A method for producing cubic boron nitride abrasive
By using Mg3N2 and LiH as catalysts and adding CaB6, TiN, and Al4C3 as additives, irregularly shaped cubic boron nitride abrasives were synthesized, solving the problem of poor self-sharpening properties of existing abrasives and achieving efficient and long-life grinding effects.
Patent Information
- Application Number
- CN202310853716.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-07-12
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2043-07-12
AI Technical Summary
Existing spherical cubic boron nitride abrasives lack sharp exposed corners, resulting in poor self-sharpening properties, which affects processing efficiency and lifespan.
Using Mg3N2 and LiH as catalysts, and adding additives CaB6, TiN and Al4C3, cubic boron nitride abrasives with irregular shapes are synthesized under high temperature and high pressure. Subsequently, they are purified by water, acid and alkali to form black irregular crystals.
It improves the self-sharpening property of abrasive, increases the grinding cutting edge, enhances grinding efficiency and lifespan, and the detached abrasive carries away heat, achieving a high-efficiency and long-life grinding effect.
Smart Images

Figure CN119347654B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of cubic boron nitride (CBN) synthesis, and specifically relates to a method for preparing cubic boron nitride abrasives. Background Technology
[0002] Cubic boron nitride possesses excellent chemical and physical properties, such as high hardness (second only to diamond), high thermal stability, and chemical inertness, as well as high hardness, high wear resistance, and a large neutron absorption cross section. Therefore, it has been widely used in processing fields of various industries and has become an indispensable material in the automotive, aerospace, mechanical electronics, and microelectronics industries. It is also an important material for improving the production efficiency of various industries.
[0003] Chinese invention patent CN110670137B discloses a method for synthesizing micronized cubic boron nitride single crystals. The method uses HBN as raw material and a mixture of Li3BN2, Li3N and NH4Cl as catalyst. The catalyst and HBN are uniformly mixed and pressed into a preform, which is then loaded into a graphite heating tube to assemble into a synthesis rod. The preform is then loaded into a pyrophyllite assembly block to form a synthesis block. Finally, the preform is subjected to high temperature and high pressure treatment to obtain cubic boron nitride crystals.
[0004] The CBN crystals synthesized by existing methods are mostly spherical in shape. This type of crystal lacks sharp corners, resulting in poor self-sharpening properties of the abrasive during grinding. Therefore, the grinding efficiency and lifespan of the grinding materials, such as high-speed steel, surface-hardened steel, cemented carbide, alloy steel, nickel-based and cobalt-based high-temperature alloys, need to be improved. Summary of the Invention
[0005] The purpose of this invention is to provide a method for preparing cubic boron nitride abrasives to solve the problem that existing spherical cubic boron nitride abrasive crystals lack sharp exposed corners, which is not conducive to improving self-sharpening properties.
[0006] To achieve the above objectives, the technical solution adopted by this invention is as follows:
[0007] A method for preparing cubic boron nitride abrasive includes the following steps: mixing raw material powder to form a preform, and then synthesizing cubic boron nitride under high temperature and high pressure; the raw material powder is composed of HBN, a catalyst and additives, the catalyst is composed of Mg3N2 and LiH, and the additives are composed of CaB6, Al4C3 and TiN.
[0008] The method for preparing cubic boron nitride abrasive of the present invention uses Mg3N2 and LiH as catalysts, and adds appropriate amounts of additives CaB6, TiN and Al4C3 to synthesize CBN. The product has an irregular crystal shape and a glossy black color. This black, irregularly shaped CBN abrasive has sharper exposed corners and higher hardness. When the abrasive grains break under stress, intergranular fracture occurs, which can generate more new sharp cutting edges on the grain grinding surface, rather than just a single one. This results in the formation of more new grinding edges. After the fine grains peel off, new cutting micro-edges are exposed, keeping the grinding efficiency at a stable level. The peeled abrasive also carries away the heat generated during grinding, achieving a higher efficiency and longer grinding life, thus making it more self-sharpening than conventional CBN abrasives.
[0009] To further improve the yield of CBN, preferably, the mass ratio of Mg3N2 to LiH in the catalyst is (5-6.5):(2.5-5). More preferably, the mass ratio of Mg3N2 to LiH in the catalyst is (5-6.5):(3.5-4).
[0010] To further promote the development of irregular crystal shapes, preferably, the mass ratio of CaB6, Al4C3, and TiN in the additive is (2-4):(2.5-5.5):(1.5-2.5). More preferably, the mass ratio of CaB6, Al4C3, and TiN in the additive is (2.5-2.7):(2.8-4):(1.5-2).
[0011] To efficiently obtain CBN abrasives with concentrated particle size and high grinding properties, preferably, the raw material powder is composed of HBN, Mg3N2, LiH, CaB6, Al4C3, and TiN in a mass ratio of (100-120):(5-6.5):(2.5-5):(2-4):(2.5-5.5):(1.5-2.5). More preferably, the raw material powder is composed of HBN, Mg3N2, LiH, CaB6, Al4C3, and TiN in a mass ratio of (105-118):(5-6.5):(3.5-4):(2.5-2.7):(2.8-4):(1.5-2).
[0012] To improve the synthesis efficiency of CBN abrasives, preferably, the high-temperature and high-pressure synthesis pressure is 90-95 MPa and the temperature is 1600-1850℃. More preferably, it is 1650-1700℃.
[0013] To better achieve product purification and improve quality, preferably, the product is crushed after high-temperature and high-pressure synthesis, and then purified sequentially using water, acid, and alkali to obtain black cubic boron nitride crystals.
[0014] Preferably, the acid purification uses a mixed acid composed of concentrated sulfuric acid and concentrated nitric acid, at a temperature of 150–180°C, for 6–8 hours. This acid purification design effectively removes relevant pickling impurities. Further optimized acid purification conditions are a temperature of 170–180°C and a time of 7–8 hours.
[0015] More preferably, the alkali purification involves boiling in industrial NaOH melt at 330–350°C for 4–6 hours. Using the above acid washing and alkali washing methods, impurities can be effectively removed, yielding black cubic boron nitride crystals. The alkali purification conditions are further preferably set at a temperature of 340–350°C for 5–6 hours. Attached Figure Description
[0016] Figure 1 This is a schematic diagram of the synthetic block structure in Embodiment 1 of the present invention; wherein, 1-conductive cap, 2-heating tube, 3-embryo, 4-pyrophyllite;
[0017] Figure 2 This is a SEM image of the black irregular cubic boron nitride crystals synthesized in Example 1 of this invention;
[0018] Figure 3 This is a morphological comparison diagram of the black CBN abrasive (3b) synthesized in Example 1 of the present invention and the conventional CBN abrasive (3a). Detailed Implementation
[0019] This invention provides a method for manufacturing a high-grinding irregular black cubic boron nitride abrasive, which uses Mg3N2 and LiH as catalysts and CaB6, TiN and Al4C3 as additives to synthesize CBN through a high temperature and high pressure process.
[0020] Specifically, the implementation scheme of the method for preparing the cubic boron nitride abrasive of the present invention is as follows:
[0021] (1) Mix the raw materials according to the following proportions: Select HBN, Mg3N2, LiH, CaB6, Al4C3, and TiN in a mass ratio of (100-120):(6.5-9):(2.5-5):(2-4):(4.5-5.5):(1.5-2.5). Mix them evenly in a sealed container for 0.5-1 hour to ensure uniform mixing. Press the mixture into a preform using a press and assemble it according to requirements for later use. The preferred mass ratio of the above raw materials is (105-118):(5-6.5):(3.5-4):(2.5-2.7):(2.8-4):(1.5-2).
[0022] like Figure 1 As shown, the conductive cap 1, heating tube 2, embryo 3, and pyrophyllite 4 are assembled into a composite block for later use.
[0023] (2) The synthetic block is loaded into the high-pressure chamber of the six-sided press and CBN is synthesized under high temperature and high pressure conditions.
[0024] During high-temperature and high-pressure synthesis, the pressure is increased to 25-35 MPa and then the temperature is introduced. The pressure is increased to 60-80 MPa and held for 3-5 minutes. During this period, the temperature is held for 0.5-2 minutes and then increased to 1600-1850℃ and held. Then the pressure is increased to the synthesis pressure of 90-95 MPa and held for 25-35 minutes before natural cooling. After natural cooling for 10-15 minutes, the pressure is released.
[0025] (3) The synthesized material is taken out, crushed, and soaked in water to remove unconverted HBN. Then, it is boiled in a mixed acid at 150-180℃ for 6-8 hours to remove impurities. Finally, it is boiled in industrial caustic soda melt at 320-350℃ for 4-6 hours. After rinsing and drying, black cubic boron nitride crystals are obtained. The mixed acid is composed of concentrated sulfuric acid with a concentration of 95-98% and concentrated nitric acid with a concentration of 63-65%, with a volume ratio of (3-4):(1-2).
[0026] (4) After acid and alkali purification, cubic boron nitride is classified by particle size and shaped to obtain black irregularly shaped cubic boron nitride finished product.
[0027] The implementation process of the present invention will be described in detail below with reference to specific embodiments. In the present invention, unless otherwise specified, "%" refers to mass percentage. In the following embodiments, the mixed acid used for acid purification is prepared by mixing concentrated sulfuric acid with a concentration of 95-98% and concentrated nitric acid with a concentration of 63-65% in a volume ratio of 3:1.
[0028] I. Specific embodiments of the preparation method of the cubic boron nitride abrasive of the present invention are as follows:
[0029] Example 1
[0030] The method for preparing cubic boron nitride abrasive in this embodiment includes the following steps:
[0031] (1) Mix 112 parts by weight of HBN powder, 6.5 parts by weight of Mg3N2, 3.5 parts by weight of LiH, 2.7 parts by weight of CaB6, 3.0 parts by weight of Al4C3 and 1.5 parts by weight of TiN in a sealed container for 0.5 hours, then press the mixture into a preform using a press, and assemble the preform into a synthetic block for later use.
[0032] (2) Load the synthetic block into the high pressure chamber of the six-sided press, pressurize to 35MPa and heat it, pressurize to 65MPa and hold for 3.5 minutes. During this period, after holding for 1 minute, heat up to 1650℃ and hold it. Then continue to pressurize to the synthetic pressure of 95MPa, hold for 25 minutes and then cool down naturally. After cooling down naturally for 10 minutes, depressurize.
[0033] (3) Take out the synthesized material, crush it, soak it in water to remove unconverted HBN, then boil it in mixed acid at 170°C for 7 hours to remove impurities, and then boil it in industrial caustic soda melt at 350°C for 5 hours. After rinsing and drying, black cubic boron nitride crystals can be obtained.
[0034] (4) After acid and alkali purification, cubic boron nitride is classified and shaped to obtain the product. The conversion rate in this embodiment is approximately 67%, of which ≥200 mesh accounts for 92%.
[0035] Example 2
[0036] The method for preparing cubic boron nitride abrasive in this embodiment includes the following steps:
[0037] (1) Mix 105 parts by weight of HBN powder, 5.5 parts by weight of Mg3N2, 4 parts by weight of LiH, 2.5 parts by weight of CaB6, 2.8 parts by weight of Al4C3 and 1.5 parts by weight of TiN in a sealed container for 0.5 hours, then press the mixture into a preform using a press, and assemble the preform into a synthetic block for later use.
[0038] (2) Load the synthetic block into the high pressure chamber of the six-sided press, pressurize to 30MPa and heat it, pressurize to 62MPa and hold for 4 minutes. During this period, after holding for 1 minute, heat up to 1650℃ and hold it. Then continue to pressurize to the synthetic pressure of 93MPa, hold for 25 minutes and then cool down naturally. After cooling down naturally for 10 minutes, depressurize.
[0039] (3) Take out the synthesized material, crush it, soak it in water to remove unconverted HBN, then boil it in mixed acid at 170°C for 7 hours to remove impurities, and then boil it in industrial caustic soda melt at 350°C for 5 hours. After rinsing and drying, black cubic boron nitride crystals can be obtained.
[0040] (4) After acid and alkali purification, cubic boron nitride is classified and shaped to obtain the product. The conversion rate in this embodiment is about 65%, of which ≥200 mesh accounts for 85%.
[0041] Example 3
[0042] The method for preparing cubic boron nitride abrasive in this embodiment includes the following steps:
[0043] (1) Mix 118 parts by weight of HBN powder, 5 parts by weight of Mg3N2, 3.5 parts by weight of LiH, 2.5 parts by weight of CaB6, 4 parts by weight of Al4C3 and 2 parts by weight of TiN in a sealed container for 0.5 hours, then press the mixture into a preform using a press, and assemble the preform into a synthetic block for later use.
[0044] (2) Load the synthetic block into the high pressure chamber of the six-sided press, pressurize to 25MPa and heat it, pressurize to 60MPa and hold for 3 minutes. During this period, after holding for 1 minute, heat up to 1650℃ and hold it. Then continue to pressurize to the synthetic pressure of 93MPa, hold for 25 minutes and then cool down naturally. After cooling down naturally for 10 minutes, depressurize.
[0045] (3) Take out the synthesized material, crush it, soak it in water to remove unconverted HBN, then boil it in mixed acid at 170°C for 7 hours to remove impurities, and then boil it in industrial caustic soda melt at 350°C for 5 hours. After rinsing and drying, black cubic boron nitride crystals can be obtained.
[0046] (4) After acid and alkali purification, cubic boron nitride is classified and shaped to obtain the product. The conversion rate in this embodiment is about 63%, of which ≥200 mesh accounts for 93%.
[0047] II. Experimental Examples
[0048] Experimental Example 1
[0049] This experimental example observes the morphology of the CBN abrasive obtained in Example 1, and the results are as follows: Figure 2 As shown.
[0050] Depend on Figure 2 It can be seen that the obtained CBN abrasive has a uniform particle size and an irregular crystal shape.
[0051] In comparison, based on Example 1, using Mg3N2 and LiH as catalysts without adding Al4C3 or CaB6, the resulting CBN abrasive is a flat, cone-shaped crystal with a smooth, flat surface and a brownish-red appearance. Based on Example 1, using Mg3N2 and LiH as catalysts with only CaB6 added, the resulting CBN abrasive exhibits octahedral or hexagonal morphology and a translucent black appearance. Based on Example 1, using Mg3N2 and LiH as catalysts with only Al4C3 added, the resulting CBN abrasive is mostly spherical, with a yellow or brownish-yellow crystal color.
[0052] Morphology comparison between the black CBN abrasive obtained in Example 1 and conventional CBN abrasive. Figure 3 As shown, Figure (3a) shows conventional CBN abrasive, and Figure (3b) shows the black CBN abrasive obtained in Example 1.
[0053] Depend on Figure 3As can be seen, compared with conventional CBN abrasives, the product of this invention has a non-spherical geometric shape, with sharper exposed corners and greater hardness. The abrasive grains fracture under stress, resulting in intergranular fracture, which generates more, rather than a single, new sharp cutting edges on the grain grinding surface, thus forming more new grinding edges. The peeling off of fine grains exposes new cutting micro-edges, keeping grinding efficiency at a stable level. The peeled abrasive also carries away the heat generated during grinding, achieving a higher efficiency and longer grinding life, thus giving it better self-sharpening properties compared to conventional CBN abrasives.
[0054] Experiment Example 2
[0055] This experiment tested the static compressive strength and thermal shock toughness of the CBN abrasives obtained in each embodiment. The thermal shock toughness was tested according to the requirements of GB / T 33144-2016 "Test Method for Impact Toughness of Superhard Abrasives". The static compressive strength was tested according to the requirements of JB / T10985-2020 "Test Method for Compressive Strength of Superhard Abrasives". The results are shown in Table 1 below.
[0056] Table 1. Test results of static compressive strength and thermal shock toughness of CBN abrasives in each embodiment.
[0057] Instance number Static pressure strength N / particle thermal shock toughness Example 1 19 22 Example 2 21 26 Example 3 23 27
[0058] As can be seen from the test results in Table 1, the CBN abrasive in the embodiment exhibits high static pressure strength and thermal shock toughness, which is beneficial for obtaining good grinding performance.
Claims
1. A method for preparing cubic boron nitride abrasive, characterized in that, Includes the following steps: The raw material powder is mixed evenly to form a blank, and then cubic boron nitride is synthesized under high temperature and high pressure. The raw material powder is composed of HBN, catalyst and additives. The catalyst is composed of Mg3N2 and LiH. The additives are composed of CaB6, Al4C3 and TiN in a mass ratio of (2~4):(2.5~5.5):(1.5~2.5). The cubic boron nitride abrasive is black and irregular in shape.
2. The method for preparing cubic boron nitride abrasive as described in claim 1, characterized in that, The mass ratio of Mg3N2 to LiH in the catalyst is (5~6.5):(2.5~5).
3. The method for preparing cubic boron nitride abrasive as described in claim 2, characterized in that, The mass ratio of Mg3N2 to LiH in the catalyst is (5~6.5):(3.5~4).
4. The method for preparing cubic boron nitride abrasive as described in claim 1, characterized in that, The mass ratio of CaB6, Al4C3, and TiN in the additive is (2.5~2.7):(2.8~4):(1.5~2).
5. The method for preparing cubic boron nitride abrasive as described in claim 1, characterized in that, The raw material powder is composed of HBN, Mg3N2, LiH, CaB6, Al4C3, and TiN in a mass ratio of (100~120): (5~6.5): (2.5~5): (2~4): (2.5~5.5): (1.5~2.5).
6. The method for preparing cubic boron nitride abrasive as described in claim 5, characterized in that, The raw material powder is composed of HBN, Mg3N2, LiH, CaB6, Al4C3, and TiN in a mass ratio of (105-118):(5~6.5):(3.5~4):(2.5~2.7):(2.8~4):(1.5~2).
7. The method for preparing cubic boron nitride abrasive as described in claim 1, characterized in that, The high-temperature and high-pressure synthesis involves a pressure of 90-95 MPa and a temperature of 1600-1850 °C.
8. The method for preparing cubic boron nitride abrasive as described in any one of claims 1 to 7, characterized in that, After being synthesized under high temperature and pressure, the crystals are crushed and then purified sequentially using water, acid, and alkali to obtain black cubic boron nitride crystals.
Citation Information
Patent Citations
A method for synthesizing micron-sized cubic boron nitride single crystals
CN110670137B
High temperature and high pressure direct synthesis method of cubic boron nitride in titanium nitride plated coating
CN103272527A
Method for preparing cubic boron nitride monocrystal micro powder by using magnesium-based compound catalyst and application of cubic boron nitride monocrystal micro powder
CN103924288A
Manufacturing method for cubic boron nitride crystals
CN104667826A