Display panel, preparation method thereof and display device

CN119096723APending Publication Date: 2024-12-06BOE TECHNOLOGY GROUP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380008496.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The operating voltage of Tandem OLED devices increases over time, resulting in increased power consumption and shortened service life. The voltage increase of laminated OLED devices of different colors is inconsistent, affecting the display effect.

Method used

Design a display panel structure, which includes a substrate, a first electrode, at least two light-emitting functional layers and a second electrode. A first electron transport layer is provided in the light-emitting functional layer with a thickness of 3 to 10 nm. By thinning the first electron transport layer layer and adjust the doping concentration of the N-type charge generation layer to ensure that the operating voltage of stacked OLED devices of different colors tends to increase in a consistent manner over time.

Benefits of technology

It effectively reduces the problem of the operating voltage of the display panel rising over time, ensures the consistency of the operating voltage of stacked OLED devices of different colors, extends the service life and improves the display effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119096723A_ABST
    Figure CN119096723A_ABST
Patent Text Reader

Abstract

The display panel comprises a substrate, a first electrode, at least two light-emitting functional layers and a second electrode, the first electrode, the at least two light-emitting functional layers and the second electrode are sequentially stacked on one side of the substrate, in any two adjacent light-emitting functional layers, one light-emitting functional layer close to the substrate comprises a first hole transport layer, a first light-emitting layer, a first electron transport layer and an N-type charge generation layer, one light-emitting functional layer far away from the substrate comprises a P-type charge generation layer, a second hole transport layer, a second light-emitting layer and a second electron transport layer; the first hole transport layer, the first light-emitting layer, the first electron transport layer, the N-type charge generation layer, the P-type charge generation layer, the second hole transport layer, the second light-emitting layer and the second electron transport layer are sequentially stacked away from the substrate. The thickness of the first electron transport layer ranges from 3 nm to 10 nm; the first electron transport layer comprises a first sub-part, a second sub-part and a third sub-part, the thickness of the first sub-part is smaller than that of the second sub-part, and the thickness of the first sub-part is smaller than that of the third sub-part.
Need to check novelty before this filing date? Find Prior Art

Description

Display panel, manufacturing method thereof, and display device Technical Field

[0001] The embodiments of the present disclosure belong to the field of display technology, and particularly relate to a display panel, a manufacturing method thereof, and a display device. Background Art

[0002] Tandem OLED (Tandem Organic Light-Emitting Diode) devices have two or more light-emitting layers. Compared with traditional single-layer OLED devices, the current required to achieve the same brightness is smaller. The smaller current can effectively reduce the power consumption of tandem OLED devices (i.e., stacked OLED devices) and extend the service life of tandem OLED devices.

[0003] Summary of the Invention

[0004] In a first aspect, an embodiment of the present disclosure provides a display panel, comprising a substrate, a first electrode, at least two light-emitting functional layers, and a second electrode.

[0005] The first electrode, the at least two light-emitting functional layers and the second electrode are sequentially stacked on one side of the substrate;

[0006] Of any two adjacent light-emitting functional layers, the light-emitting functional layer close to the substrate includes a first hole transport layer, a first light-emitting layer, a first electron transport layer and an N-type charge generation layer, and the light-emitting functional layer far from the substrate includes a P-type charge generation layer, a second hole transport layer, a second light-emitting layer and a second electron transport layer;

[0007] The first hole transport layer, the first light-emitting layer, the first electron transport layer, the N-type charge generation layer, the P-type charge generation layer, the second hole transport layer, the second light-emitting layer and the second electron transport layer are stacked in sequence away from the substrate;

[0008] The thickness of the first electron transport layer is in the range of 3 to 10 nm;

[0009] The first light-emitting layer includes a first pattern, a second pattern and a third pattern,

[0010] The orthographic projections of the first graphic, the second graphic, and the third graphic on the substrate are spaced apart from each other, and the first graphic, the second graphic, and the third graphic emit light of different colors;

[0011] The first electron transport layer includes a first sub-portion, a second sub-portion, and a third sub-portion, wherein the orthographic projections of the first sub-portion, the second sub-portion, and the third sub-portion on the substrate are spaced apart from each other.

[0012] and the first sub-portion overlaps with the orthographic projection of the first graphic on the substrate,

[0013] The second sub-portion overlaps with the orthographic projection of the second graphic on the substrate,

[0014] The third sub-portion overlaps with the orthographic projection of the third graphic on the substrate;

[0015] The thickness of the first sub-section is smaller than the thickness of the second sub-section,

[0016] The thickness of the first sub-portion is smaller than the thickness of the third sub-portion.

[0017] In some embodiments, the first graphic emits blue light, the second graphic emits red light, and the third graphic emits green light.

[0018] The thickness of the first sub-portion ranges from 3 to 5 nm;

[0019] The thickness of the second sub-portion ranges from 5 to 10 nm;

[0020] The thickness of the third sub-portion ranges from 5 nm to 10 nm.

[0021] In some embodiments, a surface of the first sub-section facing away from the substrate, a surface of the second sub-section facing away from the substrate, and a surface of the third sub-section facing away from the substrate are flush.

[0022] In some embodiments, the first light-emitting layer includes a first pattern, a second pattern, and a third pattern.

[0023] The orthographic projections of the first graphic, the second graphic, and the third graphic on the substrate are spaced apart from each other, and the first graphic, the second graphic, and the third graphic emit light of different colors;

[0024] The N-type charge generation layer includes a first sub-portion, a second sub-portion, and a third sub-portion, wherein the orthographic projections of the first sub-portion, the second sub-portion, and the third sub-portion on the substrate are spaced apart from each other.

[0025] and the first portion overlaps with the orthographic projection of the first graphic on the substrate,

[0026] The second portion overlaps with the orthographic projection of the second graphic on the substrate,

[0027] The third portion overlaps with the orthographic projection of the third graphic on the substrate.

[0028] In some embodiments, the first graphic emits blue light, the second graphic emits red light, and the third graphic emits green light.

[0029] The doping concentration of ytterbium or lithium in the material of the first section is in the range of 5% to 10%.

[0030] The doping concentration of ytterbium or lithium in the material of the second section is in the range of 1% to 5%.

[0031] The doping concentration of ytterbium or lithium in the material of the third section is in the range of 1% to 5%.

[0032] In some embodiments, the first section, the second section, and the third section have the same thickness.

[0033] In some embodiments, surfaces of the first section, the second section, and the third section facing away from the substrate are flush.

[0034] In some embodiments, the thickness of the first pattern ranges from 20 to 30 nm.

[0035] The thickness of the second pattern ranges from 45 to 60 nm.

[0036] The thickness of the third pattern is in the range of 30 to 45 nm.

[0037] In some embodiments, including a display area,

[0038] The orthographic projection of the N-type charge generation layer on the substrate covers the display area,

[0039] The material of the N-type charge generation layer includes any two or more materials selected from triazine compounds and carbazole derivatives, and ytterbium or lithium.

[0040] In some embodiments, the doping ratio of ytterbium or lithium in the material of the N-type charge generation layer is ≤5%.

[0041] The doping ratio of the material in the carbazole derivative and the triazine compound that is better in improving the operating voltage rise of the stacked OLED device is 10% to 40%.

[0042] In some embodiments, including a display area,

[0043] The N-type charge generation layer includes a first sublayer and a second sublayer, wherein the first sublayer and the second sublayer are stacked in sequence away from the substrate.

[0044] The orthographic projections of the first sub-layer and the second sub-layer on the substrate cover the display area,

[0045] The first sub-layer and the second sub-layer are made of different materials.

[0046] In some embodiments, the material of the first sub-layer includes any one or more materials selected from triazine compounds and carbazole derivatives doped with ytterbium or lithium.

[0047] The material of the second sub-layer includes any one or more materials selected from ytterbium- or lithium-doped carbazole derivatives and triazine compounds.

[0048] In some embodiments, the doping concentration of ytterbium or lithium in the first sublayer is 1% to 3%.

[0049] The doping concentration of ytterbium or lithium in the second sublayer is 1% to 5%.

[0050] In some embodiments, including a display area,

[0051] The orthographic projection of the first electron transport layer on the substrate covers the display area,

[0052] The orthographic projection of the second hole transport layer on the substrate covers the display area,

[0053] The thickness of the second hole transport layer is in the range of 20 to 40 nm.

[0054] In some embodiments, a hole injection layer and an electron injection layer are further included.

[0055] The hole injection layer is located between the first electrode and the light-emitting functional layer closest to the substrate.

[0056] The electron injection layer is located on a side of the light-emitting functional layer that is farthest from the substrate and faces away from the substrate.

[0057] In some embodiments, the second light-emitting layer includes a fourth pattern, a fifth pattern, and a sixth pattern.

[0058] The orthographic projections of the fourth graphic, the fifth graphic, and the sixth graphic on the substrate are spaced apart from each other, and the fourth graphic, the fifth graphic, and the sixth graphic emit light of different colors;

[0059] The fourth graphic overlaps with the orthographic projection of the first graphic on the substrate and has the same luminous color.

[0060] The orthographic projections of the fifth graphic and the second graphic on the substrate overlap and have the same luminous color.

[0061] The sixth graphic overlaps with the orthographic projection of the third graphic on the substrate and emits the same luminous color.

[0062] In some embodiments, a first pixel defining layer and a second pixel defining layer are further included.

[0063] The first pixel defining layer and the first light emitting layer are provided in the same layer, and the patterns of the first pixel defining layer and the first light emitting layer are complementary;

[0064] The second pixel defining layer and the second light emitting layer are disposed on the same layer, and the patterns of the second pixel defining layer and the second light emitting layer are complementary.

[0065] In a second aspect, an embodiment of the present disclosure further provides a display device, which includes the above-mentioned display panel.

[0066] In a third aspect, the present disclosure also provides a method for manufacturing a display panel, which includes: preparing a substrate,

[0067] Sequentially preparing a first electrode, at least two light-emitting functional layers, and a second electrode on one side of the substrate;

[0068] Preparing any two adjacent light-emitting functional layers comprises sequentially preparing a light-emitting functional layer close to the substrate and a light-emitting functional layer far from the substrate;

[0069] Preparing a light-emitting functional layer close to the substrate includes: sequentially preparing a first hole transport layer, a first light-emitting layer, a first electron transport layer and an N-type charge generation layer;

[0070] Preparing the light-emitting functional layer away from the substrate includes: sequentially preparing a P-type charge generation layer, a second hole transport layer, a second light-emitting layer, and a second electron transport layer;

[0071] The thickness of the first electron transport layer is in the range of 3 to 10 nm;

[0072] Preparing the first light-emitting layer includes preparing a first pattern, a second pattern and a third pattern,

[0073] The orthographic projections of the first graphic, the second graphic, and the third graphic on the substrate are spaced apart from each other, and the first graphic, the second graphic, and the third graphic emit light of different colors;

[0074] Preparing the first electron transport layer includes preparing a first sub-section, a second sub-section and a third sub-section,

[0075] The orthographic projections of the first sub-section, the second sub-section and the third sub-section on the substrate are spaced apart from each other,

[0076] and the first sub-portion overlaps with the orthographic projection of the first graphic on the substrate,

[0077] The second sub-portion overlaps with the orthographic projection of the second graphic on the substrate,

[0078] The third sub-portion overlaps with the orthographic projection of the third graphic on the substrate;

[0079] The thickness of the first sub-section is smaller than the thickness of the second sub-section,

[0080] The thickness of the first sub-portion is smaller than the thickness of the third sub-portion.

[0081] In some embodiments, a common metal mask having one opening is used to form the first hole transport layer, the first electron transport layer, the N-type charge generation layer, the P-type charge generation layer, the second hole transport layer, and the second electron transport layer by evaporation.

[0082] The first light-emitting layer and the second light-emitting layer are formed by evaporation respectively using a fine metal mask having a plurality of openings.

[0083] In some embodiments, a common metal mask having one opening is used to form the first hole transport layer, the N-type charge generation layer, the P-type charge generation layer, the second hole transport layer, and the second electron transport layer by evaporation.

[0084] The first light-emitting layer, the first electron transport layer and the second light-emitting layer are formed by evaporation respectively using a fine metal mask having a plurality of openings.

[0085] In some embodiments, a common metal mask having one opening is used to form the first hole transport layer, the P-type charge generation layer, the second hole transport layer, and the second electron transport layer by evaporation.

[0086] Using a fine metal mask having a plurality of openings to form the first light-emitting layer, the second light-emitting layer and the N-type charge generation layer by evaporation;

[0087] The first electron transport layer is formed by evaporation using a common metal mask with one opening or a fine metal mask with multiple openings.

[0088] In some embodiments, the step of forming the first light-emitting layer by evaporation using a fine metal mask having a plurality of openings includes:

[0089] forming the first pattern of the first light-emitting layer by evaporation using a first fine metal mask;

[0090] forming the second pattern of the first light-emitting layer by evaporation using a second fine metal mask;

[0091] forming the third pattern of the first light-emitting layer by evaporation using a third fine metal mask;

[0092] The method of forming the first electron transport layer by evaporation using a fine metal mask having a plurality of openings comprises:

[0093] forming the first sub-portion of the first electron transport layer by evaporation using the first fine metal mask;

[0094] forming the second sub-portion of the first electron transport layer by evaporation using the second fine metal mask;

[0095] The third sub-portion of the first electron transport layer is formed by evaporation using the third fine metal mask.

[0096] In some embodiments, the step of forming the first light-emitting layer by evaporation using a fine metal mask having a plurality of openings includes:

[0097] forming the first pattern of the first light-emitting layer by evaporation using a first fine metal mask;

[0098] forming the second pattern of the first light-emitting layer by evaporation using a second fine metal mask;

[0099] forming the third pattern of the first light-emitting layer by evaporation using a third fine metal mask;

[0100] The method of forming the N-type charge generation layer by evaporation using a fine metal mask having a plurality of openings comprises:

[0101] forming a first portion of the N-type charge generation layer by evaporation using the first fine metal mask;

[0102] forming a second portion of the N-type charge generation layer by evaporation using the second fine metal mask;

[0103] The third portion of the N-type charge generation layer is formed by evaporation using the third fine metal mask.

[0104] In some embodiments, forming the N-type charge generation layer by evaporation includes:

[0105] By simultaneously evaporating any two or more materials selected from triazine compounds and carbazole derivatives and ytterbium or lithium materials through multiple evaporation sources, the evaporation rate of each of the evaporation sources is controlled so that the doping ratio of the carbazole derivative and the triazine compound that is superior in improving the operating voltage rise of the stacked OLED device in the formed N-type charge generation layer is 10% to 40%, and the doping ratio of the ytterbium or lithium is ≤5%.

[0106] In some embodiments, forming the N-type charge generation layer by evaporation includes:

[0107] sequentially evaporating to form a first sublayer and a second sublayer;

[0108] Forming the first sub-layer by evaporation includes:

[0109] Simultaneously evaporating any one or more materials selected from triazine compounds and carbazole derivatives and ytterbium or lithium materials through multiple evaporation sources;

[0110] Controlling the evaporation rate of each of the evaporation sources so that the doping concentration of the ytterbium or lithium in the formed first sub-layer is 1% to 3%;

[0111] Forming the second sub-layer by evaporation includes:

[0112] Simultaneously evaporating any one or more materials of carbazole derivatives and triazine compounds and ytterbium or lithium materials through multiple evaporation sources;

[0113] The evaporation rate of each of the evaporation sources is controlled so that the doping concentration of the ytterbium or lithium in the formed second sub-layer is 1% to 5%. BRIEF DESCRIPTION OF THE DRAWINGS

[0114] The accompanying drawings are used to provide a further understanding of the embodiments of the present disclosure and constitute a part of the specification. Together with the embodiments of the present disclosure, they are used to explain the present disclosure and do not constitute a limitation of the present disclosure. The above and other features and advantages will become more apparent to those skilled in the art by describing the detailed exemplary embodiments with reference to the accompanying drawings, in which:

[0115] FIG1a is a graph showing the increase in operating voltage of a stacked OLED device and a single-light-emitting-layer OLED device over time.

[0116] FIG1 b is a schematic diagram showing a curve of the operating voltage of a stacked OLED device of red, green and blue increasing with time.

[0117] FIG2 a is a schematic cross-sectional view of the structure of a display panel provided by an embodiment of the present disclosure.

[0118] FIG2 b is a graph showing the increase in the operating voltage of the display panel corresponding to different first electron transport layer thicknesses over time.

[0119] FIG2 c is a schematic diagram of another arrangement of the light-emitting layer and the pixel defining layer in an embodiment of the present disclosure.

[0120] FIG3 is a schematic cross-sectional view of the structure of another display panel provided by an embodiment of the present disclosure.

[0121] FIG4 a is a schematic cross-sectional view of the structure of another display panel provided by an embodiment of the present disclosure.

[0122] FIG4 b is a schematic cross-sectional view of the structure of another display panel provided by an embodiment of the present disclosure.

[0123] FIG4 c is a graph showing that the operating voltage of the stacked OLED device increases as the doping concentration of ytterbium in the N-type charge generation layer decreases.

[0124] FIG5 a is a comparative curve diagram of the operating voltage rise of a stacked OLED device prepared using two N-type charge generation layers of different materials.

[0125] FIG5 b is a graph showing the efficiency comparison of stacked OLED devices fabricated using N-type charge generation layers made of two different materials.

[0126] FIG6 is a schematic cross-sectional view of the structure of another display panel provided by an embodiment of the present disclosure.

[0127] FIG7 a is a schematic top view of a common metal mask.

[0128] FIG7 b is a schematic top view of a fine metal mask. DETAILED DESCRIPTION

[0129] To enable those skilled in the art to better understand the technical solutions of the embodiments of the present disclosure, a display panel, a manufacturing method thereof, and a display device provided by the embodiments of the present disclosure are further described in detail below with reference to the accompanying drawings and specific implementation methods.

[0130] The embodiments of the present disclosure will be described more fully below with reference to the accompanying drawings, but the illustrated embodiments may be embodied in different forms and should not be construed as limited to the embodiments set forth herein. Rather, these embodiments are provided so that this disclosure will be thorough and complete and will fully enable those skilled in the art to understand the scope of this disclosure.

[0131] The embodiments of the present disclosure are not limited to the embodiments shown in the drawings, but include modifications of the configurations formed based on the manufacturing process. Therefore, the regions illustrated in the drawings are schematic in nature, and the shapes of the regions shown in the drawings illustrate specific shapes of the regions, but are not intended to be limiting.

[0132] In the related art, although Tandem OLED devices (i.e., stacked OLED devices) can effectively reduce device power consumption and extend device life, since Tandem OLED devices have multiple light-emitting layers, the operating voltage of Tandem OLED devices is much higher than that of single-light-emitting-layer OLED devices. In addition, as time goes by, the operating voltage of Tandem OLED devices gradually increases, and the voltage increase is more than twice that of single-light-emitting-layer OLED devices under the same conditions (refer to Figure 1a, which is a graph of the operating voltage increase of stacked OLED devices and single-light-emitting-layer OLED devices over time).

[0133] The significant increase in operating voltage over time for tandem OLED devices not only places higher demands on the transistors in the driver backplane (i.e., the array substrate that drives the OLED device to emit light, which integrates circuitry that drives the OLED device to emit light, including components such as transistors and capacitors) but also adversely affects the reduction of device power consumption. Furthermore, the voltage increase for different color stacked OLED devices (e.g., red, green, and blue stacked OLED devices) varies. Referring to FIG1b , a schematic diagram of the time-dependent increase in operating voltage for red, green, and blue stacked OLED devices is shown. The blue stacked OLED device is the most sensitive, and therefore the time-dependent increase in operating voltage for the blue stacked OLED device is more pronounced than for the red and green stacked OLED devices. In this case, the blue stacked OLED device experiences the largest increase in operating voltage over time, resulting in the largest current reduction and blue light intensity attenuation in the blue stacked OLED device. This can cause a display panel with a red, green, and blue stacked OLED device structure to appear yellowish or greenish during operation, adversely affecting the display quality of the display panel.

[0134] In order to solve the above-mentioned problems existing in the related art, on the first aspect, an embodiment of the present disclosure provides a display panel, referring to Figure 2a, which is a structural cross-sectional schematic diagram of a display panel provided by an embodiment of the present disclosure; wherein, the display panel includes a substrate 1, a first electrode 2, at least two light-emitting functional layers and a second electrode 3, and the first electrode 2, the at least two light-emitting functional layers and the second electrode 3 are stacked in sequence on one side of the substrate 1; of any two adjacent light-emitting functional layers, the light-emitting functional layer close to the substrate 1 includes a first hole transport layer 4, a first light-emitting layer 5, a first electron transport layer 6 and an N-type charge generation layer 7, and the light-emitting functional layer away from the substrate 1 includes a P-type charge generation layer 8, a second hole transport layer 9, a second light-emitting layer 10 and a second electron transport layer 11; the first hole transport layer 4, the first light-emitting layer 5, the first electron transport layer 6, the N-type charge generation layer 7, the P-type charge generation layer 8, the second hole transport layer 9, the second light-emitting layer 10 and the second electron transport layer 11 are stacked in sequence away from the substrate 1; the thickness of the first electron transport layer 6 is in the range of 3 to 10 nm.

[0135] In some embodiments, the first light-emitting layer 5 includes a first graphic 51, a second graphic 52, and a third graphic 53, the orthographic projections of the first graphic 51, the second graphic 52, and the third graphic 53 on the substrate 1 are spaced apart from each other, and the first graphic 51, the second graphic 52, and the third graphic 53 emit light of different colors.

[0136] In some embodiments, the second light-emitting layer 10 includes a fourth figure 101, a fifth figure 102 and a sixth figure 103, and the orthographic projections of the fourth figure 101, the fifth figure 102 and the sixth figure 103 on the substrate 1 are spaced apart from each other, and the fourth figure 101, the fifth figure 102 and the sixth figure 103 emit light of different colors; the fourth figure 101 overlaps with the orthographic projection of the first figure 51 on the substrate 1 and the light-emitting color is the same, the fifth figure 102 overlaps with the orthographic projection of the second figure 52 on the substrate 1 and the light-emitting color is the same, and the sixth figure 103 overlaps with the orthographic projection of the third figure 53 on the substrate 1 and the light-emitting color is the same.

[0137] In some embodiments, the first graphic 51 , the second graphic 52 , the third graphic 53 , the fourth graphic 101 , the fifth graphic 102 , and the sixth graphic 103 are respectively made of organic electroluminescent materials.

[0138] In some embodiments, the first pattern 51 emits blue light, the second pattern 52 emits red light, and the third pattern 53 emits green light. In this embodiment, the first pattern 51, the fourth pattern 101, and other film layers in the light-emitting functional layer are stacked to form a blue stacked OLED device, the second pattern 52, the fifth pattern 102, and other film layers in the light-emitting functional layer are stacked to form a red stacked OLED device, and the third pattern 53, the sixth pattern 103, and other film layers in the light-emitting functional layer are stacked to form a green stacked OLED device.

[0139] 2b , which is a graph showing the increase in the operating voltage of the display panel over time corresponding to different thicknesses of the first electron transport layer. As can be seen from FIG2b , the four thicknesses of the first electron transport layer 6 are: thickness 1 < thickness 2 < thickness 3 < thickness 4. From the curve in FIG2b , it can be seen that appropriately thinning the thickness of the first electron transport layer 6 can effectively improve the problem of the serious increase in the operating voltage of the display panel over time.

[0140] 2 b and Table 1, Table 1 shows various performance parameters of the blue stacked OLED device with different thicknesses of the first electron transport layer.

[0141] Table 1

[0142] As can be seen from Table 1, appropriately reducing the thickness of the first electron transport layer 6 has little effect on the operating voltage, efficiency, and lifespan of the blue stacked OLED device over time. Therefore, thinning the thickness of the first electron transport layer 6 can effectively improve the problem of the blue stacked OLED device's operating voltage increasing significantly over time. Furthermore, since the operating voltage of the blue stacked OLED device increases the most over time in the related art, thinning the thickness of the first electron transport layer 6 significantly improves the operating voltage increase of the blue stacked OLED device compared to the red and green stacked OLED devices. This results in the operating voltage increase of the red, green, and blue stacked OLED devices becoming more consistent over time, thereby reducing the risk of display defects in the display panel.

[0143] In this embodiment, by making the thickness range of the first electron transport layer 6 3 to 10 nm, the thickness of the first electron transport layer 6 is thinner compared to the display panel with a stacked OLED device structure in the related art. This not only effectively improves the problem of a serious increase in the operating voltage of the display panel over time, but also reduces the difference in the increase in the operating voltage of stacked OLED devices of different colors over time without affecting the performance of the stacked OLED device as much as possible, so that the increase in the operating voltage of stacked OLED devices of different colors over time tends to be consistent, thereby reducing the risk of poor display of the display panel.

[0144] In some embodiments, the substrate 1 includes a pixel driving circuit. The pixel driving circuit can be a 3T1C (i.e., three transistors and one capacitor) structure, a 7T1C (i.e., seven transistors and one capacitor) structure, or a circuit structure including other numbers of transistors and capacitors, such as a 7T2C structure, a 6T1C structure, a 6T2C structure, or a 9T2C structure. The pixel driving circuit includes a driving transistor, the source or drain of which is electrically connected to the first electrode 2 to provide a driving current to the OLED device composed of the first electrode 2, at least two light-emitting functional layers, and the second electrode 3 stacked together.

[0145] In some embodiments, referring to FIG. 2 a , the display panel further includes a hole injection layer 12 and an electron injection layer 13 , wherein the hole injection layer 12 is located between the first electrode 2 and a light-emitting functional layer closest to the substrate 1 , and the electron injection layer 13 is located on the side of the light-emitting functional layer farthest from the substrate 1 that is away from the substrate 1 .

[0146] In some embodiments, referring to FIG. 2 a , the display panel further includes a first pixel defining layer 14 and a second pixel defining layer 15 . The first pixel defining layer 14 is provided on the same layer as the first light-emitting layer 5 , and the patterns of the first pixel defining layer 14 and the first light-emitting layer 5 are complementary. The second pixel defining layer 15 is provided on the same layer as the second light-emitting layer 10 , and the patterns of the second pixel defining layer 15 and the second light-emitting layer 10 are complementary.

[0147] In some embodiments, see Figure 2c, which is a schematic diagram of another arrangement of the light-emitting layer and the pixel defining layer in the embodiment of the present disclosure, wherein a first opening is opened in the first pixel defining layer 14, most of the first light-emitting layer 5 is located in the first opening, and the surrounding edge portions of the first light-emitting layer 5 are located on the side of the first pixel defining layer 14 away from the substrate 1, and the surrounding edge portions of the first light-emitting layer 5 overlap with the orthographic projection of the first pixel defining layer 14 on the substrate 1; a second opening is opened in the second pixel defining layer 15, most of the second light-emitting layer 10 is located in the second opening, and the surrounding edge portions of the second light-emitting layer 10 are located on the side of the second pixel defining layer 15 away from the substrate 1, and the surrounding edge portions of the second light-emitting layer 10 overlap with the orthographic projection of the second pixel defining layer 15 on the substrate 1.

[0148] In some embodiments, referring to Figure 2a, the display panel includes a display area 100, the orthographic projection of the first electron transport layer 6 on the substrate 1 covers the display area 100, the orthographic projection of the second hole transport layer 9 on the substrate 1 covers the display area 100, and the thickness of the second hole transport layer 9 ranges from 20 to 40 nm.

[0149] In this embodiment, due to the thinning of the thickness of the first electron transport layer 6, the microcavity length of the stacked OLED device in the display panel (that is, the distance between the surface of the first electrode 2 facing away from the substrate 1 and the surface of the second electrode 3 close to the substrate 1) is reduced, which will have a certain impact on the performance of the stacked OLED device (such as luminous efficiency, voltage and life). In order to solve the problem caused by the reduction of the microcavity length of the stacked OLED device, the thickness of the second hole transport layer 9 is designed to be in the range of 20 to 40 nm, so that the thickness of the second hole transport layer 9 is thicker than the thickness of the second hole transport layer in the related art, thereby compensating for the microcavity length of the stacked OLED device, thereby ensuring that the performance of the stacked OLED device is not affected.

[0150] In some embodiments, referring to Figure 3, a schematic cross-sectional view of the structure of another display panel provided in an embodiment of the present disclosure, wherein the first electron transport layer 6 includes a first sub-portion 61, a second sub-portion 62 and a third sub-portion 63, and the orthographic projections of the first sub-portion 61, the second sub-portion 62 and the third sub-portion 63 on the substrate 1 are spaced apart from each other, and the first sub-portion 61 overlaps with the orthographic projection of the first figure 51 on the substrate 1, the second sub-portion 62 overlaps with the orthographic projection of the second figure 52 on the substrate 1, and the third sub-portion 63 overlaps with the orthographic projection of the third figure 53 on the substrate 1; the thickness of the first sub-portion 61 is less than the thickness of the second sub-portion 62, and the thickness of the first sub-portion 61 is less than the thickness of the third sub-portion 63.

[0151] In some embodiments, referring to Figure 3, the first sub-portion 61 coincides with the orthographic projection of the first figure 51 on the substrate 1, the second sub-portion 62 coincides with the orthographic projection of the second figure 52 on the substrate 1, and the third sub-portion 63 coincides with the orthographic projection of the third figure 53 on the substrate 1.

[0152] In this embodiment, since the operating voltages of the red stacked OLED device, the green stacked OLED device, and the blue stacked OLED device increase at different rates over time, the first electron transport layers 6 in the stacked OLED devices of different colors are isolated from each other and the thickness of the first electron transport layers 6 in the stacked OLED devices of different colors are reduced to different degrees. This allows the operating voltages of the stacked OLED devices of different colors to increase at similar rates over time, thereby ensuring a good display effect of the display panel.

[0153] In some embodiments, the thickness of the first sub-portion 61 ranges from 3 to 5 nm; the thickness of the second sub-portion 62 ranges from 5 to 10 nm; and the thickness of the third sub-portion 63 ranges from 5 to 10 nm.

[0154] Among them, since the operating voltage of the blue stacked OLED device increases more with time than that of the red and green stacked OLED devices, the thickness of the first sub-section 61 of the blue stacked OLED device is set to be the thinnest, and the thickness of the second sub-section 62 of the red stacked OLED device and the third sub-section 63 of the green stacked OLED device are basically the same. Therefore, by setting the thickness of the first electron transport layer 6 in the different color stacked OLED devices to be thinned to different degrees, the operating voltage of the different color stacked OLED devices can be adjusted to increase more consistently with time, thereby ensuring a good display effect of the display panel.

[0155] In some embodiments, the thickness of the first pattern 51 ranges from 20 to 30 nm, the thickness of the second pattern 52 ranges from 45 to 60 nm, and the thickness of the third pattern 53 ranges from 30 to 45 nm.

[0156] Among them, since the thinning thickness of the first electron transport layer 6 of the stacked OLED devices of different colors is different, the microcavity length (that is, the distance between the surface of the first electrode 2 facing away from the substrate 1 and the surface of the second electrode 3 close to the substrate 1) of the stacked OLED devices of different colors in the display panel is reduced to different degrees, which will have a certain impact on the performance of the stacked OLED devices of different colors (such as luminous efficiency, voltage and life). In order to solve the problem caused by the reduction of the microcavity length of the stacked OLED devices of different colors, the thickness range of the first pattern 51 is designed to be 20-30nm, the thickness range of the second pattern 52 is 45-60nm, and the thickness range of the third pattern 53 is 30-45nm, so that the thickness of the different color light-emitting patterns in the first light-emitting layer 5 is thicker than the thickness of the different color light-emitting patterns in the related art, thereby compensating for the microcavity length of the stacked OLED devices of different colors, thereby ensuring that the performance of the stacked OLED devices of different colors is not affected.

[0157] 3 , the surface of the first sub-section 61 facing away from the substrate 1, the surface of the second sub-section 62 facing away from the substrate 1, and the surface of the third sub-section 63 facing away from the substrate 1 are flush. This arrangement facilitates packaging of stacked OLED devices of different colors in a display panel.

[0158] In some embodiments, referring to Figures 4a and 4b, Figure 4a is a schematic structural cross-sectional view of another display panel provided in an embodiment of the present disclosure, and Figure 4b is a schematic structural cross-sectional view of another display panel provided in an embodiment of the present disclosure, wherein the N-type charge generation layer 7 includes a first division 71, a second division 72, and a third division 73, and the orthographic projections of the first division 71, the second division 72, and the third division 73 on the substrate 1 are spaced apart from each other, and the first division 71 overlaps with the orthographic projection of the first figure 51 on the substrate 1, the second division 72 overlaps with the orthographic projection of the second figure 52 on the substrate 1, and the third division 73 overlaps with the orthographic projection of the third figure 53 on the substrate 1.

[0159] In some embodiments, referring to Figures 4a and 4b, the first division 71 coincides with the orthographic projection of the first figure 51 on the substrate 1, the second division 72 coincides with the orthographic projection of the second figure 52 on the substrate 1, and the third division 73 coincides with the orthographic projection of the third figure 53 on the substrate 1.

[0160] Currently, crosstalk between stacked OLED devices of different colors in a display panel occurs. This crosstalk is caused by the N-type charge generation layer 7 being laid out as a single layer in the display panel. Crosstalk between adjacent stacked OLED devices is easily caused by this layer. In this embodiment, crosstalk between adjacent stacked OLED devices can be resolved by dividing the N-type charge generation layer 7 into a first subsection 71, a second subsection 72, and a third subsection 73, which are spaced apart from each other.

[0161] In some embodiments, the ytterbium or lithium doping concentration in the material of the first division 71 ranges from 5% to 10%, the ytterbium or lithium doping concentration in the material of the second division 72 ranges from 1% to 5%, and the ytterbium or lithium doping concentration in the material of the third division 73 ranges from 1% to 5%.

[0162] Currently, the material forming the N-type charge generation layer 7 is typically doped with ytterbium or lithium (Yb / Li). Reducing the ytterbium or lithium doping concentration in the N-type charge generation layer 7 can reduce the leakage level of the stacked OLED device. However, this reduction in the ytterbium or lithium doping concentration can significantly increase the operating voltage of the stacked OLED device over time, thereby increasing the power consumption of the stacked OLED device. Referring to Figure 4c, a graph illustrating the increase in the operating voltage of the stacked OLED device as the ytterbium doping concentration in the N-type charge generation layer decreases is shown. In Figure 4c, the ytterbium doping concentration is Yb1 < Yb2 < Yb3 < Yb4. It can be seen that as the ytterbium doping concentration decreases, the operating voltage of the stacked OLED device increases significantly.

[0163] In this embodiment, by adjusting the ytterbium or lithium doping concentration in the material of the first section 71 to be in the range of 5% to 10%, the ytterbium or lithium doping concentration in the material of the second section 72 to be in the range of 1% to 5%, and the ytterbium or lithium doping concentration in the material of the third section 73 to be in the range of 1% to 5%, the ytterbium or lithium doping concentration in the N-type charge generation layer 7 of the different color stacked OLED devices is adjusted, so that the ytterbium or lithium doping concentration in the first section 71, the second section 72, and the third section 73 is appropriately increased compared to that in the related art. On the one hand, this ensures that the leakage level of the different color stacked OLED devices in the display panel is relatively low. On the other hand, it also makes the increase in the operating voltage of the different color stacked OLED devices over time tend to be consistent, thereby ensuring a good display effect of the display panel.

[0164] In some embodiments, the thicknesses of the first section 71, the second section 72, and the third section 73 are the same. This arrangement helps ensure the normal performance of stacked OLED devices with different colors.

[0165] In some embodiments, the surfaces of the first section 71, the second section 72, and the third section 73 facing away from the substrate 1 are flush with each other. This arrangement facilitates packaging of stacked OLED devices of different colors in a display panel.

[0166] In some embodiments, referring to FIG. 2 a , the orthographic projection of the N-type charge generation layer 7 on the substrate 1 covers the display area 100 , and the material of the N-type charge generation layer 7 includes any two or more materials of triazine compounds and carbazole derivatives, and ytterbium or lithium.

[0167] Among them, the materials selected for the N-type charge generation layer 7 are different, and the increase in the operating voltage of the stacked OLED device prepared therefrom over time will also be quite different. Referring to Figures 5a and 5b, Figure 5a is a comparative curve diagram of the operating voltage increase of the stacked OLED device prepared using two different materials for the N-type charge generation layer, and Figure 5b is a comparative curve diagram of the efficiency of the stacked OLED device prepared using two different materials for the N-type charge generation layer; it can be seen from Figure 5a that in terms of improving the operating voltage increase of the stacked OLED device, the NCGL2 material is significantly better than the NCGL1 material; it can be seen from Figure 5b that in terms of the efficiency of the stacked OLED device, the NCGL2 material is worse than the NCGL1 material.

[0168] In this embodiment, when preparing the N-type charge generation layer 7, by using any two materials of triazine compounds and carbazole derivatives, the problem of the operating voltage of the stacked OLED device increasing over time can be improved while ensuring the efficiency of the stacked OLED device.

[0169] In some embodiments, when preparing the N-type charge generation layer 7, three or more materials selected from triazine compounds and carbazole derivatives may be used, as long as the problem of the operating voltage of the stacked OLED device increasing over time can be improved while ensuring the efficiency of the stacked OLED device.

[0170] In some embodiments, the doping ratio of ytterbium or lithium in the material of the N-type charge generation layer 7 is ≤5%, and the doping ratio of the carbazole derivative and triazine compound that are particularly effective in improving the operating voltage rise of the stacked OLED device is 10% to 40%. This ytterbium or lithium doping ratio ensures low leakage in the stacked OLED device. By adjusting the ratios of two or more materials used to prepare the N-type charge generation layer 7, such that the doping ratio of the material that is particularly effective in improving the operating voltage rise of the stacked OLED device is within a range of 10% to 40%, the efficiency of the stacked OLED device can be maintained while mitigating the problem of the stacked OLED device's operating voltage rising over time.

[0171] In some embodiments, referring to Figure 6, a structural cross-sectional schematic diagram of another display panel provided in an embodiment of the present disclosure is provided; wherein, the N-type charge generation layer 7 includes a first sublayer 74 and a second sublayer 75, and the first sublayer 74 and the second sublayer 75 are stacked in sequence away from the substrate 1, and the orthographic projections of the first sublayer 74 and the second sublayer 75 on the substrate 1 cover the display area 100, and the materials of the first sublayer 74 and the second sublayer 75 are different.

[0172] In this embodiment, referring to FIG6 , compared with the display panel in FIG2 a , the two materials for preparing the N-type charge generation layer 7 are not mixed. Instead, two different materials form the first sublayer 74 and the second sublayer 75 respectively. That is, the first sublayer 74 and the second sublayer 75 together constitute the N-type charge generation layer 7. This can also ensure the efficiency of the stacked OLED device while improving the problem of the operating voltage of the stacked OLED device increasing over time.

[0173] In some embodiments, the first sublayer 74 may also include multiple sublayers of different materials, and the second sublayer 75 may also include multiple sublayers of different materials, that is, multiple sublayers of multiple materials together constitute the N-type charge generation layer 7. In this way, while ensuring the efficiency of the stacked OLED device, it can also improve the problem of the operating voltage of the stacked OLED device increasing over time.

[0174] In some embodiments, the material of the first sublayer 74 includes any one or more materials of triazine compounds and carbazole derivatives doped with ytterbium or lithium, and the material of the second sublayer 75 includes any one or more materials of carbazole derivatives and triazine compounds doped with ytterbium or lithium.

[0175] In some embodiments, the doping concentration of ytterbium or lithium in the first sublayer 74 is 1% to 3%, and the doping concentration of ytterbium or lithium in the second sublayer 75 is 1% to 5%. The doping concentrations of ytterbium or lithium in the first sublayer 74 and the second sublayer 75 can ensure a low leakage level of the stacked OLED device in the display panel.

[0176] The display panel provided in the embodiment of the present disclosure has a first electron transport layer 6 with a thickness range of 3 to 10 nm. Compared with the display panel with a stacked OLED device structure in the related art, the thickness of the first electron transport layer 6 is thinner. This not only effectively improves the problem of a serious increase in the operating voltage of the display panel over time, but also reduces the difference in the increase in the operating voltage of stacked OLED devices of different colors over time without affecting the performance of the stacked OLED device as much as possible, so that the increase in the operating voltage of stacked OLED devices of different colors over time tends to be consistent, thereby reducing the risk of poor display of the display panel.

[0177] Based on the above structure of the display panel, an embodiment of the present disclosure further provides a method for manufacturing a display panel, which includes: Step S01: preparing a substrate.

[0178] Step S02: sequentially preparing a first electrode, at least two light-emitting functional layers and a second electrode on one side of the substrate.

[0179] The preparation of any two adjacent light-emitting functional layers includes sequentially preparing a light-emitting functional layer close to the substrate and a light-emitting functional layer far from the substrate.

[0180] The preparation of a light-emitting functional layer close to the substrate includes: sequentially preparing a first hole transport layer, a first light-emitting layer, a first electron transport layer and an N-type charge generation layer. The thickness of the first electron transport layer ranges from 3 to 10 nm.

[0181] The preparation of a light-emitting functional layer away from the substrate includes: sequentially preparing a P-type charge generation layer, a second hole transport layer, a second light-emitting layer and a second electron transport layer.

[0182] In some embodiments, the method for preparing the display panel in Figure 2a includes using a common metal mask (i.e., Open Mask) having one opening to evaporate and form a first hole transport layer, a first electron transport layer, an N-type charge generation layer, a P-type charge generation layer, a second hole transport layer, and a second electron transport layer; and using a fine metal mask (i.e., FMM) having multiple openings to evaporate and form a first light-emitting layer and a second light-emitting layer.

[0183] Figure 7a shows a schematic top view of a common metal mask; the openings in the common metal mask cover the entire display area on the substrate. Figure 7b shows a schematic top view of a fine metal mask; the openings in the fine metal mask correspond to the formation area of ​​the stacked OLED device (i.e., the sub-pixel area) on the substrate.

[0184] In some embodiments, the first, second, and third patterns in the first light-emitting layer are each deposited using a single fine metal mask. The fourth, fifth, and sixth patterns in the second light-emitting layer are each deposited using a single fine metal mask. In some embodiments, the fourth, fifth, and sixth patterns in the second light-emitting layer can also be deposited using the same fine metal mask used to deposit the first, second, and third patterns in the first light-emitting layer, respectively, thereby reducing mask and production costs.

[0185] In some embodiments, the method for preparing the display panel in Figure 3 includes using an ordinary metal mask plate with one opening to evaporate and form a first hole transport layer, an N-type charge generation layer, a P-type charge generation layer, a second hole transport layer and a second electron transport layer respectively; using a fine metal mask plate with multiple openings to evaporate and form a first light-emitting layer, a first electron transport layer and a second light-emitting layer respectively.

[0186] In some embodiments, the first light-emitting layer is formed by evaporation using a fine metal mask plate having multiple openings, including: using a first fine metal mask plate to evaporate to form a first pattern of the first light-emitting layer; using a second fine metal mask plate to evaporate to form a second pattern of the first light-emitting layer; using a third fine metal mask plate to evaporate to form a third pattern of the first light-emitting layer; using a fine metal mask plate to evaporate to form a first electron transport layer, including: using the first fine metal mask plate to evaporate to form a first sub-portion of the first electron transport layer; using the second fine metal mask plate to evaporate to form a second sub-portion of the first electron transport layer; using the third fine metal mask plate to evaporate to form a third sub-portion of the first electron transport layer.

[0187] In some embodiments, the first, second, and third subsections of the first electron transport layer in FIG3 can be evaporated using the same fine metal mask used to evaporate the first, second, and third patterns of the first light-emitting layer, respectively, thereby saving mask and production costs. In some embodiments, the first subsection of the first electron transport layer in FIG3 can be evaporated using a newly fabricated fine metal mask, and the second and third subsections can be evaporated using a newly fabricated fine metal mask.

[0188] In some embodiments, the method for preparing the display panel in Figure 4a includes using an ordinary metal mask plate with one opening to evaporate and form a first hole transport layer, a P-type charge generation layer, a second hole transport layer and a second electron transport layer respectively; using a fine metal mask plate with multiple openings to evaporate and form a first light-emitting layer, a second light-emitting layer and an N-type charge generation layer respectively; using an ordinary metal mask plate with one opening to evaporate and form a first electron transport layer.

[0189] In some embodiments, the method for preparing the display panel in Figure 4b includes using an ordinary metal mask plate with one opening to evaporate and form a first hole transport layer, a P-type charge generation layer, a second hole transport layer and a second electron transport layer respectively; using a fine metal mask plate with multiple openings to evaporate and form a first light-emitting layer, a second light-emitting layer and an N-type charge generation layer respectively; using a fine metal mask plate with multiple openings to evaporate and form a first electron transport layer.

[0190] In some embodiments, a first light-emitting layer is formed by evaporation using a fine metal mask having multiple openings, including: forming a first pattern of the first light-emitting layer by evaporation using a first fine metal mask; forming a second pattern of the first light-emitting layer by evaporation using a second fine metal mask; forming a third pattern of the first light-emitting layer by evaporation using a third fine metal mask; and forming an N-type charge generation layer by evaporation using a fine metal mask having multiple openings, including: forming a first portion of the N-type charge generation layer by evaporation using the first fine metal mask; forming a second portion of the N-type charge generation layer by evaporation using the second fine metal mask; and forming a third portion of the N-type charge generation layer by evaporation using the third fine metal mask, thereby saving mask costs and production costs.

[0191] In some embodiments, in the method for preparing the display panel in Figure 2a, evaporation forms an N-type charge generation layer, including: simultaneously evaporating any two or more materials selected from triazine compounds and carbazole derivatives and ytterbium or lithium materials through multiple evaporation sources, and controlling the evaporation rate of each evaporation source so that the doping ratio of the carbazole derivative and triazine compound that is superior in improving the operating voltage rise of the stacked OLED device in the formed N-type charge generation layer is 10% to 40%, and the doping ratio of ytterbium or lithium is ≤5%.

[0192] In some embodiments, in the method for manufacturing the display panel in FIG. 6 , forming the N-type charge generation layer by evaporation includes: sequentially forming a first sublayer and a second sublayer by evaporation.

[0193] Forming the first sublayer by evaporation includes: simultaneously evaporating any one or more materials of triazine compounds and carbazole derivatives and ytterbium or lithium materials through multiple evaporation sources.

[0194] The evaporation rate of each evaporation source is controlled so that the doping concentration of ytterbium or lithium in the formed first sub-layer is 1% to 3%.

[0195] Forming the second sub-layer by evaporation includes: simultaneously evaporating any one or more materials of carbazole derivatives and triazine compounds and ytterbium or lithium materials through multiple evaporation sources.

[0196] The evaporation rate of each evaporation source is controlled so that the doping concentration of ytterbium or lithium in the formed second sub-layer is 1% to 5%.

[0197] In some embodiments, in the method for manufacturing the display panel in FIG6 , a common metal mask having one opening is used to sequentially form the first sub-layer and the second sub-layer by vapor deposition.

[0198] In some embodiments, the method for preparing a display panel further includes: after the first electrode is prepared, and before the first hole transport layer in a light-emitting functional layer closest to the substrate is prepared, a hole injection layer is formed by evaporation using a common metal mask having an opening. After the second electron transport layer in a light-emitting functional layer farthest from the substrate is prepared, and before the second electrode is prepared, an electron injection layer is formed by evaporation using a common metal mask having an opening. In some embodiments, the second electrode is formed by evaporation using a common metal mask having an opening. In some embodiments, the first electrode is prepared using a patterning process (including film deposition, exposure, development, etching, and other steps).

[0199] In some embodiments, the method for manufacturing a display panel further includes: after the first hole transport layer is prepared and before the first light-emitting layer is prepared, preparing a first pixel defining layer using an evaporation process or an exposure process (including film coating, exposure, and development steps). After the second hole transport layer is prepared and before the second light-emitting layer is prepared, preparing a second pixel defining layer using an evaporation process or an exposure process.

[0200] An embodiment of the present disclosure further provides a display device, comprising the display panel in any of the above embodiments.

[0201] By adopting the display panel of any of the above embodiments, not only can the problem of a serious increase in the operating voltage of the display device over time be effectively improved, but also, under the premise of minimizing the impact on the performance of the stacked OLED device, the difference in the increase in the operating voltage of different color stacked OLED devices in the display device over time can be reduced, so that the increase in the operating voltage of different color stacked OLED devices over time tends to be consistent, thereby reducing the risk of poor display of the display device.

[0202] The display device provided in the embodiments of the present disclosure may be any product or component with a display function, such as an OLED panel, an OLED TV, an OLED billboard, a display, a mobile phone, or a navigation system.

[0203] It is understood that the above embodiments are merely exemplary embodiments for illustrating the principles of the present disclosure, and the present disclosure is not limited thereto. Those skilled in the art may make various modifications and improvements without departing from the spirit and substance of the present disclosure, and such modifications and improvements are also considered to be within the scope of protection of the present disclosure.

Claims

1. A display panel, wherein: comprising a substrate, a first electrode, at least two light-emitting functional layers and a second electrode, The first electrode, the at least two light-emitting functional layers and the second electrode are sequentially stacked on one side of the substrate; Of any two adjacent light-emitting functional layers, the light-emitting functional layer close to the substrate includes a first hole transport layer, a first light-emitting layer, a first electron transport layer and an N-type charge generation layer, and the light-emitting functional layer far from the substrate includes a P-type charge generation layer, a second hole transport layer, a second light-emitting layer and a second electron transport layer; The first hole transport layer, the first light emitting layer, the first electron transport layer, the N-type charge generation layer, the P-type charge generation layer, the second hole transport layer, the second light emitting layer and the second electron transport layer are stacked in sequence away from the substrate; The thickness of the first electron transport layer is in the range of 3 to 10 nm; The first light-emitting layer includes a first pattern, a second pattern and a third pattern, The orthographic projections of the first graphic, the second graphic, and the third graphic on the substrate are spaced apart from each other, and the first graphic, the second graphic, and the third graphic emit light of different colors; The first electron transport layer includes a first sub-portion, a second sub-portion and a third sub-portion, and the orthographic projections of the first sub-portion, the second sub-portion and the third sub-portion on the substrate are spaced apart from each other. and the first sub-portion overlaps with the orthographic projection of the first graphic on the substrate, The second sub-portion overlaps with the orthographic projection of the second graphic on the substrate, The third sub-portion overlaps with the orthographic projection of the third figure on the substrate; The thickness of the first sub-portion is smaller than the thickness of the second sub-portion, The thickness of the first sub-portion is smaller than the thickness of the third sub-portion.

2. The display panel according to claim 1, wherein: The first pattern emits blue light, the second pattern emits red light, and the third pattern emits green light. The thickness of the first sub-section ranges from 3 to 5 nm; The thickness of the second sub-portion ranges from 5 to 10 nm; The thickness of the third sub-portion is in the range of 5 to 10 nm.

3. The display panel according to claim 2, wherein: A surface of the first sub-section facing away from the substrate, a surface of the second sub-section facing away from the substrate, and a surface of the third sub-section facing away from the substrate are flush.

4. The display panel according to any one of claims 1 to 3, wherein: The first light-emitting layer includes a first pattern, a second pattern and a third pattern, The orthographic projections of the first graphic, the second graphic, and the third graphic on the substrate are spaced apart from each other, and the first graphic, the second graphic, and the third graphic emit light of different colors; The N-type charge generation layer includes a first sub-portion, a second sub-portion and a third sub-portion, wherein the orthographic projections of the first sub-portion, the second sub-portion and the third sub-portion on the substrate are spaced apart from each other. and the first portion overlaps with the orthographic projection of the first figure on the substrate, The second portion overlaps with the orthographic projection of the second figure on the substrate, The third section overlaps with the orthographic projection of the third figure on the substrate.

5. The display panel according to claim 4, wherein: The first pattern emits blue light, the second pattern emits red light, and the third pattern emits green light. The doping concentration of ytterbium or lithium in the material of the first section is in the range of 5% to 10%. The doping concentration of ytterbium or lithium in the material of the second section is in the range of 1% to 5%. The doping concentration of ytterbium or lithium in the material of the third section is in the range of 1% to 5%.

6. The display panel according to claim 5, wherein: The first section, the second section, and the third section have the same thickness.

7. The display panel according to claim 6, wherein: Surfaces of the first section, the second section, and the third section facing away from the substrate are flush.

8. The display panel according to claim 3 or 7, wherein: The thickness of the first pattern is in the range of 20 to 30 nm. The thickness of the second pattern is in the range of 45 to 60 nm. The thickness of the third pattern is in the range of 30 to 45 nm.

9. The display panel according to claim 1, wherein: Including display area, The orthographic projection of the N-type charge generating layer on the substrate covers the display area, The material of the N-type charge generation layer includes any two or more materials of triazine compounds and carbazole derivatives and ytterbium or lithium.

10. The display panel according to claim 9, wherein: In the material of the N-type charge generation layer, the doping ratio of ytterbium or lithium is ≤5%, The doping ratio of the material which is better in improving the operating voltage rise of the stacked OLED device among the carbazole derivatives and the triazine compounds is 10% to 40%.

11. The display panel according to claim 1, wherein: Including display area, The N-type charge generation layer includes a first sublayer and a second sublayer, wherein the first sublayer and the second sublayer are sequentially stacked away from the substrate. The orthographic projections of the first sublayer and the second sublayer on the substrate cover the display district, The first sub-layer and the second sub-layer are made of different materials.

12. The display panel according to claim 11, wherein: The material of the first sublayer includes any one or more materials of triazine compounds and carbazole derivatives doped with ytterbium or lithium, The material of the second sub-layer includes any one or more materials of ytterbium- or lithium-doped carbazole derivatives and triazine compounds.

13. The display panel according to claim 12, wherein: The doping concentration of ytterbium or lithium in the first sublayer is 1% to 3%. The doping concentration of ytterbium or lithium in the second sublayer is 1% to 5%.

14. The display panel according to any one of claims 1, 9 to 13, wherein: Including display area, The orthographic projection of the first electron transport layer on the substrate covers the display area, The orthographic projection of the second hole transport layer on the substrate covers the display area, The thickness of the second hole transport layer is in the range of 20 to 40 nm.

15. The display panel according to claim 1, wherein: It also includes a hole injection layer and an electron injection layer, The hole injection layer is located between the first electrode and the light-emitting functional layer closest to the substrate. The electron injection layer is located on a side of the light-emitting functional layer that is farthest from the substrate and faces away from the substrate.

16. The display panel according to claim 1, wherein: The second light emitting layer includes a fourth pattern, a fifth pattern and a sixth pattern, The orthographic projections of the fourth figure, the fifth figure and the sixth figure on the substrate are spaced apart from each other, and the fourth figure, the fifth figure and the sixth figure emit light of different colors; The fourth graphic overlaps with the orthographic projection of the first graphic on the substrate and has the same luminous color, The orthographic projections of the fifth graphic and the second graphic on the substrate overlap and have the same luminous color, The sixth figure overlaps with the orthographic projection of the third figure on the substrate and has the same luminous color.

17. The display panel according to claim 16, wherein: Also includes a first pixel defining layer and a second pixel defining layer, The first pixel defining layer and the first light emitting layer are disposed in the same layer, and the patterns of the first pixel defining layer and the first light emitting layer are complementary; The second pixel defining layer and the second light emitting layer are disposed in the same layer, and patterns of the second pixel defining layer and the second light emitting layer are complementary.

18. A display device, wherein: A display panel comprising any one of claims 1-17.

19. A method for preparing a display panel, wherein: include: preparing the substrate, Sequentially preparing a first electrode, at least two light-emitting functional layers and a second electrode on one side of the substrate; The preparation of any two adjacent light-emitting functional layers comprises sequentially preparing a layer close to the substrate. The light-emitting functional layer and a light-emitting functional layer away from the substrate; Preparing a light-emitting functional layer close to the substrate comprises: sequentially preparing a first hole transport layer, a first light-emitting layer, a first electron transport layer and an N-type charge generation layer; Preparing a light-emitting functional layer away from the substrate comprises: sequentially preparing a P-type charge generation layer, a second hole transport layer, a second light-emitting layer, and a second electron transport layer; The thickness of the first electron transport layer is in the range of 3 to 10 nm; Preparing the first light-emitting layer includes preparing a first pattern, a second pattern and a third pattern, The orthographic projections of the first graphic, the second graphic, and the third graphic on the substrate are spaced apart from each other, and the first graphic, the second graphic, and the third graphic emit light of different colors; Preparing the first electron transport layer includes preparing a first sub-section, a second sub-section and a third sub-section, The orthographic projections of the first sub-section, the second sub-section and the third sub-section on the substrate are spaced apart from each other, and the first sub-portion overlaps with the orthographic projection of the first graphic on the substrate, The second sub-portion overlaps with the orthographic projection of the second graphic on the substrate, The third sub-portion overlaps with the orthographic projection of the third figure on the substrate; The thickness of the first sub-portion is smaller than the thickness of the second sub-portion, The thickness of the first sub-portion is smaller than the thickness of the third sub-portion.

20. The method for preparing a display panel according to claim 19, wherein: Using a common metal mask with one opening to form the first hole transport layer, the first electron transport layer, the N-type charge generation layer, the P-type charge generation layer, the second hole transport layer and the second electron transport layer by evaporation respectively; The first light-emitting layer and the second light-emitting layer are formed by evaporation respectively using a fine metal mask having a plurality of openings.

21. The method for preparing a display panel according to claim 19, wherein: Using a common metal mask with one opening to form the first hole transport layer, the N-type charge generation layer, the P-type charge generation layer, the second hole transport layer and the second electron transport layer by evaporation respectively; The first light-emitting layer, the first electron transport layer and the second light-emitting layer are formed by evaporation respectively using a fine metal mask having a plurality of openings.

22. The method for preparing a display panel according to claim 19, wherein: Using a common metal mask with one opening to form the first hole transport layer, the P-type charge generation layer, the second hole transport layer and the second electron transport layer by evaporation respectively; Using a fine metal mask having a plurality of openings to form the first light-emitting layer, the second light-emitting layer and the N-type charge generation layer by evaporation respectively; The first electron transport layer is formed by evaporation using a common metal mask having one opening or a fine metal mask having multiple openings.

23. The method for preparing a display panel according to claim 21 or 22, wherein: The method of forming the first light-emitting layer by evaporation using a fine metal mask having a plurality of openings comprises: Using a first fine metal mask to form the first pattern of the first light-emitting layer by evaporation; Using a second fine metal mask to form the second pattern of the first light-emitting layer by evaporation; Using a third fine metal mask to form the third pattern of the first light-emitting layer by evaporation; The method of forming the first electron transport layer by evaporation using a fine metal mask having a plurality of openings comprises: Using the first fine metal mask to form the first sub-portion of the first electron transport layer by evaporation; Using the second fine metal mask to form the second sub-portion of the first electron transport layer by evaporation; The third sub-portion of the first electron transport layer is formed by evaporation using the third fine metal mask.

24. The method for preparing a display panel according to claim 22, wherein: The method of forming the first light-emitting layer by evaporation using a fine metal mask having a plurality of openings comprises: Using a first fine metal mask to form the first pattern of the first light-emitting layer by evaporation; Using a second fine metal mask to form the second pattern of the first light-emitting layer by evaporation; Using a third fine metal mask to form the third pattern of the first light-emitting layer by evaporation; The method of forming the N-type charge generation layer by evaporation using a fine metal mask having a plurality of openings comprises: Using the first fine metal mask to form a first portion of the N-type charge generation layer by evaporation; Using the second fine metal mask to form a second portion of the N-type charge generation layer by evaporation; The third fine metal mask is used to form a third portion of the N-type charge generation layer by evaporation.

25. The method for preparing a display panel according to claim 20 or 21, wherein: The N-type charge generation layer is formed by evaporation, comprising: By using multiple evaporation sources to simultaneously evaporate any two or more materials of triazine compounds and carbazole derivatives and ytterbium or lithium materials, the evaporation rate of each of the evaporation sources is controlled so that the doping ratio of the carbazole derivatives and the triazine compounds in the formed N-type charge generation layer that are better in improving the operating voltage rise of the stacked OLED device is 10% to 40%, and the doping ratio of ytterbium or lithium is ≤5%.

26. The method for preparing a display panel according to claim 20 or 21, wherein: The N-type charge generation layer is formed by evaporation, comprising: Sequentially evaporating to form a first sub-layer and a second sub-layer; Forming the first sub-layer by evaporation includes: Simultaneously evaporating any one or more materials of triazine compounds and carbazole derivatives and ytterbium or lithium materials through multiple evaporation sources; Controlling the evaporation rate of each of the evaporation sources so that the doping concentration of the ytterbium or lithium in the formed first sub-layer is 1% to 3%; Forming the second sub-layer by evaporation includes: Simultaneously evaporating any one or more materials of carbazole derivatives and triazine compounds and ytterbium or lithium materials through multiple evaporation sources; The evaporation rate of each of the evaporation sources is controlled so that the doping concentration of the ytterbium or lithium in the formed second sub-layer is 1% to 5%.