A zinc-aluminum-magnesium coated steel sheet resistant to filamentous corrosion and its preparation method
By introducing Mg-Bi compounds into zinc-aluminum-magnesium coatings and optimizing their composition and structure, the problem of filamentous corrosion in zinc-aluminum-magnesium coatings was solved, achieving high corrosion resistance and good formability of the coatings.
Patent Information
- Application Number
- CN202411846715.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-12-16
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2044-12-16
AI Technical Summary
Zinc-aluminum-magnesium coatings are prone to filamentous corrosion under certain conditions, which affects the corrosion resistance and appearance quality of the coating.
Introducing Mg-Bi compounds into zinc-aluminum-magnesium coatings controls the coating composition and microstructure, including Mg: 1%–4%, Al: 1%–4%, Bi: 0.5%–2%, and controlling the proportion of eutectic structure to form granular or ellipsoidal Mg-Bi compounds, thereby reducing the amount of Mg-Zn compounds in the eutectic structure.
It significantly improves the resistance of zinc-aluminum-magnesium coatings to filamentous corrosion, enhances the overall corrosion resistance and formability of the coating, reduces the brittleness of the coating, and improves the processing performance.
Smart Images

Figure CN119663055B_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of coating technology, and in particular to a zinc-aluminum-magnesium coated steel sheet resistant to filamentous corrosion and its preparation method. Background Technology
[0002] Hot-dip galvanizing is a process in which molten metal reacts with an iron substrate to create an alloy layer, thus bonding the substrate and the coating. Hot-dip galvanized steel has advantages such as uniform coating, strong adhesion, long service life, simple manufacturing process, and low product price, and is widely used in the manufacture of automobile bodies, home appliances, etc. To improve the protective effect of the hot-dip galvanized coating on the cut edges of the steel sheet and to improve the corrosion resistance of the surface, an appropriate amount of magnesium is added to the hot-dip galvanized coating to obtain a zinc-aluminum-magnesium coating. This further improves the corrosion resistance by more than 20%, while also providing corrosion resistance to machined cut edges.
[0003] However, the addition of magnesium to the hot-dip galvanized coating can cause filamentous corrosion under organic film in the zinc-aluminum-magnesium coating under certain conditions. This filamentous corrosion forms a corrosion morphology that extends in a specific direction, affecting the appearance quality of the organic film and, in severe cases, even the corrosion resistance of the coating. Summary of the Invention
[0004] This application provides a zinc-aluminum-magnesium coated steel sheet resistant to filamentous corrosion and its preparation method, in order to solve the following technical problem: how to improve the filamentous corrosion resistance of zinc-aluminum-magnesium coated steel sheets.
[0005] In a first aspect, embodiments of this application provide a zinc-aluminum-magnesium coated steel sheet resistant to filamentous corrosion. The coated steel sheet includes a steel substrate and a zinc-aluminum-magnesium coating attached to at least a portion of the surface of the steel substrate. The chemical composition of the zinc-aluminum-magnesium coating, by mass fraction, includes: Mg: 1%–4%, Al: 1%–4%, Bi: 0.5%–2%, and the matrix element Zn; the zinc-aluminum-magnesium coating contains Mg-Bi compounds.
[0006] Optionally, the volume fraction of the Mg-Bi compound is ≥0.05%.
[0007] Optionally, the volume fraction of the eutectic structure on the surface of the zinc-aluminum-magnesium coating is ≤20%.
[0008] Optionally, the volume fraction of the eutectic structure on the surface of the zinc-aluminum-magnesium coating is ≥70%.
[0009] Optionally, the chemical composition of the zinc-aluminum-magnesium coating satisfies: [Mg] = (2~10) × [Bi], where [Mg] represents the mass fraction of Mg and [Bi] represents the mass fraction of Bi.
[0010] Optionally, the Mg-Bi compound is in the form of granules and / or ellipsoids, and the circumscribed circle diameter of the Mg-Bi compound is 10 μm to 500 μm.
[0011] Optionally, the chemical composition of the zinc-aluminum-magnesium coating satisfies: Al+Mg≤2.5%, where Al+Mg represents the sum of the mass fractions of Al and Mg.
[0012] Optionally, the chemical composition of the zinc-aluminum-magnesium coating satisfies: Al+Mg≥5%, where Al+Mg represents the sum of the mass fractions of Al and Mg.
[0013] Secondly, embodiments of this application provide a method for preparing the zinc-aluminum-magnesium coated steel sheet resistant to filamentous corrosion as described in the first aspect, the method comprising:
[0014] The steel substrate is hot-dip coated to obtain a zinc-aluminum-magnesium coated steel sheet.
[0015] The zinc-aluminum-magnesium coated steel sheet is cooled.
[0016] Optionally, the temperature of the plating solution for hot-dip plating is 450℃~500℃.
[0017] The technical solutions provided in this application have the following advantages compared with the prior art:
[0018] This application provides a zinc-aluminum-magnesium coated steel sheet resistant to filamentous corrosion. The coated steel sheet includes a steel substrate and a zinc-aluminum-magnesium coating attached to at least a portion of the surface of the steel substrate. The chemical composition of the zinc-aluminum-magnesium coating, by mass fraction, includes: Mg: 1%–4%, Al: 1%–4%, Bi: 0.5%–2%, and the matrix element Zn; the zinc-aluminum-magnesium coating contains Mg-Bi compounds. By adding Bi to the coating, Mg-Bi compounds are formed with Mg in the coating. The Mg-Bi compounds exist in the coating in granular or ellipsoidal form. On the one hand, this consumes some magnesium, reducing the amount of eutectic Mg-Zn compounds in the coating, thereby reducing the susceptibility to filamentous corrosion; on the other hand, the Mg-Bi compounds themselves also have certain anti-corrosion properties, further enhancing the overall corrosion resistance of the coating. Attached Figure Description
[0019] The accompanying drawings, which are incorporated in and form part of this specification, illustrate embodiments consistent with this application and, together with the description, serve to explain the principles of the embodiments of this application.
[0020] To more clearly illustrate the technical solutions in the embodiments of this application or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, for those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0021] Figure 1 A schematic flowchart illustrating a method for preparing a zinc-aluminum-magnesium coated steel sheet resistant to filamentous corrosion, as provided in an embodiment of this application.
[0022] Figure 2 This is a microstructure diagram provided in Embodiment 3 of this application;
[0023] Figure 3 The microstructure diagram provided for Comparative Example 5 of this application. Detailed Implementation
[0024] To make the objectives, technical solutions, and advantages of the embodiments of this application clearer, the technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, not all embodiments. Based on the embodiments of this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application.
[0025] Various embodiments of this application may exist in the form of a range; it should be understood that the description in the form of a range is merely for convenience and brevity and should not be construed as a hard limitation on the scope of this application; therefore, it should be considered that the range description has specifically disclosed all possible sub-ranges and single numerical values within that range; for example, it should be considered that the range description from 1 to 6 has specifically disclosed sub-ranges such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., and single numbers within the range such as 1, 2, 3, 4, 5, and 6, regardless of the range; in addition, whenever a numerical range is indicated herein, it means including any referenced number (fraction or integer) within the indicated range.
[0026] In this document, terms such as “comprising” mean “including but not limited to”. Relational terms such as “first” and “second” are used only to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. “And / or” describes the relationship between related objects, indicating that there can be three relationships, for example, A and / or B can mean: A exists alone, A and B exist simultaneously, or B exists alone; where A and B can be singular or plural. “At least one” means one or more, “more” means two or more; “at least one,” “at least one of the following,” or similar expressions refer to any combination of these items, including any combination of single or plural items; for example, “at least one of a, b, or c,” or “at least one of a, b, and c,” can both mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, and c can be single or multiple. "Parts representation" such as parts by weight or parts by mass indicates the proportional relationship between components. In the proportional relationships discussed in this article, the parameters that need to be described by proportion should be understood as the first term of the proportion in the order of description, and the proportion figures should be understood as the second term of the proportion. For example, if the weight ratio of substance A, substance B, and substance C is 1:2:3, then substances A, B, and C should correspond one-to-one with the proportion figures in the proportion in the order of description, that is, the weight of substance A: the weight of substance B: the weight of substance C = 1:2:3.
[0027] Unless otherwise specified, all raw materials, reagents, instruments and equipment used in this article can be purchased from the market or prepared by existing methods.
[0028] In a first aspect, embodiments of this application provide a zinc-aluminum-magnesium coated steel sheet resistant to filamentous corrosion. The coated steel sheet includes a steel substrate and a zinc-aluminum-magnesium coating attached to at least a portion of the surface of the steel substrate. The chemical composition of the zinc-aluminum-magnesium coating, by mass fraction, includes: Mg: 1%–4%, Al: 1%–4%, Bi: 0.5%–2%, and the matrix element Zn; the zinc-aluminum-magnesium coating contains Mg-Bi compounds.
[0029] The zinc-aluminum-magnesium coated steel sheet of this application includes a steel substrate and a zinc-aluminum-magnesium coating attached to at least a portion of the surface of the steel substrate. There are no particular limitations on the steel substrate; ordinary steel sheets such as hot-rolled steel sheets and cold-rolled steel sheets can be used. There are also no particular limitations on the type of steel; for example, aluminum-killed steel, ultra-low carbon steel, and high-strength steel can be used.
[0030] Magnesium oxide (Mg) is one of the key elements in zinc-aluminum-magnesium (ZAMg) coatings that enhance atmospheric corrosion resistance. When the mass fraction of Mg is between 1% and 4%, the Mg in the coating preferentially dissolves into the water film on the coating surface in the atmosphere, reacts with dissolved carbon dioxide, and precipitates a dense protective film. This protective film is stable in neutral and weakly alkaline environments, thus significantly improving the corrosion resistance of the coating, especially in high-humidity atmospheric environments, where the protective effect of Mg is particularly pronounced. In the deep-drawing process of ZAMg-coated automotive steel sheets, the brittleness of the coating is a critical concern. Excessively high or low Mg mass fractions can increase coating brittleness, thus affecting the processing performance of the automotive steel sheets. When the Mg mass fraction is controlled between 1% and 4%, the strength and toughness of the coating can be effectively balanced, ensuring good processing performance while meeting corrosion resistance requirements. This helps reduce cracking and peeling of the coating during processing, improving the yield and quality of the automotive steel sheets. For example, the mass fraction of Mg in the coating can be: 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, etc.
[0031] In corrosive environments, Al can form a dense protective film of oxides and hydroxides on the coating surface. This protective film has high stability and density, effectively isolating corrosive media such as oxygen, moisture, and carbon dioxide, thereby slowing down or preventing corrosion. When the mass fraction of Al is in the range of 1% to 4%, it ensures the formation of a sufficient quantity and quality of protective film while avoiding other negative effects that may result from excessive Al content. Secondly, the addition of 1% to 4% Al also helps improve the adhesion between the coating and the steel substrate. If the mass fraction of Al in the coating is too low, the adhesion between the coating and the steel plate may be poor, leading to peeling or detachment of the coating during processing or use, thus reducing the corrosion resistance of the coating. In addition, limiting the mass fraction of Al to the range of 1% to 4% also helps control the physical and processing properties of the coating. Within this range, the physical properties of the coating, such as hardness, toughness, and ductility, are well balanced. This not only ensures that the coating maintains good formability during processing but also reduces defects such as cracks and fractures that occur during deep processing. Meanwhile, 1% to 4% Al helps improve the fatigue resistance of the coating and extend its service life. However, it is worth noting that although Al has positive effects on the corrosion resistance, adhesion, and physical properties of the coating, if the content exceeds 4%, it may lead to the formation of excessive aluminum-rich phases in the coating. These phases are prone to causing cracking and peeling during processing. Therefore, limiting the mass fraction of Al to the range of 1% to 4% can fully utilize its positive effects while avoiding its potential negative impacts. For example, the mass fraction of Al in the coating can be: 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, etc.
[0032] The addition of bismuth can form Mg-Bi compounds with Mg in the coating. The presence of these compounds effectively consumes some of the magnesium, thereby reducing the amount of Mg-Zn compounds in the eutectic structure. Eutectic structures, especially Mg-Zn compounds, readily dissolve in acidic environments, leading to filamentary corrosion. Therefore, the formation of Mg-Bi compounds is an effective corrosion protection mechanism, reducing the risk of filamentary corrosion. The amount of bismuth added has a significant impact on the overall performance of the coating. If the mass fraction of bismuth exceeds 2%, it results in the formation of large, bulky Mg-Bi compounds instead of granular structures, which greatly impairs the coating's resistance to filamentary corrosion. Furthermore, a bismuth mass fraction exceeding 2% also increases the brittleness of the coating, reducing its formability. In addition, a bismuth mass fraction exceeding 2% leads to significant galvanic corrosion in the coating, significantly reducing its corrosion resistance. Therefore, limiting the bismuth mass fraction to between 0.5% and 2% ensures both corrosion resistance and good formability and toughness. For example, the mass fraction of Bi in the coating can be: 0.5%, 0.8%, 1.1%, 1.4%, 1.7%, 2%, etc.
[0033] Zn is a matrix element, and the specific content / range of Zn can be obtained through the upper and lower limit formulas of the component, that is:
[0034] The sum of the percentages of all components in a composition shall be equal to 100%, and the content ranges of several components shall meet the following conditions: the upper limit of a certain component + the lower limit of other components ≤ 100; the lower limit of a certain component + the upper limit of other components ≥ 100.
[0035] In some embodiments, the volume fraction of the Mg-Bi compound is ≥0.05%.
[0036] Filament corrosion is a form of localized corrosion that can occur in zinc-aluminum-magnesium (ZAMg) coatings under specific environments (such as acidic environments). It leads to gradual coating failure, ultimately affecting the overall performance of the automotive body panels. The formation of Mg-Bi compounds can consume some of the Mg element in the coating, reducing the content of Mg-Zn compounds in the eutectic structure. Since the eutectic structure is a prone area for filament corrosion, reducing the proportion of Mg-Zn compounds helps to reduce the risk of filament corrosion. By limiting the volume fraction of Mg-Bi compounds to ≥0.05%, a sufficient amount of Mg-Bi compounds can be ensured to form, thereby effectively inhibiting the occurrence of filament corrosion.
[0037] In some embodiments, the volume fraction of the eutectic structure on the surface of the zinc-aluminum-magnesium coating is ≤20%.
[0038] In some embodiments, the volume fraction of the eutectic structure on the surface of the zinc-aluminum-magnesium coating is ≥70%.
[0039] Eutectic structures are classified into ternary eutectic structures and binary eutectic structures. In zinc-aluminum-magnesium (ZAM) coatings, Mg is mainly concentrated in the eutectic structure. The ternary eutectic structure includes aluminum-rich phases, zinc-rich phases, and magnesium-zinc compounds, such as Mg₂Zn. 11 Magnesium-zinc oxide (Mg-Zn2), etc., are used in binary eutectic structures, which typically contain only magnesium-zinc compounds and zinc-rich or aluminum-rich phases. In acidic environments, Mg-Zn compounds in the eutectic structure preferentially dissolve. As the eutectic structure dissolves, acid radicals combine with magnesium to form compounds with low solubility that precipitate out. If this reaction occurs under an organic film, the location of acid dissolution and the location of precipitated compounds are not the same, resulting in filamentous corrosion. To suppress this filamentous corrosion, the most effective method is to eliminate the acidic environment. For eutectic structures, zinc-aluminum-magnesium (ZAM) coatings are difficult to completely eliminate because the addition of aluminum and magnesium will form a eutectic structure. Since eutectic structures are prone to localized corrosion in acidic environments, which can then evolve into filamentous corrosion, reducing the proportion of eutectic structures is beneficial. In the embodiments of this application, the proportion of eutectic structures in the coating can be controlled to below 20%. For example, the volume fraction of the eutectic structure on the surface of the zinc-aluminum-magnesium coating can be 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, etc.
[0040] However, if the eutectic structure content is high, although localized corrosion is more likely to occur, it will not evolve into filamentary corrosion. Therefore, further increasing the proportion of eutectic structure is also beneficial. Studies have found that if the proportion of eutectic structure in the coating is not less than 70%, the possibility of filamentary corrosion is also very low. For example, the volume fraction of eutectic structure on the surface of zinc-aluminum-magnesium coatings can be 70%, 72%, 74%, 76%, 78%, 80%, 82%, 84%, 86%, 88%, 90%, etc.
[0041] In some embodiments, the chemical composition of the zinc-aluminum-magnesium coating satisfies: [Mg] = (2~10) × [Bi], where [Mg] represents the mass fraction of Mg and [Bi] represents the mass fraction of Bi.
[0042] The purpose of adding Bi is to obtain Mg-Bi compounds. Therefore, there should be a certain relationship between the contents of Mg and Bi so that Mg and Bi can be formed to the maximum extent. Thus, the amount of Bi added should be one-tenth to one-half of that of Mg.
[0043] In some embodiments, the Mg-Bi compound is in the form of granules and / or ellipsoids, and the circumscribed circle diameter of the Mg-Bi compound is 10 μm to 500 μm.
[0044] The morphology and size of Mg-Bi compounds are crucial to their corrosion protection effect. When the mass fraction of bismuth is controlled between 0.5% and 2%, granular or ellipsoidal Mg-Bi compounds can be formed. If the Mg-Bi compounds are too small, they cannot effectively prevent the spread of filamentous corrosion. However, if the Mg-Bi compounds are too large, the coating becomes more brittle, making it prone to cracking and peeling during deep drawing of automotive panels. Therefore, the outer circle diameter of the Mg-Bi compound is limited to between 10 μm and 500 μm. Mg-Bi compounds of this size can effectively prevent the spread of filamentous corrosion without making the coating too brittle, thus avoiding the problems of coating cracking and peeling during deep drawing. For example, the outer circle diameter of the Mg-Bi compound can be 10 μm, 50 μm, 100 μm, 150 μm, 200 μm, 250 μm, 300 μm, 350 μm, 400 μm, 450 μm, 500 μm, etc.
[0045] In some embodiments, the chemical composition of the zinc-aluminum-magnesium coating satisfies: Al+Mg≤2.5%, where Al+Mg represents the sum of the mass fractions of Al and Mg.
[0046] To control the proportion of eutectic structure in the coating to ≤20%, the sum of Al and Mg content in the coating needs to be controlled to ≤2.5%, and of course, the Al and Mg content cannot be less than 1%. For example, the sum of the mass fractions of Al and Mg in the coating can be 2.0%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, etc.
[0047] In some embodiments, the chemical composition of the zinc-aluminum-magnesium coating satisfies: Al+Mg≥5%, where Al+Mg represents the sum of the mass fractions of Al and Mg.
[0048] To control the eutectic structure in the coating to ≥70%, the sum of Al and Mg content in the coating needs to be controlled to 5% or more, while the combined Al and Mg content cannot exceed 4%. For example, the sum of the mass fractions of Al and Mg in the coating can be 5.5%, 6%, 6.5%, 7%, 7.5%, 8%, etc.
[0049] In summary, the embodiments of this application provide a zinc-aluminum-magnesium coated steel sheet resistant to filamentous corrosion, which has the following technical advantages:
[0050] This zinc-aluminum-magnesium coated steel sheet, resistant to filamentous corrosion, boasts excellent corrosion resistance, hardness, and wear resistance, making it widely applicable in various fields such as construction, automobiles, and home appliances. Especially in environments requiring high corrosion resistance, such as coastal areas and industrial zones, this coated steel sheet will exhibit even more outstanding performance advantages.
[0051] The zinc-aluminum-magnesium coated steel sheet resistant to filamentous corrosion provided in this application significantly improves the coating's resistance to filamentous corrosion by introducing Mg-Bi compounds and optimizing the coating composition and structure. This innovative achievement represents a new breakthrough in the field of coating technology and provides related industries with higher-quality, higher-performance material options.
[0052] Figure 1 This is a schematic flowchart illustrating a method for preparing a zinc-aluminum-magnesium coated steel sheet resistant to filamentous corrosion, as provided in an embodiment of this application.
[0053] Please see Figure 1 Secondly, embodiments of this application provide a method for preparing the zinc-aluminum-magnesium coated steel sheet resistant to filamentous corrosion as described in the first aspect, the method comprising:
[0054] The steel substrate is hot-dip coated to obtain a zinc-aluminum-magnesium coated steel sheet.
[0055] The zinc-aluminum-magnesium coated steel sheet is cooled.
[0056] In some embodiments, the temperature of the plating solution for hot-dip plating is 450°C to 500°C.
[0057] In hot-dip galvanizing, the temperature of the plating bath has a significant impact on the microstructure and properties of the coating. When the bath temperature is too low, it becomes difficult for Mg-Bi compounds to form in the coating; conversely, when the temperature is too high, coarse, blocky Mg-Bi phases form. The large size of these Mg-Bi phases weakens the corrosion protection effect and also leads to brittleness in the coating. Therefore, hot-dip galvanizing should be performed at a bath temperature of 450℃ to 500℃ to ensure that the content and morphology of Mg-Bi compounds in the coating are optimal, thereby improving the quality and performance of the coating. Examples of suitable bath temperatures include 450℃, 460℃, 470℃, 480℃, 490℃, and 500℃.
[0058] The product prepared by the method for preparing the zinc-aluminum-magnesium coated steel sheet resistant to filamentous corrosion is the aforementioned zinc-aluminum-magnesium coated steel sheet resistant to filamentous corrosion. Since the method for preparing the zinc-aluminum-magnesium coated steel sheet resistant to filamentous corrosion adopts some or all of the technical solutions of the zinc-aluminum-magnesium coated steel sheet resistant to filamentous corrosion, it has at least all the beneficial effects brought about by the technical solution of the zinc-aluminum-magnesium coated steel sheet resistant to filamentous corrosion, which will not be elaborated here.
[0059] The present application is further illustrated below with reference to specific embodiments. Experimental methods in the following embodiments that do not specify specific conditions are generally determined according to national / industry standards; if there is no corresponding national / industry standard, they are performed according to general international standards, conventional conditions, or conditions recommended by the manufacturer.
[0060] A steel plate with a thickness of 1.0 mm and a width of 1500 mm was used as the substrate, and the coating weight was 100 grams per square meter on both sides. The features of embodiments 1-13 and comparative examples 1-5 are shown in Table 1.
[0061] Table 1
[0062]
[0063] The preparation process conditions of Examples 1-13 and Comparative Examples 1-5 of the present invention are shown in Table 2.
[0064] The zinc-aluminum-magnesium coated steel sheets prepared in Examples 1-13 and Comparative Examples 1-5 were subjected to an evaluation experiment on resistance to filamentous corrosion. A 20-micron-thick PVB organic film was coated on the zinc-aluminum-magnesium coating surface. Then, scratches were made on the surface of the organic film, with a scratch width of 1 mm and a scratch depth reaching the steel substrate. 5 μL of acetic acid solution with a pH of 3 was injected into the scratch location. The samples were then placed in a constant temperature and humidity environment (40℃, 86% RH) and stored for 4 weeks. The maximum length of filamentous corrosion on the sample surface was then evaluated according to GB / T 30789.9. The longer the corrosion wire, the more likely filamentous corrosion will occur. If the length of the filamentous corrosion is no more than 2 mm, the resistance to filamentous corrosion is excellent (□). If the length of the filamentous corrosion is more than 2 mm but less than 4 mm, the resistance to filamentous corrosion is good (▲). If the length of the filamentous corrosion is more than 4 mm, the resistance to filamentous corrosion is poor (×).
[0065] The zinc-aluminum-magnesium coated steel sheets prepared in Examples 1-13 and Comparative Examples 1-5 were evaluated for coating brittleness: the samples were bent 180° using a bending method, and the occurrence of coating cracking and peeling at the bending location was observed. If coating cracking or peeling occurred at the bending location, the coating brittleness was considered poor (×); otherwise, the coating brittleness was considered excellent (□).
[0066] Neutral salt spray tests were conducted on the zinc-aluminum-magnesium coated steel sheets prepared in Examples 1-13 and Comparative Examples 1-5. The average thickness of the coating before corrosion and the average thickness of the coating after corrosion were measured, the difference between the two was calculated, and then divided by the corrosion time to obtain the average corrosion rate of the coating.
[0067] Average corrosion rate = (average coating thickness before corrosion - average coating thickness after corrosion) / corrosion time (μm / h).
[0068] If the average corrosion rate of the coating does not exceed 0.03 micrometers / hour, the coating has excellent corrosion resistance (□); if the average corrosion rate of the coating exceeds 0.03 micrometers / hour, the coating has poor corrosion resistance (×).
[0069] The experimental evaluation results are shown in Table 2.
[0070] Table 2
[0071] Group Plating solution temperature / ℃ Coating resistance to filamentous corrosion Coating corrosion resistance Coating brittleness Example 1 500 ▲ Example 2 480 Example 3 480 Example 4 450 Example 5 460 Example 6 460 Example 7 480 Example 8 470 Example 9 480 Example 10 460 Example 11 500 Example 12 500 Example 13 490 Comparative Example 1 430 × × × Comparative Example 2 410 × × × Comparative Example 3 540 × Comparative Example 4 580 × × × Comparative Example 5 510 ×
[0072] As shown in Tables 1-2, in Examples 1-13, the chemical composition and characteristics of the zinc-aluminum-magnesium coating are all within the required range of the present invention, and the corrosion resistance is good.
[0073] Appendix Figure 2-3 Detailed explanation:
[0074] Figure 2 This is a microstructure diagram provided in Embodiment 3 of this application; as follows: Figure 2 As shown, the bright white dots are compounds formed by Mg and Bi, the light gray ones are the Zn phase, and the rest are eutectic structures.
[0075] Figure 3 This is a microstructure diagram provided in Comparative Example 5 of the embodiments of this application; as shown Figure 3 As shown, the light gray area represents the Zn phase, while the rest represents the eutectic structure.
[0076] One or more technical solutions in the embodiments of the present invention have at least the following technical effects or advantages:
[0077] The method for preparing zinc-aluminum-magnesium coated steel sheets provided in this invention is simple to operate, has low production cost, and is easy to promote and use.
[0078] The above description is merely a specific embodiment of this application, enabling those skilled in the art to understand or implement this application. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of this application. Therefore, this application is not to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features claimed in this application.
Claims
1. A zinc-aluminum-magnesium coated steel sheet resistant to filamentous corrosion, the coated steel sheet comprising a steel substrate and a zinc-aluminum-magnesium coating attached to at least a portion of the surface of the steel substrate; The chemical composition of the zinc-aluminum-magnesium coating, by mass fraction, is: Al: 1.5%, Mg: 1%, Bi: 0.5%, and the base element Zn; The zinc-aluminum-magnesium coating contains a Mg-Bi compound, which is in particulate form, has a volume fraction of 0.08%, and a circumscribed circle diameter of 100 μm. The volume fraction of the eutectic structure on the surface of the zinc-aluminum-magnesium coating is 15%. The method for preparing the zinc-aluminum-magnesium coated steel sheet resistant to filamentous corrosion includes: The steel substrate is hot-dip coated to obtain a zinc-aluminum-magnesium coated steel sheet. The zinc-aluminum-magnesium coated steel sheet is cooled. The temperature of the plating solution used in the hot-dip plating is 480°C.
2. A zinc-aluminum-magnesium coated steel sheet resistant to filamentous corrosion, the coated steel sheet comprising a steel substrate and a zinc-aluminum-magnesium coating attached to at least a portion of the surface of the steel substrate; The chemical composition of the zinc-aluminum-magnesium coating, by mass fraction, is: Al: 1.1%, Mg: 1.3%, Bi: 0.6%, and the base element Zn; The zinc-aluminum-magnesium coating contains a Mg-Bi compound, which is in particulate form, has a volume fraction of 0.21%, and a circumscribed circle diameter of 450 μm. The volume fraction of the eutectic structure on the surface of the zinc-aluminum-magnesium coating is 14%. The method for preparing the zinc-aluminum-magnesium coated steel sheet resistant to filamentous corrosion includes: The steel substrate is hot-dip coated to obtain a zinc-aluminum-magnesium coated steel sheet. The zinc-aluminum-magnesium coated steel sheet is cooled. The temperature of the plating solution used in the hot-dip plating is 460°C.
Citation Information
Patent Citations
FUSED Zn-Al-Mg-BASED PLATED STEEL SHEET, COMPONENT FOR AUTOMOBILE, AND METHODS OF MANUFACTURING THEM
JP2023074874A
Highly corrosion-resistant zinc alloy-plating steel wire and method of manufacturing same
WO2017078195A1