein the anionic oxide nanoparticles have a fractal shape.

[0041] Aspect 15: The aqueous slurry composition according to any one of aspects 1 to 14, further comprising inorganic particles having a particle size of 1 micrometer or more.

[0042] Aspect 16: A separator for a secondary battery, comprising a coating composition comprising a) at least one polymer binder and b) at least one anionic oxide nanoparticle having a volume average particle size between 5 nm and 500 nm.

[0043] Aspect 17: The separator according to aspect 16, wherein the thickness of the coating is 0.5 to 30 micrometers, preferably 1 to 20 micrometers, and more preferably 2 to 10 micrometers.

[0044] Aspect 18: A separator for a secondary battery, comprising the composition according to any one of aspects 1 to 15 in a dry form.

[0045] Aspect 19: A separator formed from the aqueous slurry composition according to any one of aspects 1 to 15.

[0046] Aspect 20: A method for manufacturing a separator for a battery, comprising 1) providing an aqueous slurry composition, wherein the aqueous slurry composition comprises a) at least 20 weight percent of anionic oxide nanoparticles and b) up to 80 weight percent of a polymer binder, the weight percent being based on the total weight of the anionic oxide nanoparticles and the polymer binder, 2) applying the aqueous slurry composition on a substrate, and 3) drying the aqueous slurry to form a coating on the substrate.

[0047] Aspect 21: The method of aspect 20, wherein the aqueous slurry is the slurry of any one or more aspects of aspects 1 to 15.

[0048] Aspect 22: The method of aspect 20 or 21, wherein the substrate is an electrode.

[0049] Aspect 23: The method of aspect 20 or 21, wherein the substrate is a free-standing membrane.

[0050] Aspect 24: The method of any one of aspects 20, 21 or 22, wherein the aqueous slurry is applied simultaneously with the electrode slurry in a wet on wet process. DETAILED DESCRIPTION

[0051] "Copolymer" is used to refer to a polymer having two or more different monomer units. "Polymer" is used to include homopolymers and copolymers. Resin and polymer are used interchangeably. Polymers can be homogeneous, heterogeneous, and can have a gradient distribution of comonomer units. All cited references are incorporated herein by reference. As used herein, unless otherwise indicated, percentages shall refer to weight percentages.

[0052] For the purposes of the present invention, solids refer to the nanoparticles and the polymeric binder.Solids content is the weight % of solids in the aqueous slurry based on the total slurry weight.

[0053] Nanoparticles refer to oxides with a particle size of less than 500 nm, preferably less than 200 nm, and the nanoparticles may be less than 100 nm. In addition, the specific surface area of ​​the nanoparticles is higher than 15 m 2 / g, preferably higher than 20m 2 / g, more preferably higher than 30m 2 / g. Particle size is the volume average particle size measured by light scattering, Nicom or Microtech instruments.

[0054] The slurry must be castable, meaning that the slurry is homogeneous (without any aggregation) and its viscosity is less than 20,000 cP, preferably less than 10,000 cP at room temperature. Haake viscometer, shear rate at 25°C is 11 seconds.

[0055] The present invention provides an aqueous slurry composition that can be used, for example, in the coating of electrodes and / or diaphragms in electrochemical devices. The aqueous slurry composition comprises a) at least one polymer binder and b) at least one anionic oxide nanoparticle. The polymer binder is water-based. The water-based polymer includes but is not limited to PVDF, SBR or acrylic latex or water-soluble polymers such as PVA, CMC and PAA or mixtures thereof, and then adheres the anionic charged oxide particles together at each contact point.

[0056] When a water-insoluble polymer latex is used as a binder component, a water-soluble binder may also be added to the aqueous slurry composition. The water-soluble binder may act as a binder or as a thickener. For the purposes of the present invention, any polymer thickener is considered to be part of the water-soluble binder. The polymer thickener may be used alone as a binder or may be used together with another water-soluble binder or a water-insoluble binder.

[0057] The present invention also provides a coating made of an aqueous slurry composition on a substrate. The substrate can be a diaphragm or an electrode or a base substrate, and the coating is removed from the substrate to provide a film that can be applied to a desired substrate. The coating can serve as an in-situ diaphragm between an anode and a cathode in a battery, as described in US 11,133,562, the contents of which are incorporated herein by reference. The coating described herein is produced by the application of the aqueous slurry composition of the present invention.

[0058] Anionic oxide nanoparticles that can be used in the present invention include, but are not limited to, ceramics, metal oxides, and may include aluminum oxide (Al 2 O 3 ), aluminum oxide, titanium oxide (TiO2 ), silicon oxide, silicon dioxide (SiO 2 ), zirconium oxide (ZrO 2 ), zinc oxide (ZnO), silicate, kaolin, talc and mixtures thereof. Preferably, the anionic oxide nanoparticles are zinc oxide, aluminum oxide or silicon dioxide, and most preferably aluminum oxide (fumed alumina, fumed aluminum oxide) and silicon dioxide (fumed silica).

[0059] Anionic oxide nanoparticles under dilute conditions carry anionic charges, and their zeta potential is negative and less than -10 mV.

[0060] The oxide particles preferably have a diameter of 15 to 600 m 2 / g, preferably 30 to 500m 2 The nanoparticles have a high specific surface area of ​​1000 Å / g and have a surface with anionic charge. Examples of anionic oxide nanoparticles include anionic fumed alumina and fumed silica.

[0061] Some high specific surface area particles have a 3-dimensional branched structure, which can be called a fractal shape, which can lead to particles with a large aspect ratio. The fractal shape is an aggregate of primary particles with 3-dimensional branches. Preferably, the anionic oxide nanoparticles have a fractal shape.

[0062] The volume average diameter size range of the anionic oxide nanoparticles suitable for the present invention is from about 5 nm to about 500 nm, preferably from about 5 nm to about 400 nm, and most preferably from about 15 nm to about 350 nm. The particles can have a variety of shapes, such as but not limited to rectangular, spherical, fractal, elliptical, cylindrical, oval, dog bone or amorphous.

[0063] Furthermore, in some embodiments, the particles purchased from the particle manufacturer may be pre-coated with materials, for example, to enhance the compatibility of the particles with the polymer matrix, to improve the uniformity of the particles, the solubility of the particles in some parts of the polymer matrix, the dispersion of the particles in the polymer matrix, to avoid agglomeration of the particles and / or to stabilize the particles in the aqueous slurry composition.

[0064] Binder used in the present invention:

[0065] Preferred polymeric binders provide interconnectivity to the anionic oxide particles and act as a binder (or adhesive) to provide and promote adhesion between: 1) particles in the oxide particle / polymer coating, 2) coating and base substrate or porous membrane, and / or 3) coated separator and battery electrode. Good adhesion between particles can be important so that the resulting coating has physical integrity and does not flake off. Good adhesion between the anionic oxide / polymer coating and base substrate and between the coated separator and battery electrode is important to ensure adequate and optimal ion transport in the battery during charge and discharge cycles and to reduce impedance at interfaces such as boundary layers.

[0066] The polymer binders that can be used in the present invention include, but are not limited to, polyvinylidene (PVDF), polyethylene-tetrafluoroethylene (PETFE), polyvinyl fluoride (PVF), poly(alkyl) acrylates, poly(alkyl) methacrylates, polystyrene, polyvinyl alcohol (PVOH), polyacrylonitrile, polyacrylamide and copolymers thereof, and water-soluble polymers of carboxymethyl cellulose (CMC), polyacrylic acid (PAA), polymethacrylic acid (PMAA) homopolymers or copolymers thereof or mixtures thereof.

[0067] High molecular weight refers to a solution viscosity of at least 100 cp. The binder should have a high solution viscosity, i.e., measured at room temperature (25 ° C), for non-water-soluble binders, higher than 100 cp at 5% by weight in an organic solvent (NMP), or for water-soluble binders, higher than 100 cp at 2% by weight in water. Preferably, the solution viscosity is between 100 and 10,000 cp, more preferably between 100 and 5000 cp, when measured at 5% solids in NMP at room temperature. For water-soluble polymers, the viscosity is 100 cp to 10000 cp, preferably between 100 cp and 5000 cp, when measured at 2% by weight and pH 7 in water at room temperature (25 ° C). For this application, the pH can vary between 2 and 12, depending on the polymer type and application. Preferably, the Rv of the binder is at least 0.2 dl / g to a maximum of 2 dl / g.

[0068] Among fluoropolymers, PVDF has been found to be useful as a polymer binder for separator coatings, as well as in-situ coatings on the electrodes of electrolyzers, due to its excellent electrochemical tolerance and outstanding adhesion. The separator forms a barrier between the cathode and anode of the battery to prevent electronic short circuits while allowing high ion transport.

[0069] Polyvinylidene fluoride

[0070] In a preferred embodiment, the polymer is a polyvinylidene fluoride homopolymer or copolymer. The term "vinylidene fluoride polymer" (PVDF) as used herein includes homopolymers, copolymers and terpolymers within its meaning. PVDF homopolymers exhibit high solvent resistance, low swelling in battery electrolytes (less than 50%) and high melting points (greater than 150°C), thereby improving dimensional stability (shrinkage less than 10%) at high temperatures (at 100°C). PVDF copolymers are particularly preferred because they are softer - having a lower melting point ("Tm") and a reduced crystalline structure compared to homopolymers. Such copolymers include vinylidene fluoride copolymerized with at least one comonomer. The most preferred copolymers and terpolymers of the present invention are those in which the vinylidene fluoride units account for at least 50 mole percent, at least 70 mole percent, preferably at least 75 mole percent, more preferably at least 80 mole percent, and even more preferably 85 mole percent of the total weight of all monomer units in the polymer.

[0071] The PVDF used in the coating composition preferably has a melt viscosity greater than 10 kpoise, preferably greater than 20 kpoise, as measured according to ASTM method D-3835 at 230°C and 100 sec-1.

[0072] Fluorine-containing polymers such as polyvinylidene polymers are prepared by any method known in the art. Methods such as emulsion polymerization and suspension polymerization are preferred. These methods are known in the art.

[0073] Acrylic

[0074] Acrylic polymers as used herein are intended to include polymers, copolymers and terpolymers and mixtures thereof formed by methacrylate and acrylate monomers in the form of acid or ester.Methacrylate monomers and acrylate monomers can account for 51 to 100 percent of the monomer mixture, and there can be other ethylenically unsaturated monomers of 0 to 49 percent, including but not limited to styrene, α-methylstyrene, acrylonitrile, acrylamide.Suitable acrylate and methacrylate monomers and comonomers include but are not limited to methyl acrylate, ethyl acrylate and ethyl methacrylate, butyl acrylate and butyl methacrylate, isooctyl methacrylate and isooctyl methacrylate, lauryl acrylate and lauryl methacrylate, stearyl acrylate and stearyl methacrylate, isobornyl acrylate and isobornyl methacrylate, methoxyethyl acrylate and methoxyethyl methacrylate, 2-ethoxyethyl acrylate and 2-ethoxyethyl methacrylate, dimethylaminoethyl acrylate and dimethylaminoethyl methacrylate monomers.(Meth)acrylic acid such as methacrylic acid and acrylic acid can be comonomers. Acrylic polymers include multi-layer acrylic polymers such as core-shell structures typically prepared by emulsion polymerization.

[0075] Styrene

[0076] As used herein, styrene polymers are intended to include polymers, copolymers and terpolymers formed from styrene and alpha methyl styrene monomers and mixtures thereof. Styrene and alpha methyl styrene monomers may account for 50 to 100 percent of the monomer mixture, and there may be 0 to 50 percent of other ethylenically unsaturated monomers, including but not limited to acrylates, methacrylates, acrylonitrile. Styrene polymers include but are not limited to polystyrene, acrylonitrile-styrene-acrylate (ASA) copolymers, styrene acrylonitrile (SAN) copolymers, styrene-butadiene copolymers such as styrene butadiene rubber (SBR), methyl methacrylate-butadiene-styrene (MBS) and styrene-(meth) acrylate copolymers such as styrene-methyl methacrylate copolymers (S / MMA).

[0077] As used herein, polyolefins are intended to include polyethylene, polypropylene, and copolymers of ethylene and propylene. Ethylene and propylene monomers may account for 51 to 100 percent of the monomer mixture, and there may be 0 to 49 percent of other ethylenically unsaturated monomers, including but not limited to acrylates, methacrylates, acrylonitrile, anhydrides. Examples of polyolefins include ethylene ethyl acetate copolymers (EVA), ethylene (meth) acrylate copolymers, ethylene anhydride copolymers and graft polymers, propylene (meth) acrylate copolymers, acrylic anhydride copolymers and graft polymers.

[0078] Other additives:

[0079] The aqueous slurry composition of the present invention may further contain inorganic particles (P) having a particle size of about 1 micron or more as measured by SEM. The inorganic particles (P) are not particularly limited as long as they are electrochemically stable. In other words, the inorganic particles (P) that can be used in the present invention are not particularly limited as long as they are within the driving voltage range of the battery to which they are applied (e.g., based on Li / Li + 0-5V) does not undergo oxidation and / or reduction. Exemplary inorganic particles (P) include, but are not limited to, BaTiO 3 、Pb(Zr,Ti)O 3 (PZT), Pb 1-x La x Zr l-y Ti y O 3 (PLZT), PB(Mg 3 Nb 2 / 3 ) 3 —PbTiO 3 (PMN-PT), hafnium oxide (HfO 2 ), lithium phosphate (Li 3 PO 4) Lithium titanium phosphate (Li x Ti y (PO 4 ) 3 , 0 < x < 2, 0 < y < 3), lithium aluminum titanium phosphate (Li x Al y Ti z (PO 4 ) 3 , 0 < x < 2, 0 < y < 1, 0 < z < 3), (LiAlTiP) x O y type glass (0 < x < 4, 0 < y < 13) such as 14Li 2 O - 9Al 2 O 3 - 38TiO 2 - 39P 2 O 5 , lanthanum lithium titanate (Li x La y TiO 3 , 0 < x < 2, 0 < y < 3), lithium germanium thiophosphate (Li x Ge y P z S w , 0 < x < 4, 0 < y < 1, 0 < z < 1, 0 < w < 5), such as Li 3.25 Ge 0.25 P 0.75 S 4 , lithium nitride (Li x N y , 0 < x < 4, 0 < y < 2) such as Li 3 N, SiS 2 type glass (Li x Si y S z , 0 < x < 3, 0 < y < 2, 0 < z < 4) such as Li 3 PO 4 — Li 2 S — SiS 2 , P 2 S 5 type glass (Li x P y S z , 0 < x < 3, 0 < y < 3, 0 < z < 7) such as LiI — Li 2 S — P 2 S 5 , SrTiO 3 , SnO 2 , CeO 2 , MgO, NiO, CaO, ZnO, ZrO 2, Y 2 O 3 、Al 2 O 3 、TiO 2 , SiC or a mixture thereof. The preferred inorganic particles (P) include at least one of the following: BaTiO 3 、Pb(Zr,Ti)O 3 , Pb 1-x La x Zr y O 3 (0 <x<1、0<y<1)、PBMg 3 Nb 2 / 3 ) 3 、PbTiO 3 、HfO(HfO 2 ))、SrTiO 3 SnO 2 、CeO 2 、MgO、NiO、CaO、ZnO、Y 2 O 3 、Al 2 O 3 、TiO 2 、SiC、ZrO 2 , borosilicate, BaSO 4 More preferably, the inorganic particles (P) include at least one of the following: SrTiO 3 SnO 2 、CeO 2 、MgO、NiO、CaO、ZnO、Y 2 O 3 、Al 2 O 3 、TiO 2 、SiC.

[0080] The weight ratio of the inorganic particles (P) to the polymer binder in the aqueous slurry composition is between 5:95 and 95:5, preferably between 15:85 and 85:15, and more preferably between 25:75 and 75:25.

[0081] The aqueous slurry composition of the present invention may further contain effective amounts of other additives, including but not limited to fillers, leveling agents, defoamers, pH buffers, and other adjuvants that are commonly used in formulations and simultaneously meet the desired membrane requirements.

[0082] The slurry composition of the present invention may optionally have a wetting agent, a thickening agent or a rheology modifier.

[0083] Optionally, a wetting agent may be present in the slurry composition. Surfactants may act as wetting agents, but wetting agents may also include non-surfactants. The presence of an optional wetting agent allows the anionic oxide nanoparticles to be uniformly dispersed in the slurry. Useful wetting agents include, but are not limited to, ionic and non-ionic surfactants such as the TRITON series (from Dow) and the PLURONIC series (from BASF), BYK-346 (from BYK additives), and organic liquids compatible with solvents, including, but not limited to, NMP, DMSO, isopropanol, and acetone.

[0084] Thickeners and / or rheology modifiers may be present in the slurry composition. One or more thickeners or rheology modifiers may be used in an amount of 0 to 10 parts, preferably 0 to 5 parts, per 100 parts of water (parts by weight). Adding a thickener or rheology modifier to the above dispersion prevents or slows down the sedimentation of the anionic oxide nanoparticles while providing a suitable slurry viscosity for the casting process. In addition to organic rheology modifiers, inorganic rheology modifiers may also be used alone or in combination. Examples include carboxymethyl cellulose (CMC), polyacrylic acid (PAA), and alkali-swellable rheology modifiers [including alkali-swellable emulsions (ASE), hydrophobically modified alkali-swellable emulsions (HASE)], as well as other materials that provide pH-triggered rheological changes.

[0085] The solids content of the aqueous slurry composition may be 10 to 70 weight percent solids, preferably 10 to 50 weight percent, and even more preferably 10 to 35% (based on the weight of the polymer binder plus the weight of the nanoparticles).

[0086] application:

[0087] The aqueous slurry of the invention can be used, for example, to provide a coating on electrodes and / or separators in electrochemical devices. The coating is highly porous (greater than 20% by volume) and exhibits high dimensional stability (less than 10% shrinkage at 100°C) after drying.

[0088] One application of a coating made using the aqueous slurry composition of the present invention is by using aqueous PVDF latex, anionically charged nanoparticles (examples include fumed alumina, fumed silica or fumed zirconia) and PAA as a rheology modifier. The resulting coating has a porosity of 20 to 80% by volume, preferably 25 to 75% by volume and can be used as a separator in a lithium electronic battery or any other type of electrochemical device. This new coating using the aqueous slurry composition of the present invention can provide greater safety and enhanced performance, as well as reduced manufacturing costs. The porosity is measured by gravimetric analysis techniques. Not only does the resulting coating not shrink at high temperatures, but it also expands at hot spots inside the battery to further isolate runaway electrodes from each other. The response to temperature can be adjusted by the resin composition, such as changing the amount of HFP comonomer in the PVDF resin, because a film composite made from a resin with a higher HFP (i.e., 20% HFP) content swells / expands at a lower temperature than a film composite with a lower HFP (i.e., 8% HFP) content, which may require a higher temperature to obtain the same swelling / expansion. The preferred weight percentage of HFP in the copolymer of VDF is 1 to 25 weight %.

[0089] Another advantage of the aqueous slurry composition is that it can be cast simultaneously with the electrode, that is, two slurry layers (active electrode and separator layer) are cast simultaneously onto the current collector using a double-slot die-casting machine using a wet-on-wet casting technique. An integrated electrode and separator structure is subsequently formed during the drying and calendering steps. For multilayer composite structures (such as electrode separators in electrochemical devices), wet-on-wet casting is possible. When using wet-on-wet technology, the two layers are intertwined at the contact point without abrupt interfaces, resulting in better adhesion. Films or coatings can be cast simultaneously with the substrate and directly onto the substrate in a one-step wet-on-wet process.

[0090] Diaphragm

[0091] In a preferred embodiment, the aqueous slurry composition of the present invention, when dried on a substrate (thereby forming a coating), is able to withstand the harsh environment within a battery or other electrochemical device. The aqueous slurry composition can be easily processed into a coating. When the aqueous slurry composition is applied to an electrode, the resulting coating acts as a diaphragm without the need for a separate self-supporting diaphragm. The aqueous slurry composition contains anionic oxide nanoparticles. Preferably, the anionic oxide nanoparticles account for at least 20% of the weight of the coated diaphragm composite. The anionic oxide nanoparticles provide dimensional stability (minimum shrinkage) for the diaphragm. The particles may be spherical or fractal structures, but more commonly irregular shapes.

[0092] The anionic oxide nanoparticles in the aqueous slurry composition allow interstitial volume to be formed within the coating during drying, thereby serving to form micropores in the coating and maintain a physical shape as a spacer. In addition, because the anionic oxide nanoparticles are characterized in that their physical properties do not change even at high temperatures of 200° C. or higher, the coated separator using the anionic oxide particles has dimensional stability. Mixtures of anionic oxides are also contemplated.

[0093] In one embodiment, the nanoparticles may be surface treated by chemical (eg, by etching or functionalization), mechanical or radiation (eg, by plasma treatment).

[0094] The anionic oxide nanoparticles are present in the aqueous slurry composition at 5 to 95 weight percent, preferably 15 to 85 weight percent, more preferably 20 to 85 weight percent, preferably 30 to 85 weight percent, and preferably 25 to 75 weight percent, based on the total weight of the polymer and the anionic oxide nanoparticles.

[0095] The weight ratio of the anionic oxide nanoparticles to the polymer binder in the aqueous slurry composition is between 5:95 and 95:5, preferably between 15:85 and 85:15, and more preferably between 25:75 and 75:25.

[0096] Coating method

[0097] The aqueous slurry composition is applied to at least one surface of a substrate (e.g., a self-supporting diaphragm or electrode) by methods known in the art, such as by brushing, roller, inkjet, dip coating, knife, gravure, wire rod, scraper, foam applicator, curtain coating, vacuum coating, slot die or spraying. The aqueous slurry composition is then dried at room temperature or in an oven at an elevated temperature between 40 and 200° C. The drying step can be used to evaporate most or nearly all of the water initially present in the aqueous slurry composition. When the slurry composition is applied to a substrate and dried, it forms a coating on the substrate. The final dry thickness of the coating is 0.5 to 30 microns, preferably 1 to 20 microns, and more preferably 2 to 10 microns.

[0098] The aqueous slurry composition can also be cast onto a substrate, then removed from the substrate and placed on the electrode, or directly cast onto the electrode. Non-limiting examples of substrates are porous and / or microporous films, which can include any commercially available single-layer, double-layer, three-layer and / or multilayer (coextruded or laminated) porous films known to those skilled in the art. The substrate can be a polyolefin and includes, for example, polyethylene, polypropylene, or a combination thereof, including homopolymers and / or copolymers of such polyolefins.

[0099] Example

[0100] Test Method

[0101] Fumed oxides (alumina and silica). Fumed silica - average particle size 50-300nm, surface area 30-450m 2 / g. Fumed alumina, average particle size 50-300nm, surface area 30-450m 2 / g.

[0102] The zeta potential of the aqueous slurry composition is measured under dilute conditions (preferably 1% solids) using a Malvern Zetasizer.

[0103] The BET surface area, pore volume and pore size distribution of the materials were measured using a QUANTACHROME NOVA-E gas adsorption instrument. Nitrogen adsorption and desorption isotherms were generated at 77K.

[0104] General Procedure: A waterborne slurry composition was prepared using a Thinky ARE-310 mixer. Five 6.5 mm zirconium beads were added to a 125 ml Thinky jar. The fumed alumina dispersion and (1.5 wt%) aqueous CMC solution (BVH9 CMC supplied by Ashland) were added to the jar and mixed in the Thinky at 2000 rpm for 2 minutes. Acrylic latex of 2008WAL35 (acid functional copolymer of styrene and 2-ethylhexyl ester) was added to the jar and mixed at 2000 rpm for another 2 minutes. Add PVDF latex of LBG-2200LX ("LBG-2200") (provided by Arkema) was mixed at 2000 rpm for 4 minutes. PAA was purchased from Aldrich and had a molecular weight of 3,000,000 Daltons.

[0105] Depending on the application and manufacturing requirements, different slurry properties (i.e., fluidity, adhesion, etc.) are required. The aqueous slurry compositions are listed in the table below. Other components may include thickeners or dispersants / surfactants such as Pluronic or IPA.

[0106] 2008WAL35 is a water-based acrylic adhesive with a MFFT below 25°C. PP06_3 is a water-based acrylic adhesive with a MFFT below 25°C. LBG-2200LX is a PVDF binder available from Arkema SA.

[0107] In the following examples, various coated separators for use in lithium electronic batteries were formed and tested. The thickness of the separator coating was determined using a Mitutoyo digital indicator. Using the exemplary formulations, various separator thicknesses (0.5 μm to 30 μm) can be produced by adjusting the thickness of the wet coating.

[0108] The flexibility of the coated diaphragms was determined by ASTM D522 using the TQC cylindrical bend test. The coated diaphragms on aluminum foil were tested to withstand a No. 2 mandrel without breaking.

[0109] Examples of aqueous slurry compositions involving the use of anionic and cationic fumed alumina are prepared in the following table. The table shows that slurries containing high weight percentages of anionic oxide nanoparticles can be produced that exhibit excellent fluidity, reported by a Hegman fineness value of less than 5. Hegman fineness measurements were performed according to ASTM D1210-05. The comparative examples (varying the surface charge of the alumina) exhibited significantly different Hegman fineness values. It is noteworthy that cationic fumed alumina produces a large number of aggregates, with a Hegman fineness value reported as 8. In contrast, when anionic alumina is used, the measured Hegman fineness value is low (less than 5). Low Hegman fineness values ​​are necessary to ensure defect-free diaphragm coatings. The viscosity of the formulations was measured using a Haake viscometer at a shear rate of 11 seconds at 25°C. The slurries formulated using cationic oxides exhibited severe coagulation, exceeding the torque limit of the instrument. The weight percentages are based on total solids.

[0110] Table 1

[0111]

[0112]

[0113] Examples 1, 2 and 3 use anionic fumed alumina ( W-640ZX (Evonik). Examples C-4, C-5 and C-6 use cationic fumed alumina ( PG-003 (Cabot).

[0114] A Yokogawa digital resistance meter model 755601 (up to 100 MΩ) was used with a load of 60 N between two gold-plated electrodes (3 cm 2 The volume resistivity of the coated membrane was measured between the coated membrane (using Example 1) and the Celgard membrane (a commercially available membrane) by placing the membrane on top of aluminum foil and measuring the resistivity. Both membranes were non-conductive because their resistivity exceeded the measurable value of the instrument.

[0115] In Table 2, the viscosity of the formulations was measured at 25° C. using a Haake viscometer at a shear rate of 11 seconds. Examples 7, 8, 9 and 10 used Aerodisp W-640ZX (anionic fumed alumina from Evonik) as the fumed oxide. Examples 11, 12, 13 and 14 used Aerodisp W 7520 (anionic fumed silica from Evonik) as the fumed oxide.

[0116] Table 2

[0117]

[0118]

[0119] The table shows that various binders work well with either anionic silica or anionic alumina.

[0120] The viscosity of the formulations was measured using a Haake viscometer at a shear rate of 11 seconds at 25°C.

[0121] Table 3

[0122]

[0123] Examples 15 and 16 used Aerodisp W-640ZX (anionic fumed alumina from Evonik) as the fumed oxide. The alumina used in Table 3 is an inorganic particle having a particle size greater than 1 micron.

[0124] Various embodiments of the present invention have been described to achieve various purposes of the present invention. It should be appreciated that these embodiments are merely illustrations of the principles of the present invention. Many modifications and adjustments will be apparent to those skilled in the art without departing from the spirit and scope of the present invention.

Claims

1. An aqueous slurry composition comprising a) at least one polymer binder, and b) at least one anionic oxide nanoparticle having a volume average particle size between 5 nm and 500 nm.

2. The aqueous slurry composition of claim 1, wherein the anionic oxide nanoparticles comprise at least one of zinc oxide, aluminum oxide, zirconium oxide, or silicon dioxide.

3. The aqueous slurry composition of claim 1, wherein the anionic oxide nanoparticles comprise anionic fumed aluminum oxide and have a volume average particle size between 5 nm and 200 nm, preferably between 20 nm and 100 nm.

4. The aqueous slurry composition of claim 1, wherein the anionic oxide nanoparticles have a diameter of 15 to 600 m 2 / g, preferably 20 to 300m 2 / g of surface area. 5 . The aqueous slurry composition of claim 1 , wherein the weight ratio of the anionic oxide nanoparticles to the polymer binder is between 5:95 and 95:

5.

6. The aqueous slurry composition of claim 1, wherein the weight ratio of the anionic oxide nanoparticles to the polymer binder is between 15:85 and 85:15, preferably between 25:75 and 75:

25.

7. The aqueous slurry composition according to any one of claims 1 to 6, wherein the solid content of the aqueous slurry is 10 wt% to 70 wt% based on the total weight of the aqueous slurry composition.

8. The aqueous slurry composition according to any one of claims 1 to 6, wherein the zeta potential of the aqueous slurry composition is anionic.

9. The aqueous slurry composition according to any one of claims 1 to 6, wherein the zeta potential of the aqueous slurry composition is a negative zeta potential of less than -10 mV, preferably less than -20 mV, and more preferably less than -30 mV.

10. The aqueous slurry composition according to any one of claims 1 to 6, wherein the viscosity is less than 20,000 cP, preferably less than 10,000 cP.

11. The aqueous slurry composition of any one of claims 1 to 6, wherein the polymer binder comprises both a water-soluble polymer binder and a water-insoluble polymer binder.

12. The aqueous slurry composition according to any one of claims 1 to 6, wherein the polymer binder comprises at least one of SBR, an acrylic binder, a PVDF binder, or a mixture thereof.

13. The aqueous slurry composition according to any one of claims 1 to 6, wherein the polymer binder comprises at least one water-soluble binder selected from the group consisting of PAA, CMC, PVA, HASE and ASE, or a mixture thereof.

14. The aqueous slurry composition of any one of claims 1 to 6, wherein the anionic oxide nanoparticles have a fractal shape.

15. The aqueous slurry composition according to any one of claims 1 to 6, further comprising inorganic particles having a particle size of 1 micrometer or more.

16. A separator for a secondary battery, comprising a coating composition comprising a) at least one polymer binder and b) at least one anionic oxide nanoparticle having a volume average particle size between 5 nm and 500 nm. 17 . The membrane of claim 16 , wherein the coating has a thickness of 0.5 to 30 μm, preferably 1 to 20 μm, and more preferably 2 to 10 μm.

18. A separator for a secondary battery, the secondary battery comprising the composition according to any one of claims 1 to 15 in a dry form.

19. A separator formed from the aqueous slurry composition according to any one of claims 1 to 6.

20. A method for making a separator for a battery, comprising 1) providing an aqueous slurry composition comprising a) at least 5 weight percent of anionic oxide nanoparticles and b) up to 95 weight percent of a polymer binder, the weight percent being based on the total weight of the anionic oxide nanoparticles and the polymer binder, and c) optionally inorganic particles having a particle size of 1 micron or greater, 2) applying the aqueous slurry composition to a substrate, and 3) drying the aqueous slurry to form a coating on the substrate.

21. The method of claim 20, wherein the substrate is an electrode.

22. The method of claim 20, wherein the substrate is a free-standing membrane.

23. The method of claim 20, wherein the aqueous slurry is applied simultaneously with the electrode slurry in a wet-on-wet process.

24. The method of claim 20, wherein the aqueous slurry is the slurry of any one of claims 1-15.