Residue-free flux and solder paste for formic acid atmosphere soldering and their preparation methods

By using a residue-free flux formulation and preparation process, the problem of solder paste residue in a formic acid atmosphere has been solved, achieving high-quality, low-voidity, and high-reliability soldering results, and is suitable for various solder alloys.

CN119794655BActive Publication Date: 2026-11-17YOUYANNA MICRO NEW MATERIALS (BEIJING) CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411972899.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-12-30
Publication Date
2026-11-17
Estimated Expiration
2044-12-30

AI Technical Summary

Technical Problem

Existing solder paste has residue problems after soldering in a formic acid atmosphere, which affects the soldering quality and reliability. In particular, it can easily lead to aging and corrosion of circuit insulation under high temperature and humidity conditions, increasing production costs.

Method used

A residue-free flux formulation, including solvents, thixotropic agents, activators, and leveling agents, is used to prepare a residue-free solder paste suitable for formic acid atmosphere soldering by precisely controlling the component ratios and stirring process. This forms a protective film, slows down the oxidation rate, and improves the soldering quality.

Benefits of technology

This achieves zero residue during the welding process, reduces weld voids, improves wettability and the mechanical and thermal stress resistance of the weld layer, ensures long-term product reliability, and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119794655B_ABST
    Figure CN119794655B_ABST
Patent Text Reader

Abstract

This invention belongs to the field of electronic soldering materials technology, specifically relating to a residue-free flux and solder paste for formic acid atmosphere soldering, and their preparation method. The residue-free flux for formic acid atmosphere soldering comprises the following components by weight: 46-55 parts solvent, 19-29 parts thixotropic agent, 12-24 parts activator, and 6-15 parts leveling agent. This flux has strong applicability and at least solves the problems of residue and void suppression in electronic soldering materials under formic acid conditions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of electronic soldering materials technology, specifically to a residue-free flux and solder paste for formic acid atmosphere soldering and its preparation method. Background Technology

[0002] Solder paste soldering is a widely used soldering technology in the electronics manufacturing industry, such as computers, communications, consumer electronics, automotive electronics, LED lighting, and solar photovoltaics. In these fields, solder paste soldering technology provides strong support for the high performance and high reliability of electronic products. Solder paste is composed of metal alloy powder and flux. It is melted at high temperatures through reflow heating and penetrates the contact points between electronic components and circuit boards, thereby achieving the connection between electronic components and circuit boards. Organic additives play a fixing and supporting role during the melting process, ensuring the stability and reliability of the solder joint.

[0003] Formic acid reflow soldering is a new application technology that utilizes the chemical reaction between formic acid and metal oxides. Hydroxyl groups replace oxygen atoms to form formate, and formate decomposes at high temperature to form metal elements. The reaction formulas are as follows: (1) and (2). The heat generated in this process is used to heat and melt the solder, thereby realizing the soldering process and eliminating the adverse effects of metal oxides on the solder joint.

[0004] SnO2 + 4HCOOH = Sn(COOH)4 + 2H2O (Equation 1) Sn(COOH)4→4CO2+Sn+2H2 (Equation 2) However, in practical applications, existing solder pastes often leave significant residue after soldering in a formic acid atmosphere. This not only affects the appearance but also poses a potential threat to application reliability. Especially when electronic devices are exposed to high temperature and humidity for extended periods, the accumulation of flux residue can easily lead to serious problems such as insulation aging, short circuits, and corrosion, resulting in unstable soldering quality and ultimately affecting the long-term stable operation of electronic products. Although there are flux residues that can be cleaned, this undoubtedly increases the consumption of cleaning agents and labor costs, thereby raising the overall production cost.

[0005] Therefore, existing solder pastes and fluxes still need improvement. Summary of the Invention

[0006] The main objective of this invention is to provide a residue-free flux and solder paste for formic acid atmosphere soldering, and a method for preparing the same. This flux has strong applicability and at least solves the problems of residual electronic soldering materials and void suppression in formic acid environments.

[0007] A first aspect of the present invention provides a residue-free flux for welding in a formic acid atmosphere, the flux comprising the following components in parts by weight: 46 to 55 parts solvent, 19 to 29 parts thixotropic agent, 12 to 24 parts activator, and 6 to 15 parts leveling agent.

[0008] In some embodiments of the present invention, the solvent includes one or more combinations of isopropanol, n-butanol, hexanediol, rosin alcohol, tripropanol butyl ether, terpineol, ethylene glycol methyl ether, diethylene glycol ethyl ether, diethylene glycol butyl ether, 2-ethyl-1,3-hexanediol, diethylene glycol hexane ether, glycerol, propylene glycol, divalent esters, diethyl adipate, butyl formate, amyl formate, diglycidyl ether, dioctyl phthalate, tetraethylene glycol, isohexadecanol, diethylene glycol butyl ether acetate, and nitrobenzene mixed solvents.

[0009] In some embodiments of the present invention, the thixotropic agent includes at least one of wax-based thixotropic agents and amide-based thixotropic agents.

[0010] In some embodiments of the present invention, the wax-based thixotropic agent comprises methyl hydrogenated castor oil.

[0011] In some embodiments of the present invention, the amide thixotropic agent includes one or more combinations of polyamide wax, erucamide, octadecyl stearamide, lauramide, fatty acid triglycerides, oleamide, p-toluenemethaneamide, and fatty acid ester amides.

[0012] In some embodiments of the present invention, the activator includes one or more combinations of stearic acid, propylenediamine phosphate, 2,2-dimethylolbutyric acid, p-tert-butylbenzoic acid, 4-methyl-2-phenylimidazolium, citric acid, dibromosuccinic acid, ethylene bis-stearamide, succinic acid, oxalic acid, malic acid, glutaric acid, tetradecanoic acid, stearic acid, dioctyl sebacate, dioctyl hexanoate, methylsuccinic acid, stearic acid, phthalic acid, glutamic acid, glycine, 2-methylbenzimidazole, 2-undecylimidazolium, 2-methylacetic acid, 2-phenylbutyric acid, N-ethylimidazolium, and benzimidazole.

[0013] In some embodiments of the present invention, the leveling agent comprises one or more of the following: potassium monododecyl phosphate, dodecyltrimethylammonium chloride, fatty alcohol polyoxyethylene ether, trisodium citrate, pentaerythritol hexadecanoate, sodium hypophosphite, nonylphenol polyoxyethylene ether, imidazoline, and alkylphenol polyoxyethylene ether.

[0014] The second aspect of the present invention provides a method for preparing the residue-free flux for formic acid atmosphere welding as described in the first aspect. The preparation method includes: adding each component forming the flux into a reaction vessel according to the required ratio, and performing a first stirring after each component is added, and performing a second stirring after all components have been added, thereby obtaining the flux.

[0015] In some embodiments of the present invention, the first stirring is carried out at 60°C to 100°C, and the speed of the first stirring is 8 rpm / min to 12 rpm / min.

[0016] In some embodiments of the present invention, the speed of the second stirring is 10 rpm / min to 20 rpm / min.

[0017] A third aspect of the present invention provides a residue-free solder paste for soldering in a formic acid atmosphere, the solder paste comprising the following components by weight percentage: 86 wt% to 90 wt% alloy powder and 10 wt% to 14 wt% flux; wherein the flux is the residue-free flux for soldering in a formic acid atmosphere described in the first aspect or a flux prepared by the method for preparing the residue-free flux for soldering in a formic acid atmosphere described in the second aspect.

[0018] The fourth aspect of the present invention provides a method for preparing the residue-free solder paste for formic acid atmosphere soldering as described in the third aspect, the method comprising: mixing and stirring alloy powder and flux in a required ratio, and vacuuming to obtain the solder paste.

[0019] This invention provides a residue-free flux for welding in a formic acid atmosphere. The equipment and materials required for using this flux are low-cost, and the formulation and manufacturing process are convenient. Furthermore, formic acid acts as both a reducing agent and a flux, forming a protective film on the metal surface, slowing down oxidation, helping to maintain the cleanliness of the metal surface during welding, and improving weld quality.

[0020] The residue-free flux for welding in formic acid atmosphere provided by this invention has a simple formula and manufacturing process and can be applied to a variety of solder alloys.

[0021] The residue-free solder paste for formic acid atmosphere welding provided by this invention can effectively reduce the generation of voids in the solder layer and the surface tension of liquid metal during the welding process. It has strong applicability and improves wetting performance, allowing liquid metal to spread better on the surface of solid metal and fill the weld.

[0022] The residue-free solder paste for formic acid atmosphere soldering provided by this invention has the advantages of low soldering void rate, strong wettability, no residue in the post-soldering system, and the solder layer can withstand greater mechanical and thermal stress, thereby ensuring the long-term reliability of the product.

[0023] The residue-free flux and solder paste for formic acid atmosphere soldering provided by this invention offer a new solution to the technical problems of material residue and void suppression in electronic soldering under formic acid environment.

[0024] The above description is merely an overview of the technical solution of the present invention. In order to better understand the technical means of the present invention and to implement it in accordance with the contents of the specification, and in order to make the above and other objects, features and advantages of the present invention more apparent and understandable, specific embodiments of the present invention are described below. Attached Figure Description

[0025] Various other advantages and benefits will become apparent to those skilled in the art upon reading the following detailed description of preferred embodiments. The accompanying drawings are for illustrative purposes only and are not intended to limit the invention. In the drawings: Figure 1 The images show the wetting and residue of the solder paste prepared in the examples and comparative examples; wherein, Figure 1 (a) ~ Figure 1 (d) Wetting and residue images of the solder paste prepared in Examples 1-4, respectively; Figure 1 (e)~ Figure 1 (f) Wetting and residue diagrams of the solder paste prepared in Comparative Examples 1 and 2, respectively; Figure 2 The void ratio of the solder paste prepared in the examples and comparative examples is shown; wherein, Figure 2 (a) ~ Figure 2 (d) represents the void ratio of the solder paste prepared in Examples 1-4, respectively; Figure 2 (e)~ Figure 2 (f) represents the void ratio of the solder paste prepared in Comparative Examples 1 and 2, respectively. Detailed Implementation

[0026] Hereinafter, embodiments of the present invention will be described with reference to the accompanying drawings. However, it should be understood that these descriptions are merely exemplary and not intended to limit the scope of the invention. Furthermore, descriptions of well-known structures and techniques are omitted in the following description to avoid unnecessarily obscuring the concept of the invention.

[0027] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains; the terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit the invention; the terms “comprising” and “having”, and any variations thereof, in the specification, claims, and foregoing description of the invention, are intended to cover non-exclusive inclusion.

[0028] In the description of the embodiments of this invention, technical terms such as "first" and "second" are used only to distinguish different objects and should not be construed as indicating or implying relative importance or implicitly specifying the number, specific order, or primary and secondary relationship of the indicated technical features. In the description of the embodiments of this invention, "multiple" means two or more, unless otherwise explicitly defined.

[0029] In this document, the term "embodiment" means that a particular feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment of the invention. The appearance of this phrase in various places throughout the specification does not necessarily refer to the same embodiment, nor is it a separate or alternative embodiment mutually exclusive with other embodiments. It will be explicitly and implicitly understood by those skilled in the art that the embodiments described herein can be combined with other embodiments.

[0030] In the description of the embodiments of this invention, the term "and / or" is merely a description of the relationship between related objects, indicating that three relationships can exist. For example, A and / or B can represent: A existing alone, A and B existing simultaneously, and B existing alone. Additionally, the character " / " in this document generally indicates that the preceding and following related objects have an "or" relationship.

[0031] In the description of the embodiments of the present invention, the term "multiple" refers to two or more (including two), similarly, "multiple groups" refers to two or more (including two groups), and "multiple pieces" refers to two or more (including two pieces).

[0032] The first aspect of the present invention provides a residue-free flux for welding in a formic acid atmosphere, the flux comprising the following components in parts by weight: 46 to 55 parts solvent, 19 to 29 parts thixotropic agent, 12 to 24 parts activator, and 6 to 15 parts leveling agent.

[0033] In the embodiments of this invention, the formulation of the residue-free flux for formic acid atmosphere welding is simple. Through component design, the content of each component is precisely controlled, and the interaction between components is optimized, thereby achieving excellent compatibility with the formic acid reflow soldering process. Not only does the post-soldering system exhibit a residue-free state, but it also effectively reduces the generation of voids within the weld layer and the surface tension of the liquid metal during welding, significantly improving wettability, slowing oxidation, and fully filling the weld seam. Furthermore, the flux provided by this invention has strong applicability, offering a new solution to the technical problems of residue and void suppression in electronic welding materials under formic acid conditions.

[0034] In embodiments of the present invention, the solvent weight fraction is 46 to 55 parts. Exemplarily, the solvent weight fraction can be one of 46, 47, 48, 49, 50, 51, 52, 53, 54, or 55 parts, or any value satisfying the above range.

[0035] In embodiments of the present invention, the solvent includes one or more combinations of isopropanol, n-butanol, hexanediol, rosin alcohol, tripropanol butyl ether, terpineol, ethylene glycol methyl ether, diethylene glycol ethyl ether, diethylene glycol butyl ether, 2-ethyl-1,3-hexanediol, diethylene glycol hexane ether, glycerol, propylene glycol, divalent esters, diethyl adipate, butyl formate, amyl formate, diglycidyl ether, dioctyl phthalate, tetraethylene glycol, isohexadecanol, diethylene glycol butyl ether acetate, and nitroethane mixed solvents.

[0036] In embodiments of the present invention, the weight fraction of the thixotropic agent is 19 to 29 parts. Exemplarily, the weight fraction of the thixotropic agent can be one of 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, or 29 parts, or any value satisfying the above range.

[0037] In embodiments of the present invention, the thixotropic agent includes at least one of wax-based thixotropic agents and amide-based thixotropic agents.

[0038] In some embodiments of the present invention, the wax-based thixotropic agent may be, but is not limited to, methyl hydrogenated castor oil.

[0039] In some embodiments of the present invention, amide thixotropic agents include one or more combinations of polyamide wax, erucamide, octadecyl stearamide, lauramide, fatty acid triglycerides, oleamide, p-toluenemethaneamide, and fatty acid ester amides.

[0040] In embodiments of the present invention, the amount of surfactant is 12 to 24 parts by weight. Exemplarily, the amount of surfactant by weight can be one of 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, or 24 parts, or any value satisfying the above range.

[0041] In embodiments of the present invention, the active agent includes one or more combinations of stearic acid, propylenediamine phosphate, 2,2-dimethylolbutyric acid, p-tert-butylbenzoic acid, 4-methyl-2-phenylimidazolium, citric acid, dibromosuccinic acid, ethylene bis-stearamide, succinic acid, oxalic acid, malic acid, glutaric acid, tetradecanoic acid, stearic acid, dioctyl sebacate, dioctyl hexanoate, methylsuccinic acid, stearic acid, phthalic acid, glutamic acid, glycine, 2-methylbenzimidazole, 2-undecylimidazolium, 2-methylacetic acid, 2-phenylbutyric acid, N-ethylimidazolium, and benzimidazole.

[0042] In embodiments of the present invention, the weight fraction of the leveling agent is 6 to 15 parts. Exemplarily, the weight fraction of the leveling agent can be one of 6, 7, 8, 9, 10, 11, 12, 13, 14, or 15 parts, or any value satisfying the above range.

[0043] In embodiments of the present invention, the leveling agent comprises one or more of the following: potassium monododecyl phosphate, dodecyltrimethylammonium chloride, fatty alcohol polyoxyethylene ether, trisodium citrate, pentaerythritol hexadecanoate, sodium hypophosphite, nonylphenol polyoxyethylene ether, imidazoline, and alkylphenol polyoxyethylene ether.

[0044] The second aspect of the present invention provides a method for preparing a residue-free flux for welding in a formic acid atmosphere. The key point is that each component forming the flux is added to a reaction vessel according to the required ratio, and a first stirring is performed after each component is added, and a second stirring is performed after all components are added to obtain the flux.

[0045] In the embodiments of the present invention, the flux for welding in formic acid atmosphere provided by the present invention has a convenient manufacturing process. Not only does the system exhibit a residue-free state after welding, but it can also effectively reduce the generation of voids inside the weld layer and the surface tension of liquid metal during the welding process, significantly improve wettability, slow down the oxidation rate, and fully fill the weld.

[0046] In embodiments of the present invention, the first stirring is performed at a temperature of 60°C to 100°C, and the stirring speed is 8 rpm / min to 12 rpm / min. Exemplarily, the temperature of the first stirring can be one of 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C, 95°C, and 100°C, or any value satisfying the above range. The stirring speed can be one of 8 rpm / min, 9 rpm / min, 10 rpm / min, 11 rpm / min, and 12 rpm / min, or any value satisfying the above range.

[0047] In an embodiment of the present invention, the second stirring speed is 10 rpm / min to 20 rpm / min. Exemplarily, the second stirring speed can be one of 10 rpm / min, 11 rpm / min, 12 rpm / min, 13 rpm / min, 14 rpm / min, 15 rpm / min, 16 rpm / min, 17 rpm / min, 18 rpm / min, 19 rpm / min, or 20 rpm / min, or any value satisfying the above range.

[0048] In an embodiment of the present invention, the preparation method of the residue-free flux for welding in a formic acid atmosphere includes: accurately weighing each component and adding them to a reaction vessel respectively, and stirring at 60°C to 100°C for 8 min to 12 min after each component is added, and stirring for 15 min to 25 min after all components have been added to obtain the flux.

[0049] In embodiments of the present invention, the stirring time after each component is added can be one of 8 min, 9 min, 10 min, 11 min, 12 min, or any value within the above range. The stirring time after all components have been added can be one of 15 min, 16 min, 17 min, 18 min, 19 min, 20 min, 21 min, 22 min, 23 min, 24 min, 25 min, or any value within the above range.

[0050] In an embodiment of the present invention, the prepared flux is finely ground and left to stand for 24 hours before use.

[0051] In embodiments of the present invention, the reaction vessel may be a reaction kettle.

[0052] The third aspect of the present invention provides a residue-free solder paste for soldering in a formic acid atmosphere, the solder paste comprising the following components by mass percentage: 86 wt% to 90 wt% alloy powder and 10 wt% to 14 wt% flux; wherein the flux is the residue-free flux for soldering in a formic acid atmosphere described in the first aspect or the flux prepared by the method for preparing the residue-free flux for soldering in a formic acid atmosphere described in the second aspect.

[0053] In embodiments of the present invention, the alloy powder may be, but is not limited to, one of Sn5Ag2.5Pb92.5 powder, Sn5Ag1.5Pb93.5 powder, Sn5Ag2.2Pb92.8 powder, and Sn2Ag2.5Pb95.5 powder.

[0054] In embodiments of the present invention, the mass percentage of the alloy powder can be one of 86 wt%, 87 wt%, 88 wt%, 89 wt%, 90 wt%, or any value satisfying the above range. The mass percentage of the flux can be one of 10 wt%, 11 wt%, 12 wt%, 13 wt%, 14 wt%, or any value satisfying the above range.

[0055] The fourth aspect of the present invention provides a method for preparing a residue-free solder paste for formic acid atmosphere soldering, the key being that alloy powder and flux are mixed and stirred in the required proportions, and vacuum is applied to obtain the solder paste.

[0056] In an embodiment of the present invention, the flux is first stirred evenly at a stirring speed of 8 rpm / min to 12 rpm / min, for example, the stirring speed can be one of 8 rpm / min, 9 rpm / min, 10 rpm / min, 11 rpm / min, or 12 rpm / min or any value within the above range; the stirring time is 8 min to 10 min, for example, the stirring time can be one of 8 min, 9 min, or 10 min or any value within the above range.

[0057] Then, add the powder to the flux while stirring. The stirring speed is 6 rpm / min to 10 rpm / min, for example, the stirring speed can be one of 6 rpm / min, 7 rpm / min, 8 rpm / min, 9 rpm / min, 10 rpm / min or any value within the above range; the stirring time is 1 min to 3 min, for example, the stirring time can be one of 1 min, 2 min, 3 min or any value within the above range, to obtain solder paste.

[0058] Next, the solder paste is stirred at a speed of 6 rpm / min to 10 rpm / min, for example, a stirring speed of 6 rpm / min, 7 rpm / min, 8 rpm / min, 9 rpm / min, or 10 rpm / min, or any value within the above range; the stirring time is 1 min to 3 min, for example, a stirring time of 1 min, 2 min, or 3 min, or any value within the above range; then, vacuum stirring is performed at a speed of 16 rpm / min to 20 rpm / min, for example, a stirring speed of 16 rpm / min, 17 rpm / min, 18 rpm / min, 19 rpm / min, or 20 rpm / min, or any value within the above range; the stirring time is 8 min to 12 min, for example, a stirring time of 8 min, 9 min, 10 min, 11 min, or 12 min, or any value within the above range, with the vacuum level adjusted to -0.08 MPa to -0.1 MPa, for example, adjusted to -0.08 MPa. Solder paste is obtained by applying a value of one of MPa, -0.09 MPa, -0.1 MPa, or any value within the above range.

[0059] Unless otherwise defined, the technical terms used in the following embodiments have the same meaning as commonly understood by those skilled in the art. Unless otherwise specified, the experimental reagents used in the following embodiments are all conventional biochemical reagents; the raw materials, instruments, and equipment used in the following embodiments can all be obtained commercially or through existing methods; unless otherwise specified, the amounts of experimental reagents used are the amounts used in conventional experimental operations; unless otherwise specified, the experimental methods are all conventional methods.

[0060] Example 1 A residue-free flux for welding in a formic acid atmosphere comprises the following components in parts by weight: 9 parts isopropanol, 41 parts 2-ethyl-1,3-hexanediol, 14 parts methyl hydrogenated castor oil, 10 parts p-toluenemethaneamide, 6 parts p-tert-butylbenzoic acid, 4 parts phthalic acid, 7 parts 2-methylbenzimidazole, 2 parts dodecyltrimethylammonium chloride, 6 parts trisodium citrate, and 1 part nonylphenol polyoxyethylene ether.

[0061] Preparation method of residue-free flux for welding in formic acid atmosphere: Each of the above components is added to a reaction vessel, and after each component is added, it is stirred at 80°C for 10 min at a stirring speed of 10 rpm / min. After all components are added, it is stirred for another 15 min at a stirring speed of 15 rpm / min. Then, it is finely ground and left to stand for 24 h to return to room temperature to obtain residue-free flux.

[0062] A residue-free solder paste for soldering in a formic acid atmosphere comprises the following components by weight percentage: 88% Sn5Ag2.5Pb92.5 powder and 12% flux.

[0063] Preparation method of solder paste for formic acid atmosphere soldering: The flux is placed in a reaction vessel and stirred at a speed of 12 rpm / min for 10 min; then powder is added while stirring for 1 min at a speed of 8 rpm / min; the resulting solder paste is then stirred for 1 min at a speed of 8 rpm / min; then vacuum stirring is carried out for 10 min at a speed of 18 rpm / min, and the vacuum degree is drawn to -0.08 MPa to obtain the solder paste prepared from the above flux.

[0064] Finally, the solder paste prepared in Example 1 was soldered in a formic acid atmosphere, and the residual condition was observed under a microscope and the presence of internal voids was observed by X-ray.

[0065] Example 2 The remaining operations are the same as in Example 1, except that the residue-free flux used for welding in formic acid atmosphere in Example 2 includes the following components by weight: 8 parts isopropanol, 43 parts 2-ethyl-1,3-hexanediol, 12 parts methyl hydrogenated castor oil, 12 parts p-toluenemethaneamide, 8 parts p-tert-butylbenzoic acid, 2 parts phthalic acid, 5 parts 2-methylbenzimidazole, 4 parts dodecyltrimethylammonium chloride, 3 parts trisodium citrate, and 3 parts nonylphenol polyoxyethylene ether.

[0066] The residue-free solder paste used for formic acid atmosphere soldering in Example 2 comprises the following components by mass percentage: 88% Sn5Ag1.5Pb93.5 powder and 12% flux.

[0067] Example 3 The remaining operations are the same as in Example 1, except that the residue-free flux used for welding in formic acid atmosphere in Example 3 includes the following components by weight: 10 parts isopropanol, 38 parts 2-ethyl-1,3-hexanediol, 16 parts methyl hydrogenated castor oil, 7 parts p-toluenemethaneamide, 7 parts p-tert-butylbenzoic acid, 5 parts phthalic acid, 4 parts 2-methylbenzimidazole, 5 parts dodecyltrimethylammonium chloride, 7 parts trisodium citrate, and 1 part nonylphenol polyoxyethylene ether.

[0068] The residue-free solder paste used for formic acid atmosphere soldering in Example 3 comprises the following components by mass percentage: 88% Sn5Ag2.2Pb92.8 powder and 12% flux.

[0069] Example 4 The remaining operations are the same as in Example 1, except that the residue-free flux used for welding in formic acid atmosphere in Example 4 includes the following components by weight: 9 parts isopropanol, 45 parts 2-ethyl-1,3-hexanediol, 12 parts methyl hydrogenated castor oil, 13 parts p-toluenemethaneamide, 8 parts p-tert-butylbenzoic acid, 3 parts phthalic acid, 9 parts 2-methylbenzimidazole, 3 parts dodecyltrimethylammonium chloride, 5 parts trisodium citrate, and 2 parts nonylphenol polyoxyethylene ether.

[0070] The residue-free solder paste used for formic acid atmosphere soldering in Example 4 comprises the following components by mass percentage: 88% Sn2Ag2.5Pb95.5 powder and 12% flux.

[0071] Comparative Example 1 Comparative Example 1 uses commercially available flux of the same specifications, and the rest of the operation is the same as in Example 1.

[0072] Comparative Example 2 Example 2 uses commercially available flux of the same specifications 2, and the rest of the operation is the same as in Example 1.

[0073] In this invention, the solder pastes prepared in the examples and comparative examples were subjected to relevant performance tests, and the test results are detailed in Table 1.

[0074] Table 1 Summary of performance tests of solder pastes prepared in the Examples and Comparative Examples

[0075] Combined with appendix Figure 1-2 As shown in Table 1, multiple sets of solder pastes were prepared by using the flux of the present invention in combination with different alloy powders. After soldering in a formic acid atmosphere, the solder pastes not only showed a state with almost no residue after soldering but also had bright solder joints, exhibiting an ultra-low void rate of less than 5%. Among them, the solder paste prepared using Sn5Ag2.5Pb92.5-T4 powder had the lowest void rate of 1.78%.

[0076] Meanwhile, by using commercially available fluxes as a comparative example, it can be seen that the flux provided by this invention for welding in a formic acid atmosphere is convenient in terms of formulation and manufacturing process. Not only does it result in a residue-free system after welding, but it also effectively reduces the generation of voids in the weld layer and the surface tension of the liquid metal during the welding process, significantly improves wettability, slows down the oxidation rate, and fully fills the weld.

[0077] In summary, the flux for welding in formic acid atmosphere provided by this invention has strong applicability and provides a new solution to the technical problems of residual electronic welding materials and void suppression in formic acid environment.

[0078] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features therein. These modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention, and they should all be covered within the scope of the claims and specification of the present invention. In particular, as long as there is no structural conflict, the various technical features mentioned in the embodiments can be combined in any way. The present invention is not limited to the specific embodiments disclosed herein, but includes all technical solutions falling within the scope of the claims.

Claims

1. A residue-free flux for welding in a formic acid atmosphere, characterized in that, The flux consists of the following components in parts by weight: Solvent 46-55 parts, thixotropic agent 19-29 parts, surfactant 12-24 parts, leveling agent 6-15 parts; The solvent is isopropanol and 2-ethyl-1,3-hexanediol; the thixotropic agent includes wax-based thixotropic agents and amide-based thixotropic agents, wherein the wax-based thixotropic agent is methyl hydrogenated castor oil and the amide-based thixotropic agent is p-toluenemethaneamide; the activator is p-tert-butylbenzoic acid, phthalic acid and 2-methylbenzimidazole; the leveling agent is dodecyltrimethylammonium chloride, trisodium citrate and nonylphenol polyoxyethylene ether. The method for preparing the residue-free flux for welding in formic acid atmosphere includes: According to the required proportions, each component of the flux is added to the reaction vessel, and a first stirring is performed after each component is added. The first stirring is carried out at 60℃~100℃ and the stirring speed is 8 rpm~12 rpm. After all components are added, a second stirring is performed at a speed of 10 rpm~20 rpm to obtain the residue-free flux.

2. A method for preparing a residue-free flux for formic acid atmosphere welding as described in claim 1, characterized in that, The preparation method includes: The components that form the flux are added to the reaction vessel according to the required ratio. After each component is added, the mixture is stirred for the first time. After all components have been added, the mixture is stirred for the second time to obtain the flux.

3. A residue-free solder paste for soldering in a formic acid atmosphere, characterized in that, The solder paste comprises the following components by weight percentage: Alloy powder 86 wt%~90 wt%, flux 10 wt%~14 wt%; Wherein, the flux is the residue-free flux for welding in formic acid atmosphere as described in claim 1 or the flux prepared by the method for preparing the residue-free flux for welding in formic acid atmosphere as described in claim 2.

4. A method for preparing residue-free solder paste for formic acid atmosphere soldering as described in claim 3, characterized in that, The preparation method includes: The alloy powder and flux are mixed and stirred in the required proportions, and then vacuumed to obtain the solder paste.

Citation Information

Patent Citations

  • Lead-free and cleaning-free solder paste capable of realizing few-cavity welding layers and preparation method of lead-free cleaning-free solder paste

    CN102528315A

  • Halogen-free scaling powder used for lead-free solder paste and preparation method thereof

    CN103008921A

  • Lead-free environment-friendly welding-aid paste

    CN104148825A

  • Scaling powder for no-clean lead-free low-silver welding paste

    CN104400257A

  • Halogen-free sulfur-free and lead-free solder paste

    CN108161269A