Oxide perovskite / sulfide perovskite composite material and preparation method and application thereof
By epitaxially growing sulfide perovskites on oxide perovskites, oxide perovskite/sulfide perovskite micro-nanocomposites are prepared, which solves the problems of high energy consumption, long synthesis period and low photocatalytic efficiency in the prior art, and achieves the green synthesis and high-efficiency photocatalytic performance of the material.
Patent Information
- Application Number
- CN202311748773.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-19
- Publication Date
- 2025-06-20
AI Technical Summary
The existing preparation technologies for oxide perovskite and sulfide perovskite materials have problems such as high energy consumption, long synthesis cycle and low photocatalytic efficiency.
Epitaxial growth method is used to grow sulfide perovskites on oxide perovskites, and oxide perovskite/sulfide perovskite micro-nanocomposites are prepared to optimize the interface structure of the material and the transmission and separation properties of photogenerated charges.
The green, low energy consumption and rapid synthesis of materials are achieved, the photocatalytic performance is improved, and the II-type or S-type charge transport paths suitable for photocatalytic reactions are formed.
Smart Images

Figure CN120169389A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to inorganic functional micro-nano composites, and specifically to an oxide perovskite / sulfide perovskite composite material, a preparation method and uses thereof, belonging to the technical field of inorganic functional materials. Background Art
[0002] Due to its excellent physical and chemical properties such as abundant raw materials, diverse structures, environmental stability, easy synthesis, and suitable band structures, inorganic oxide perovskites have attracted extensive attention from researchers. At present, they have shown good application prospects in the fields of energy, environment, electronics, optoelectronics, catalysis, etc. (Solar RRL, 2017, 1, 1700126; Energy Environ. Sci. 2019, 12, 442 - 462; Nature 2019, 570, 87 - 90; Angew. Chem. Int. Ed. 2020, 59, 136 - 152; Adv. Funct. Mater. 2023, 33, 2301981). However, single oxide perovskite materials always have the disadvantages of too large band gaps and low charge separation efficiency, resulting in a narrow spectral absorption range and low photocatalytic efficiency, which seriously restricts their popularization and industrial application (Chem. Soc. Rev. 2021, 50, 13692 - 13729; Small 2021, 17, 2005345; ACS Appl. Mater. Interfaces 2022, 14, 51819 - 51834; Angew. Chem. Int. Ed. 2023, 135, e202215700). For this reason, scientists have made various attempts and efforts to solve the shortcomings faced by oxide perovskite materials, including morphology regulation, element doping, surface / interface structure optimization, introduction of cocatalysts, and construction of composite materials by combining with other materials. In particular, the effective construction of composite materials has shown good application prospects in promoting charge separation and optimizing material light absorption. However, most composite materials are only obtained by simple physical mixing, which results in unsatisfactory interfacial bonding quality of the materials, hinders their charge separation and transport, and leads to low photocatalytic efficiency. Therefore, designing and developing simple and effective synthesis methods to prepare advanced oxide perovskite composite materials is an important research direction in this field.
[0003] Sulfide perovskites are a new type of perovskite materials, which have excellent light absorption ability, chemical stability, carrier transport properties, tunable bandgap width, non-toxicity and other advantages, and have been widely used in basic research and optoelectronic device applications (Chem. Mater. 2020, 32, 2450-2460; Sci. China Mater. 2021, 64, 2976-2986; Chem. Eng. J. 2023, 473, 145351; Nano Res. 2023, 16, 7867-7873; Adv. Optical Mater. 2023, 2301977, https: / / doi.org / 10.1002 / adom.202301977). However, the synthesis temperature of the vast majority of sulfide perovskite materials is too high (1000 °C and above) and the preparation period is too long (the reaction time requires several days or weeks and above) and other harsh conditions (J. Am. Chem. Soc. 2022, 144, 22403-22408; Adv. Optical. Mater. 2023, 11, 2201859; Nano Res. 2023, 16, 7867-7873; Adv. Funct. Mater. 2023, 2309514, https: / / doi.org / 10.1002 / adfm.202309514), which seriously affect their popularization and application. Summary of the Invention
[0004] Aiming at the problems of generally excessive energy consumption, long synthesis cycle and low photocatalytic efficiency in the preparation technologies of existing oxide perovskite and sulfide perovskite materials, the present invention provides a new method for synthesizing oxide perovskite / sulfide perovskite micro-nano composites, and originally develops a way of epitaxial growth for rapidly and effectively preparing novel oxide perovskite / sulfide perovskite micro-nano composites. The preparation conditions of the oxide perovskite / sulfide perovskite micro-nano composites are mild, the raw materials are easy to obtain, the process is short, and it has a closely contacted interface structure and staggered energy levels, which can effectively promote the separation and transport of photo-generated charges and has outstanding photocatalytic performance. To achieve the above technical objectives, the technical solutions adopted by the present invention are as follows:
[0005] According to the first embodiment of the present invention, there is provided an oxide perovskite / sulfide perovskite composite material:
[0006] An oxide perovskite / sulfide perovskite composite material, the composite material comprising an oxide perovskite substance and a sulfide perovskite substance epitaxially grown on the oxide perovskite substance.
[0007] Preferably, the perovskite oxide materials are one or more of Bi2MoO6, Bi2WO6, Bi2CrO6, Bi3TiNbO9, Bi3Fe 0.5 Nb 1.5 O9, Bi4Ti3O 12 , Bi5FeTi3O 15 , Bi6Fe2Ti3O 18 , Bi7Fe3Ti3O 21 ; preferably, they are Bi2MoO6, Bi3TiNbO9, Bi4Ti3O 12 or Bi5FeTi3O 15 .
[0008] Preferably, the perovskite sulfide materials are one or more of CaZrS3, CaTiS3, CaHfS3, SrZrS3, SrTiS3, SrHfS3, BaZrS3, BaTiS3, BaHfS3; preferably, they are CaZrS3, SrZrS3, SrTiS3 or BaZrS3.
[0009] Preferably, in the composite material, the molar ratio of the perovskite oxide material to the perovskite sulfide material is 0.5 - 10:1; preferably 1 - 8:1; more preferably 2 - 5:1.
[0010] Preferably, the particle size of the composite material is 0.1 - 5 μm; preferably 0.3 - 4 μm; more preferably 0.5 - 3 μm (i.e., the composite material of the present invention is a micro-nano composite material).
[0011] Preferably, the composite material is one or more of Bi2MoO6 / CaZrS3, Bi2WO6 / SrZrS3, Bi2CrO6 / BaTiS3, Bi3TiNbO9 / BaZrS3, Bi3TiNbO9 / SrZrS3, Bi4Ti3O 12 / BaZrS3, Bi4Ti3O 12 / BaTiS3, Bi5FeTi3O 15 / SrTiS3, Bi5FeTi3O 15 / BaHfS3, Bi7Fe3Ti3O 21 / BaZrS3; preferably, they are Bi2MoO6 / CaZrS3, Bi3TiNbO9 / BaZrS3, Bi3TiNbO9 / SrZrS3, Bi5FeTi3O 15 / SrTiS3 or Bi4Ti3O 12 / BaZrS3.
[0012] According to a second embodiment of the present invention, a method for preparing an oxide perovskite / sulfide perovskite composite material is provided:
[0013] A method for preparing an oxide perovskite / sulfide perovskite composite material or a method for preparing the oxide perovskite / sulfide perovskite composite material as described in the first embodiment, the method comprising the following steps:
[0014] 1) At least two of a bismuth source, a molybdenum source, a tungsten source, a chromium source, a titanium source, a niobium source, and an iron source are mixed with a metal halide salt, optionally an additive, and ethanol, and then subjected to grinding or dissolution and dispersion treatment, and then calcined and / or dried or hydrothermally treated to obtain an oxide perovskite micro-nano material. Here, optionally means adding or not adding.
[0015] 2) At least one of a calcium source, a barium source, and a strontium source and at least one of a zirconium source, a hafnium source, and a titanium salt are mixed or dissolved and dispersed with a sulfur source, a reducing agent, and a solvent to obtain a sulfide perovskite precursor solution.
[0016] 3) The oxide perovskite micro-nano material obtained in step 1) is added to the sulfide perovskite precursor solution obtained in step 2) for hydrothermal reaction, and after the reaction is completed, an oxide perovskite / sulfide perovskite composite material is obtained.
[0017] Preferably, in step 1), the bismuth source is one or more of Bi2O3, Bi(NO3)3·5H2O, BiBr3, BiCl3, bismuth ethanolate (C6H9BiO6), and bismuth citrate (C6H5BiO7).
[0018] Preferably, in step 1), the molybdenum source is one or more of (NH4)6Mo7O 24 ·4H2O, Na2MoO4·2H2O, and K2MoO4·2H2O.
[0019] Preferably, in step 1), the tungsten source is one or more of (NH4)6W7O 24 ·6H2O, Na2WO4·2H2O, and K2WO4·2H2O.
[0020] Preferably, in step 1), the chromium source is one or more of Na2CrO4, K2CrO4, and MgCrO4.
[0021] Preferably, in step 1), the titanium source is one or more of TiO2, tetrabutyl titanate, titanium isopropoxide, and potassium oxalate titanate.
[0022] Preferably, in step 1), the niobium source is Nb2O5, niobium ethanolate (C 10 H25 one or more of NbO5) and NbCl5.
[0023] Preferably, in step 1), the iron source is one or more of Fe(NO3)3·9H2O, FeCl3·6H2O, Fe2O3, and Fe2(SO4)3·7H2O.
[0024] Preferably, in step 1), the metal halide salt is one or more of chlorides, bromides, and iodides of lithium / sodium / potassium metals, preferably one or more of NaCl, KCl, LiCl, NaBr, KBr, NaI, and KI.
[0025] Preferably, in step 1), the auxiliary agent is one of citric acid monohydrate (C6H8O7·H2O), polyvinylpyrrolidone (PVP), and acetic acid (CH3COOH).
[0026] Preferably, in step 2), the sulfur source is one or more of sulfur powder, thiourea, L-cysteine, methionine, CS2, (NH4)2S, CH3CSNH2, and Na2S2O3.
[0027] Preferably, in step 2), the calcium source is one or more of Ca(NO3)2, CaCl2, CaI2, CaBr2, Ca(HSO3)2, and Ca(ClO)2.
[0028] Preferably, in step 2), the zirconium source is one or more of Zr(SO4)2, Zr(NO3)4, ZrOCl2·8H2O, ZrCl4, and Zr(C6H5O7)2.
[0029] Preferably, in step 2), the barium source is one or more of Ba(NO3)2, BaCl2, BaS, and Ba(CH3COO)2.
[0030] Preferably, in step 2), the strontium source is one or more of Sr(NO3)2, SrCl2, SrBr2, and SrI2.
[0031] Preferably, in step 2), the hafnium source is one or more of HfOCl2·8H2O, Hf(SO4)2, and HfCl4.
[0032] Preferably, in step 2), the titanium salt is one or more of TiO2, tetrabutyl titanate, titanium isopropoxide, and potassium oxalate titanate.
[0033] Preferably, in step 2), the reducing agent is one or more of hydrazine hydrate, Na2SO3, H2C2O4, FeSO4, NaBH4, and KBH4.
[0034] Preferably, in step 2), the solvent is one or more of ethylene glycol, DMF, deionized water, ethanol, and isopropanol.
[0035] Preferably, in step 1), the grinding time is 0.5 - 10 h, preferably 2 - 6 h. The temperature for calcination treatment is 100 - 900 °C, preferably 120 - 850 °C, the time for calcination treatment is 1 - 12 h, preferably 3 - 10 h; the heating rate is 2 - 20 °C / min, preferably 5 - 10 °C / min.
[0036] Preferably, in step 3), the temperature of the reaction is 100 - 250 °C, preferably 150 - 220 °C. The reaction time is 5 - 48 h, preferably 8 - 36 h.
[0037] Preferably, in step 3), the addition amounts of the oxide perovskite micro-nanomaterials and the sulfide perovskite precursor solution are such that the molar ratio of the oxide perovskite substances to the sulfide perovskite substances is 1 - 12:1, preferably 1.5 - 10:1, more preferably 2 - 6:1.
[0038] Preferably, step 1) is specifically as follows: According to the composition of the target oxide perovskite micro-nanomaterials, at least two of bismuth source, molybdenum source, tungsten source, chromium source, titanium source, niobium source, and iron source are weighed in proportion, and an appropriate amount of metal halide salt (as a grinding aid, the addition amount of which can be reasonably adjusted according to the grinding requirements), optionally an auxiliary agent, and ethanol are weighed. After mixing all the raw materials, they are placed in a mortar or ball mill (or other grinding equipment) and ground and crushed to the micro-nano level. Then, the ground mixture powder is dried and placed in a crucible and sent into a calcination furnace (such as a muffle furnace) for calcination treatment (the calcination heating rate is 0.1 - 30 °C / min) and / or placed in a drying oven for drying treatment (for example, the drying temperature is 50 - 250 °C, and the drying time is 1 - 48 h). After calcination and / or drying or hydrothermal treatment is completed, the calcined product is washed with deionized water, and then dried again to obtain the oxide perovskite micro-nanomaterials.
[0039] In the present invention, the oxide perovskite micro-nanomaterials include, but are not limited to, microscopic morphologies such as nanosheets, nanowires, nanorods, nanotubes, nanoflowers, nanospheres, nanosponges, nanocrystals, nanoparticles, and superlattices.
[0040] Preferably, step 2) is specifically as follows: First, one (or more) of a calcium source, a barium source, and a strontium source is added to a part of the solvent together with a sulfur source to obtain a mixed solution A, and then one (or more) of a zirconium source, a hafnium source, and a titanium salt is added to the remaining solvent together with a reducing agent to obtain a mixed solution B; then the mixed solution B is added to the mixed solution A and mixed evenly to obtain a sulfide perovskite precursor solution.
[0041] Preferably, step 3) is specifically as follows: The oxide perovskite micro-nano material is added to the sulfide perovskite precursor solution, stirred and mixed evenly, and then hydrothermal reaction is carried out. After the reaction is completed, the product is washed (for example, washed with deionized water at a rotation speed of 1000-9000 rpm until the upper liquid becomes clear, and then centrifugally washed with absolute ethanol 1-8 times. Finally, the mixture is filtered by suction to obtain a solid sample), and finally the washed solid sample is dried (for example, dried in a vacuum oven at a temperature of 50-100 °C for 1-10 h) to obtain an oxide perovskite / sulfide perovskite composite material.
[0042] In the present invention, the oxide perovskite / sulfide perovskite composite material includes, but is not limited to, micro-morphologies such as nanosheet-nanorod, nanowire-nanoparticle, nanorod-nanorod, nanotube-nanosheet, nanoflower-nanorod, nanosphere-nanoparticle, nanosponge-nanorod, nanosponge-nanoparticle, nanocrystal-nanorod, nanorod-nanoparticle, superlattice-nanoparticle, etc.
[0043] In the present invention, in step 1), the selection and dosage of the bismuth source, molybdenum source, tungsten source, chromium source, titanium source, niobium source, and iron source are determined according to the elemental composition and stoichiometric ratio of the target oxide perovskite micro-nano material. For example, when the target oxide perovskite micro-nano material is Bi3TiNbO9, the raw materials to be selected are the bismuth source, titanium source, and niobium source, and the addition amounts of the three are such that the molar ratio of bismuth:titanium:niobium contained is matched with the atomic number ratio in Bi3TiNbO9. Similarly, in step 2), the selection and dosage of the calcium source, zirconium source, barium source, strontium source, hafnium source, titanium salt, and sulfur source are determined according to the elemental composition and stoichiometric ratio of the sulfide perovskite-like substances in the target oxide perovskite / sulfide perovskite composite material.
[0044] According to the third embodiment of the present invention, a use for preparing an oxide perovskite / sulfide perovskite composite material is provided:
[0045] Use of an oxide perovskite / sulfide perovskite composite material, or use of an oxide perovskite / sulfide perovskite composite material as described in the first embodiment, or use of an oxide perovskite / sulfide perovskite composite material prepared by the method described in the second embodiment, wherein the oxide perovskite / sulfide perovskite composite material is used in the field of photocatalysis.
[0046] Preferably, the oxide perovskite / sulfide perovskite composite material is used for photocatalytic synthesis of H2O2, photocatalytic production of H2, photocatalytic synthesis of ammonia, photocatalytic degradation of pesticide residues or dye molecules.
[0047] In the present invention, the use of the oxide perovskite / sulfide perovskite composite material for photocatalytic synthesis of H2O2 is specifically as follows: A certain mass of the oxide perovskite / sulfide perovskite composite material is placed in a beaker, and a certain volume of deionized water or ultrapure water is added. After stirring and dispersing evenly, air or oxygen is introduced under dark conditions (the ventilation time is 0.1 - 4 h). After stirring for a certain time (for example, 0.1 - 5 h), a photocatalytic reaction is carried out. After the reaction is completed, the mixed solution is filtered with a filter head, and the filtrate is collected; then a certain volume of the filtrate is measured and placed in a centrifuge tube, and then a certain concentration and volume of cerium sulfate and sulfuric acid solutions are pipetted into the centrifuge tube for reaction. Finally, the absorbance is detected using a UV-visible spectrophotometer to judge the photocatalytic H2O2 production performance of the material.
[0048] It should be noted that when based on the dosage of the oxide perovskite / sulfide perovskite composite material (for example, the dosage is 1 g), the dosage of deionized water or ultrapure water is generally 10 - 2000 ml. The concentration of the cerium sulfate solution is 0.0001 - 0.003 mol / L, and the dosage is 1 - 100 ml; the concentration of the sulfuric acid solution is 0.1 - 1 mol / L, and its dosage is 1 - 80 ml. In addition, the light treatment time is 0.1 - 10 h, and the light intensity used is between 100 - 300 mW cm -2 between.
[0049] In the present invention, the use of the oxide perovskite / sulfide perovskite composite material for photocatalytic degradation of tetracycline hydrochloride is specifically as follows: A certain mass of the oxide perovskite / sulfide perovskite composite material is placed in a photoreactor, and a certain volume of tetracycline hydrochloride solution is added. After stirring and dispersing evenly, it is stirred for a certain time (for example, 0.1 - 5 h) under dark conditions, and then a photocatalytic reaction is carried out. After the reaction is completed, the mixed solution is filtered with a filter head, and the filtrate is collected; then a certain volume of the filtrate is measured and placed in a centrifuge tube, and finally the absorbance is detected using a UV-visible spectrophotometer to judge the photocatalytic degradation performance of the material for tetracycline.
[0050] In the present invention, the use of the oxide perovskite / sulfide perovskite composite material for photocatalytic degradation of glyphosate solution is specifically as follows: A certain amount of the oxide perovskite / sulfide perovskite composite material and a certain volume of the liquid to be degraded are added to a photoreactor. First, air is introduced and magnetically stirred for a period of time under dark conditions to form a uniform suspension system, and then the light is turned on for 1 h of photocatalytic degradation. After completion, a sample is taken and placed in a centrifuge tube, and then centrifuged at 4000 rpm for 10 min in a centrifuge. 4.5 mL of the supernatant is taken and placed in a 10 mL colorimetric tube, 0.50 mL of the molybdenum antimony anti-reagent is added and shaken well. After color development for 30 min, the absorbance at a wavelength of 710 nm is detected with a UV-visible spectrophotometer.
[0051] In the present invention, a new method for synthesizing an oxide perovskite / sulfide perovskite composite material is developed, that is, by utilizing the structural similarity of the two perovskite materials, the oxide perovskite is used as a nucleation site, and then the sulfide perovskite is epitaxially grown on the oxide perovskite. A micro-nano scale oxide perovskite / sulfide perovskite composite material is designed and prepared. By introducing the sulfide perovskite, the light absorption ability of the oxide perovskite is improved, and the interfacial structure of the composite material and the transport and separation properties of photo-generated charges are optimized. The oxide perovskite / sulfide perovskite composite material is expected to form a type-II or S-type charge transport path, promote the spatial separation and transport of photo-generated electron-hole pairs, and enhance the photocatalytic reaction performance. By studying the structure-activity relationship of the material, the deep mechanism of the photocatalytic reaction is revealed, providing a new idea for the rational design of advanced catalyst materials. In addition, the oxide perovskite / sulfide perovskite composite material can not only be used in the field of photocatalysis, but also be expected to be used in application fields such as photoelectrocatalysis, photothermal catalysis, and piezoelectric catalysis.
[0052] In the present invention, the method for effectively growing the sulfide perovskite on the oxide perovskite by the epitaxial growth strategy has the characteristics of low temperature, simplicity, and short time. Compared with most of the existing synthesis methods of sulfide perovskite materials, this method has the advantages of simple operation, low reaction temperature, short preparation cycle, and batch preparation, etc. It can realize the green, low-energy consumption, rapid and batch synthesis of the oxide perovskite / sulfide perovskite composite material, and solve the problems of high energy consumption, long reaction time, and complicated synthesis process in the existing preparation technology of sulfide perovskite materials; at the same time, the material described in the present invention is also expected to realize the efficient artificial photosynthesis of hydrogen peroxide, leading the development of sulfide perovskite photocatalyst materials.
[0053] Compared with the prior art, the beneficial technical effects of the present invention are as follows:
[0054] 1: The present invention has pioneered a new method for synthesizing oxide perovskite / sulfide perovskite micro-nano composites, that is, by taking advantage of the structural similarity of the two perovskite materials to epitaxially grow sulfide perovskite on oxide perovskite, an oxide perovskite / sulfide perovskite micro-nano composite material is designed and prepared. This method has the advantages of simple operation, low reaction temperature, short preparation cycle, and batch preparation compared with most of the existing synthesis methods of sulfide perovskite materials. It can achieve the green, low-energy consumption, rapid and batch synthesis of oxide perovskite / sulfide perovskite composites, and solve the problems of high energy consumption, long reaction time, and complicated synthesis process in the existing preparation technology of sulfide perovskite materials. At the same time, the materials of the present invention are also expected to achieve efficient artificial photosynthesis of H2O2 and lead the development of sulfide perovskite photocatalyst materials.
[0055] 2: The present invention improves the light absorption ability of oxide perovskite by introducing sulfide perovskite, and optimizes the interfacial structure of the material and the transport and separation properties of photo-generated charges. The oxide perovskite / sulfide perovskite micro-nano composite material is expected to form a type-II or S-type charge transport path, promote the spatial separation and transport of photo-generated electron-hole pairs, and improve the photocatalytic reaction performance. By studying the structure-activity relationship of the material, the deep mechanism of the photocatalytic reaction is revealed, providing new ideas for the rational design of advanced catalyst materials. In addition, the oxide perovskite / sulfide perovskite composite material can not only be used in the field of photocatalysis, but also be expected to be used in application fields such as photoelectrocatalysis, photothermal catalysis, and piezoelectric catalysis. Brief Description of the Drawings
[0056] Figure 1 XRD pattern of the Bi3TiNbO9 / BaZrS3 composite material obtained in Example 1 of the present invention.
[0057] Figure 2 TEM (1μm) image of the Bi3TiNbO9 / BaZrS3 composite material obtained in Example 1 of the present invention.
[0058] Figure 3 TEM (200nm) image of the Bi3TiNbO9 / BaZrS3 composite material obtained in Example 1 of the present invention.
[0059] Figure 4 Photocatalytic H2O2 production performance diagrams of the materials obtained in Examples 1, 3, 4, 5, 6 and Comparative Examples 1, 3, 4.
[0060] Figure 5 XRD pattern of the Bi4Ti3O 12 / BaZrS3 composite material obtained in Example 8 of the present invention.
[0061] Figure 6XRD pattern of the Bi3TiNbO9 / SrZrS3 composite material obtained in Example 9 of the present invention.
[0062] Figure 7 Performance graphs of the materials obtained in Examples 1, 3, 4, 5, 6 and Comparative Examples 1 and 3 for the photocatalytic degradation of tetracycline hydrochloride in 1 h.
[0063] Figure 8 Performance graphs of the materials obtained in Examples 1, 3, 4, 5, 6 and Comparative Examples 1 and 3 for the photocatalytic degradation of glyphosate in 1 h Detailed implementation manners
[0064] The technical solutions of the present invention will be illustrated by way of examples below. The scope claimed by the present invention includes but is not limited to the following examples.
[0065] Example 1
[0066] First, weigh 2.50 g of Bi2O3, 0.24 g of TiO2, 0.50 g of Nb2O5, 10.50 g of NaCl, 10.30 g of KCl and 2 ml of absolute ethanol and place them in a ball milling jar. Grind them on a ball mill for 2 h clockwise and counterclockwise respectively to obtain a mixture; then transfer the obtained mixture to an oven and dry it at 60 °C for 10 h to obtain a mixed powder; then put the obtained mixed powder into a crucible and place it in a muffle furnace. Heat it to 850 °C at a heating rate of 5 °C / min and calcine it at this temperature for 6 h. Finally, wash the calcined solid powder with deionized water until there is no Cl - , and after drying, Bi3TiNbO9 powder, denoted as BTNO, is obtained.
[0067] Weigh 0.013 g of Ba(NO3)2 and 0.018 g of L-cysteine and place them in an 80 mL beaker. Add 20 mL of ethylene glycol and stir for 1 h to obtain a mixed solution A. Weigh 0.016 g of ZrOCl2·8H2O and place it in a double-jacketed beaker in a cell disruptor. Then add 20 mL of ethylene glycol and 100 μL of hydrazine hydrate, and mix and process for 30 min to obtain a mixed solution B. Then add all of the mixed solution B to the mixed solution A and mix evenly to obtain a mixed solution C. Weigh 0.136 g of the above-obtained Bi3TiNbO9 powder and add it to the mixed solution C. After stirring for 1 h, transfer the uniformly dispersed mixture to a 100 mL polytetrafluoroethylene reaction inner liner and place it in a constant-temperature drying oven for hydrothermal reaction at 200 °C for 24 h. After the reaction is completed, wash the obtained product with deionized water at a rotation speed of 6000 rpm until the upper liquid becomes clear, then centrifuge and wash it with absolute ethanol 5 times, and then filter the mixture to obtain a solid sample. Finally, place the above-obtained solid sample in a vacuum oven and dry it at 70 °C for 6 h to obtain a Bi3TiNbO9 / BaZrS3 composite material with a molar ratio of oxide perovskite to sulfide perovskite of about 3:1, denoted as BTNO:BZS = 3:1.
[0068] Perform phase characterization on the Bi3TiNbO9 / BaZrS3 composite material obtained in Example 1, and the results are as Figure 1 shown. It can be seen from Figure 1 this that the obtained composite material simultaneously contains the X-ray characteristic diffraction peaks of both Bi3TiNbO9 and BaZrS3 substances, which are in good agreement with the standard card number (JCPDS No.79-1550) of Bi3TiNbO9 and the standard card (JCPDS No.15-0327) of BaZrS3, indicating that the Bi3TiNbO9 / BaZrS3 composite material has been successfully prepared. Figure 2 and Figure 3 are the TEM images of the prepared Bi3TiNbO9 / BaZrS3 composite material. It can be clearly found from the figure that compared with single Bi3TiNbO9, there are filamentous or rod-like structures in the obtained composite material, and this structure is the BaZrS3 material, which further proves the successful synthesis of the composite material.
[0069] Example 2
[0070] First, weigh 2.50 g of Bi2O3, 0.24 g of TiO2, 0.50 g of Nb2O5, 10.50 g of NaCl, 10.30 g of KCl and 2 ml of absolute ethanol and place them in a ball milling jar. Grind them clockwise and counterclockwise on a ball mill for 2 h each to obtain a mixture. Then transfer the obtained mixture to an oven and dry it at 60 °C for 10 h to obtain a mixed powder. Then put the obtained mixed powder into a crucible and place it in a muffle furnace. Heat it to 850 °C at a heating rate of 5 °C / min and calcine it at this temperature for 6 h. Finally, wash the calcined solid powder with deionized water until there is no Cl - and dry it to obtain Bi3TiNbO9 powder.
[0071] Weigh 0.013 g of Ba(NO3)2 and 0.018 g of L-cysteine and place them in an 80 mL beaker. Add 20 mL of ethylene glycol and stir for 1 h to obtain a mixed solution A. Weigh 0.016 g of ZrOCl2·8H2O and place it in a double-jacketed beaker in a cell crusher. Then add 20 mL of ethylene glycol and 100 μL of hydrazine hydrate, and mix and process for 30 min to obtain a mixed solution B. Then add all of the mixed solution B to the mixed solution A, mix evenly to obtain a mixed solution C. Weigh 0.014 g of the above-obtained Bi3TiNbO9 powder and add it to the mixed solution C. After stirring for 1 h, transfer the uniformly dispersed mixture to a 100 mL polytetrafluoroethylene reaction inner liner and place it in a constant temperature drying oven for hydrothermal reaction at 200 °C for 24 h. After the reaction is completed, wash the obtained product with deionized water at a rotation speed of 6000 rpm until the upper liquid becomes clear, then wash it centrifugally with absolute ethanol 5 times, and then filter the mixture by suction to obtain a solid sample. Finally, place the above-obtained solid sample in a vacuum oven and dry it at 70 °C for 6 h to obtain a Bi3TiNbO9 / BaZrS3 composite material with a molar ratio of oxide perovskite to sulfide perovskite of about 0.3:1, denoted as BTNO:BZS = 0.3:1.
[0072] Example 3
[0073] First, weigh 2.50 g of Bi2O3, 0.24 g of TiO2, 0.50 g of Nb2O5, 10.50 g of NaCl, 10.30 g of KCl and 2 ml of absolute ethanol and place them in a ball milling jar. Grind them clockwise and counterclockwise on a ball mill for 2 h each to obtain a mixture. Then transfer the obtained mixture to an oven and dry it at 60 °C for 10 h to obtain a mixed powder. Then put the obtained mixed powder into a crucible and place it in a muffle furnace. Heat it to 850 °C at a heating rate of 5 °C / min and calcine it at this temperature for 6 h. Finally, wash the calcined solid powder with deionized water until there is no Cl - and dry it to obtain Bi3TiNbO9 powder.
[0074] Weigh 0.013 g of Ba(NO3)2 and 0.018 g of L-cysteine and place them in an 80 mL beaker. Add 20 mL of ethylene glycol and stir for 1 h to obtain mixture A. Weigh 0.016 g of ZrOCl2·8H2O and place it in the double-jacketed beaker of the cell crusher. Then add 20 mL of ethylene glycol and 100 μL of hydrazine hydrate, and mix and process for 30 min to obtain mixture B. Then add all of mixture B to mixture A and mix evenly to obtain mixture C. Then weigh 0.045 g of the obtained Bi3TiNbO9 powder and add it to mixture C. After stirring for 1 h, transfer the uniformly dispersed mixture to a 100 mL polytetrafluoroethylene reaction inner liner, place it in a constant temperature drying oven, and carry out hydrothermal reaction at 200 °C for 24 h. After the reaction is completed, wash the obtained product with deionized water at a rotation speed of 6000 rpm until the upper liquid becomes clear, then centrifuge and wash it with absolute ethanol 5 times, and then carry out suction filtration on the mixture to obtain a solid sample. Finally, place the obtained solid sample in a vacuum oven and dry it at 70 °C for 6 h to obtain a Bi3TiNbO9 / BaZrS3 composite material with a molar ratio of perovskite oxide to perovskite sulfide of about 1:1, denoted as BTNO:BZS = 1:1.
[0075] Example 4
[0076] First, weigh 2.50 g of Bi2O3, 0.24 g of TiO2, 0.50 g of Nb2O5, 10.50 g of NaCl, 10.30 g of KCl, and 2 mL of absolute ethanol and place them in a ball milling tank. Grind them clockwise and counterclockwise on the ball mill for 2 h each to obtain a mixture. Then transfer the obtained mixture to an oven and dry it at 60 °C for 10 h to obtain a mixed powder. Then place the obtained mixed powder in a crucible and place it in a muffle furnace. Heat it to 850 °C at a heating rate of 5 °C / min and calcine it at this temperature for 6 h. Finally, wash the calcined solid powder with deionized water until there is no Cl - and dry it to obtain Bi3TiNbO9 powder.
[0077] Weigh 0.013 g of Ba(NO3)2 and 0.018 g of L-cysteine and place them in an 80 mL beaker. Add 20 mL of ethylene glycol and stir for 1 h to obtain mixture A. Weigh 0.016 g of ZrOCl2·8H2O and place it in a double-jacketed beaker in a cell disruptor. Then add 20 mL of ethylene glycol and 100 μL of hydrazine hydrate, and mix for 30 min to obtain mixture B. Then add all of mixture B to mixture A and mix evenly to obtain mixture C. Weigh 0.091 g of the obtained Bi3TiNbO9 powder and add it to mixture C. After stirring for 1 h, transfer the evenly dispersed mixture to a 100 mL polytetrafluoroethylene reaction liner, place it in a constant temperature drying oven, and carry out hydrothermal reaction at 200 °C for 24 h. After the reaction is completed, wash the obtained product with deionized water at a rotation speed of 6000 rpm until the upper liquid becomes clear, then centrifuge and wash it with absolute ethanol 5 times, and then filter the mixture to obtain a solid sample. Finally, place the obtained solid sample in a vacuum oven and dry it at 70 °C for 6 h to obtain a Bi3TiNbO9 / BaZrS3 composite material with a molar ratio of perovskite oxide to perovskite sulfide of about 2:1, denoted as BTNO:BZS = 2:1.
[0078] Example 5
[0079] First, weigh 2.50 g of Bi2O3, 0.24 g of TiO2, 0.50 g of Nb2O5, 10.50 g of NaCl, 10.30 g of KCl, and 2 mL of absolute ethanol and place them in a ball milling tank. Grind them on a ball mill clockwise and counterclockwise for 2 h each to obtain a mixture. Then transfer the obtained mixture to an oven and dry it at 60 °C for 10 h to obtain a mixed powder. Then place the obtained mixed powder in a crucible, place it in a muffle furnace, and heat it to 850 °C at a heating rate of 5 °C / min, and calcine it at this temperature for 6 h. Finally, wash the calcined solid powder with deionized water until there is no Cl - and dry it to obtain Bi3TiNbO9 powder.
[0080] Weigh 0.013 g of Ba(NO3)2 and 0.018 g of L-cysteine and place them in an 80 mL beaker. Add 20 mL of ethylene glycol and stir for 1 h to obtain mixture A. Weigh 0.016 g of ZrOCl2·8H2O and place it in the double-jacketed beaker of the cell crusher. Then add 20 mL of ethylene glycol and 100 μL of hydrazine hydrate, and mix for 30 min to obtain mixture B. Then add all of mixture B to mixture A and mix evenly to obtain mixture C. Weigh 0.181 g of the obtained Bi3TiNbO9 powder and add it to mixture C. After stirring for 1 h, transfer the evenly dispersed mixture to a 100 mL polytetrafluoroethylene reaction liner, place it in a constant temperature drying oven, and carry out hydrothermal reaction at 200 °C for 24 h. After the reaction is completed, wash the obtained product with deionized water at a rotation speed of 6000 rpm until the upper liquid becomes clear, then centrifuge and wash it with absolute ethanol 5 times, and then filter the mixture to obtain a solid sample. Finally, place the obtained solid sample in a vacuum oven and dry it at 70 °C for 6 h to obtain a Bi3TiNbO9 / BaZrS3 composite material with a molar ratio of perovskite oxide to perovskite sulfide of about 4:1, denoted as BTNO:BZS = 4:1.
[0081] Example 6
[0082] First, weigh 2.50 g of Bi2O3, 0.24 g of TiO2, 0.50 g of Nb2O5, 10.50 g of NaCl, 10.30 g of KCl, and 2 ml of absolute ethanol and place them in a ball milling jar. Grind them on the ball mill clockwise and counterclockwise for 2 h each to obtain a mixture. Then transfer the obtained mixture to an oven and dry it at 60 °C for 10 h to obtain a mixed powder. Then place the obtained mixed powder in a crucible, place it in a muffle furnace, and heat it to 850 °C at a heating rate of 5 °C / min, and calcine it at this temperature for 6 h. Finally, wash the calcined solid powder with deionized water until there is no Cl - and dry it to obtain Bi3TiNbO9 powder.
[0083] Weigh 0.013 g of Ba(NO3)2 and 0.018 g of L-cysteine and place them in an 80 mL beaker. Add 20 mL of ethylene glycol and stir for 1 h to obtain mixture A. Weigh 0.016 g of ZrOCl2·8H2O and place it in a double-jacketed beaker in a cell crusher. Then add 20 mL of ethylene glycol and 100 μL of hydrazine hydrate, and mix for 30 min to obtain mixture B. Then add all of mixture B to mixture A and mix evenly to obtain mixture C. Weigh 0.227 g of the above-obtained Bi3TiNbO9 powder and add it to mixture C. After stirring for 1 h, transfer the evenly dispersed mixture to a 100 mL polytetrafluoroethylene reaction liner and place it in a constant-temperature drying oven for hydrothermal reaction at 200 °C for 24 h. After the reaction is completed, wash the obtained product with deionized water at a rotation speed of 6000 rpm until the upper liquid becomes clear, then centrifuge and wash with absolute ethanol 5 times, and then filter the mixture to obtain a solid sample. Finally, place the above-obtained solid sample in a vacuum oven and dry it at 70 °C for 6 h to obtain a Bi3TiNbO9 / BaZrS3 composite material with a molar ratio of perovskite oxide to perovskite sulfide of about 5:1, denoted as BTNO:BZS = 5:1.
[0084] Example 7
[0085] First, weigh 2.50 g of Bi2O3, 0.24 g of TiO2, 0.50 g of Nb2O5, 10.50 g of NaCl, 10.30 g of KCl and 2 ml of absolute ethanol and place them in a ball mill jar. Grind them clockwise and counterclockwise on the ball mill for 2 h each to obtain a mixture. Then transfer the obtained mixture to an oven and dry it at 60 °C for 10 h to obtain a mixed powder. Then place the obtained mixed powder in a crucible and heat it in a muffle furnace at a heating rate of 5 °C / min to 850 °C and calcine it at this temperature for 6 h. Finally, wash the calcined solid powder with deionized water until there is no Cl - and dry it to obtain Bi3TiNbO9 powder.
[0086] Weigh 0.013 g of Ba(NO3)2 and 0.018 g of L-cysteine and place them in an 80 mL beaker. Add 20 mL of ethylene glycol and stir for 1 h to obtain mixture A. Weigh 0.016 g of ZrOCl2·8H2O and place it in the double-jacketed beaker of the cell crusher. Then add 20 mL of ethylene glycol and 100 μL of hydrazine hydrate, and mix and process for 30 min to obtain mixture B. Then add all of mixture B to mixture A and mix evenly to obtain mixture C. Weigh 0.453 g of the obtained Bi3TiNbO9 powder and add it to mixture C. After stirring for 1 h, transfer the uniformly dispersed mixture to a 100 mL polytetrafluoroethylene reaction inner liner, place it in a constant temperature drying oven, and carry out hydrothermal reaction at 200 °C for 24 h. After the reaction is completed, wash the obtained product with deionized water at a rotation speed of 6000 rpm until the upper liquid becomes clear, then wash it by centrifugation with absolute ethanol 5 times, and then carry out suction filtration on the mixture to obtain a solid sample. Finally, place the obtained solid sample in a vacuum oven and dry it at 70 °C for 6 h to obtain a Bi3TiNbO9 / BaZrS3 composite material with a molar ratio of perovskite oxide to perovskite sulfide of about 10:1, denoted as BTNO:BZS = 10:1.
[0087] Example 8
[0088] First, weigh 0.079 g of C6H8O7·H2O and 0.776 g of Bi(NO3)3·5H2O and place them in a 50 mL beaker. Then add 0.425 mL of tetrabutyl titanate, 4 mL of DMF, 6 mL of absolute ethanol and stir until the solution becomes clear. Then add 1.0 g of polyvinylpyrrolidone (PVP) and stir to dissolve to obtain a mixture. Then dry the obtained mixture in a vacuum oven at 65 °C for 12 h to obtain a mixed powder. Then put the obtained mixed powder into a crucible and place it in a muffle furnace. Heat it to 650 °C at a heating rate of 8 °C / min and calcine it at this temperature for 4 h to obtain Bi4Ti3O 12 powder.
[0089] Weigh 0.013 g of Ba(NO3)2 and 0.018 g of L-cysteine and place them in an 80 mL beaker. Add 22 mL of ethylene glycol and stir for 1.5 h to obtain mixture A. Weigh 0.016 g of ZrOCl2·8H2O and place it in the double-jacketed beaker of the cell crusher. Then add 22 mL of ethylene glycol and 100 μL of hydrazine hydrate, and mix and process for 35 min to obtain mixture B. Then add all of mixture B to mixture A and mix evenly to obtain mixture C. Weigh 0.176 g of the obtained Bi4Ti3O 12The powder was added to the mixed solution C. After stirring for 1.5 h, the well-dispersed mixture was transferred to a 100 mL polytetrafluoroethylene reaction liner and hydrothermally reacted at 220 °C in a constant-temperature drying oven for 24 h. After the reaction was completed, the obtained product was washed with deionized water at a rotation speed of 6000 rpm until the upper liquid became clear, and then centrifugally washed with absolute ethanol 6 times. Then the mixture was filtered by suction to obtain a solid sample; finally, the obtained solid sample was placed in a vacuum drying oven and dried at 75 °C for 5 h to obtain a Bi4Ti3O 12 / BaZrS3 composite material with a molar ratio of perovskite oxide to perovskite sulfide of about 3:1.
[0090] The Bi4Ti3O 12 / BaZrS3 micro-nano composite material synthesized in Example 8 was subjected to phase characterization, and the results are as Figure 5 shown. As can be seen from the figure, the obtained composite material simultaneously has the X-ray characteristic diffraction peaks of both Bi4Ti3O 12 and BaZrS3 substances, and it basically coincides with the standard card number (JCPDS No.80-2143) of Bi4Ti3O 12 and the standard card (JCPDS No.15-0327) of BaZrS3, indicating that the Bi4Ti3O 12 / BaZrS3 composite material was successfully prepared.
[0091] Example 9
[0092] First, 2.50 g of Bi2O3, 0.24 g of TiO2, 0.50 g of Nb2O5, 10.50 g of NaCl, 10.30 g of KCl and 2 ml of absolute ethanol were weighed and placed in a ball milling tank. After milling clockwise and counterclockwise on a ball mill for 2 h each, a mixture was obtained; then the obtained mixture was transferred to an oven and dried at 65 °C for 10 h to obtain a mixed powder; then the obtained mixed powder was put into a crucible and heated in a muffle furnace at a heating rate of 6 °C / min to 850 °C and calcined at this temperature for 6 h. Finally, the solid powder obtained after calcination was washed with hot deionized water until there was no Cl - and dried to obtain Bi3TiNbO9 powder.
[0093] Weigh 0.011 g of Sr(NO3)2 and 0.018 g of L-cysteine and place them in an 80 mL beaker. Add 22 mL of ethylene glycol and stir for 1.5 h to obtain a mixed solution A. Weigh 0.016 g of ZrOCl2·8H2O and place it in a double-jacketed beaker in a cell crusher. Then add 22 mL of ethylene glycol and 100 μL of hydrazine hydrate, and mix for 35 min to obtain a mixed solution B. Then add all of the mixed solution B to the mixed solution A, mix evenly to obtain a mixed solution C. Weigh 0.136 g of the obtained Bi3TiNbO9 powder and add it to the mixed solution C. After stirring for 1.5 h, transfer the uniformly dispersed mixture to a 100 mL polytetrafluoroethylene reaction liner, and place it in a constant temperature drying oven for hydrothermal reaction at 220 °C for 24 h. After the reaction is completed, wash the obtained product with deionized water at a rotation speed of 6000 rpm until the upper liquid becomes clear, then centrifuge and wash it with absolute ethanol 6 times, and then filter the mixture to obtain a solid sample. Finally, place the obtained solid sample in a vacuum oven and dry it at 75 °C for 5 h to obtain a Bi3TiNbO9 / SrZrS3 composite material with a molar ratio of perovskite oxide to perovskite sulfide of approximately 3:1.
[0094] Perform phase characterization on the synthesized Bi3TiNbO9 / SrZrS3 micro-nano composite material in the example. As shown in Figure 6 It can be seen that the diffraction peaks of the obtained composite material are consistent with the X-ray characteristic diffraction peaks of Bi3TiNbO9 and SrZrS3, and it basically coincides with the standard card number (JCPDS No.79-1550) of Bi3TiNbO9 and the standard card (JCPDS No.73-0846) of SrZrS3, indicating that the Bi3TiNbO9 / SrZrS3 composite material is successfully prepared.
[0095] Example 10
[0096] First, weigh 3.64 g of Bi(NO3)3·5H2O and 0.663 g of (NH4)6Mo7O 24 ·4H2O in an 80 mL beaker, then add 30 mL of ethylene glycol, and while stirring with a glass rod, add 5% NH3·H2O to adjust the pH to 8-9. Then pour the solution into a 100 mL polytetrafluoroethylene liner and place it in an oven for hydrothermal reaction. The set conditions are reaction at 140 °C for 20 h. After the reaction is completed, wash it with deionized water and ethanol twice each, and finally place it in an oven and dry it for 6 h to obtain the final sample of Bi2MoO6 powder.
[0097] Weigh 0.010 g of Ca(NO3)2 and 0.018 g of L-cysteine and place them in an 80 mL beaker. Add 22 mL of ethylene glycol and stir for 1.5 h to obtain a mixed solution A. Weigh 0.016 g of ZrOCl2·8H2O and place it in a double-jacketed beaker in a cell crusher. Then add 22 mL of ethylene glycol and 100 μL of hydrazine hydrate, and mix and process for 35 min to obtain a mixed solution B. Then add all of the mixed solution B to the mixed solution A, mix evenly to obtain a mixed solution C. Weigh 0.092 g of the obtained Bi2MoO6 powder and add it to the mixed solution C. After stirring for 1.5 h, transfer the uniformly dispersed mixture to a 100 mL polytetrafluoroethylene reaction inner liner, and place it in a constant temperature drying oven for hydrothermal reaction at 220 °C for 24 h. After the reaction is completed, wash the obtained product with deionized water at a rotation speed of 6000 rpm until the upper liquid becomes clear, then centrifuge and wash with absolute ethanol 6 times, and then filter the mixture by suction to obtain a solid sample. Finally, place the obtained solid sample in a vacuum oven and dry it at 75 °C for 5 h to obtain a Bi2MoO6 / CaZrS3 composite material with a molar ratio of oxide perovskite to sulfide perovskite of approximately 3:1.
[0098] Example 11
[0099] First, place 2.425 g of Bi(NO3)3·5H2O and 5 mL of CH3COOH in a 25 mL beaker and stir for 5 min to form solution A. Then place 0.825 g of Na2WO4·2H2O and 45 mL of deionized water in a 100 mL beaker and stir for 5 min to form solution B. Finally, pour solution A into solution B, adjust the pH to 2, stir for 1 h to obtain a mixed solution, pour the mixed solution into a 100 mL polytetrafluoroethylene inner liner, and set the reaction conditions to react at 140 °C for 20 h. After the reaction is completed, wash it three times with deionized water and place it in an oven to dry for 10 h. Finally, perform calcination treatment in a muffle furnace. The calcination conditions are to calcine at a temperature of 300 °C for 4 h, and the heating rate is 5 °C / min. After the reaction is completed, obtain Bi2WO6 powder.
[0100] Weigh 0.011 g of Sr(NO3)2 and 0.018 g of L-cysteine and place them in an 80 mL beaker. Add 22 mL of ethylene glycol and stir for 1.5 h to obtain mixture A. Weigh 0.016 g of ZrOCl2·8H2O and place it in the double-jacketed beaker of the cell crusher. Then add 22 mL of ethylene glycol and 100 μL of hydrazine hydrate, and mix for 35 min to obtain mixture B. Then add all of mixture B to mixture A and mix evenly to obtain mixture C. Weigh 0.105 g of the obtained Bi2WO6 powder and add it to mixture C. After stirring for 1.5 h, transfer the uniformly dispersed mixture to a 100 mL polytetrafluoroethylene reaction liner, place it in a constant-temperature drying oven, and carry out a hydrothermal reaction at 220 °C for 24 h. After the reaction is completed, wash the obtained product with deionized water at a rotation speed of 6000 rpm until the upper liquid becomes clear, then wash it centrifugally with absolute ethanol 6 times, and then filter the mixture by suction to obtain a solid sample. Finally, place the obtained solid sample in a vacuum oven and dry it at 75 °C for 5 h to obtain a Bi2WO6 / SrZrS3 composite material with a molar ratio of perovskite oxide to perovskite sulfide of approximately 3:1.
[0101] Example 12
[0102] First, weigh 0.194 g of Bi(NO3)3·5H2O and 0.032 g of Na2CrO4 and place them in a 100 mL beaker. Then add 20 mL of deionized water, stir for 30 min, and pour it into a 100 mL polytetrafluoroethylene liner for hydrothermal reaction. The reaction conditions are set to react at 180 °C for 20 h. After the reaction is completed, wash it 3 times with deionized water, and finally dry it to obtain Bi2CrO6 powder.
[0103] Weigh 0.013 g of Ba(NO3)2 and 0.018 g of L-cysteine and place them in an 80 mL beaker. Add 22 mL of ethylene glycol and stir for 1.5 h to obtain a mixed solution A. Weigh 0.017 g of tetrabutyl titanate and place it in a double-jacketed beaker in a cell crusher. Then add 22 mL of ethylene glycol and 100 μL of hydrazine hydrate, and mix for 35 min to obtain a mixed solution B. Then add all of the mixed solution B to the mixed solution A and mix evenly to obtain a mixed solution C. Weigh 0.085 g of the obtained Bi2CrO6 powder and add it to the mixed solution C. After stirring for 1.5 h, transfer the uniformly dispersed mixture to a 100 mL polytetrafluoroethylene reaction liner and place it in a constant temperature drying oven for hydrothermal reaction at 220 °C for 24 h. After the reaction is completed, wash the obtained product with deionized water at a rotation speed of 6000 rpm until the upper liquid becomes clear, then centrifuge and wash it with absolute ethanol 6 times, and then filter the mixture to obtain a solid sample. Finally, place the obtained solid sample in a vacuum drying oven and dry it at 75 °C for 5 h to obtain a Bi2CrO6 / BaTiS3 composite material with a molar ratio of perovskite oxide to perovskite sulfide of about 3:1.
[0104] Example 13
[0105] First, weigh 0.079 g of C6H8O7·H2O and 0.776 g of Bi(NO3)3·5H2O and place them in a 50 mL beaker. Then add 0.425 mL of tetrabutyl titanate, 4 mL of DMF, 6 mL of absolute ethanol and stir until the solution becomes clear. Then add 1.0 g of polyvinylpyrrolidone (PVP) and stir to dissolve to obtain a mixture. Then dry the obtained mixture in a vacuum drying oven at 65 °C for 12 h to obtain a mixed powder. Then place the obtained mixed powder in a crucible and heat it in a muffle furnace at a heating rate of 8 °C / min to 650 °C and calcine it at this temperature for 4 h to obtain Bi4Ti3O 12 powder.
[0106] Weigh 0.013 g of Ba(NO3)2 and 0.018 g of L-cysteine and place them in an 80 mL beaker. Add 22 mL of ethylene glycol and stir for 1.5 h to obtain a mixed solution A. Weigh 0.014 mL of tetrabutyl titanate and place it in a double-jacketed beaker in a cell crusher. Then add 22 mL of ethylene glycol and 100 μL of hydrazine hydrate, and mix for 35 min to obtain a mixed solution B. Then add all of the mixed solution B to the mixed solution A and mix evenly to obtain a mixed solution C. Weigh 0.176 g of the obtained Bi4Ti3O 12The powder was added to the mixed solution C. After stirring for 1.5 h, the uniformly dispersed mixture was transferred into a 100 mL polytetrafluoroethylene reaction inner liner and placed in a constant-temperature drying oven for hydrothermal reaction at 220 °C for 24 h. After the reaction was completed, the obtained product was washed with deionized water at a rotation speed of 6000 rpm until the upper-layer liquid became clear, then centrifugally washed with absolute ethanol 6 times, and then the mixture was filtered by suction to obtain a solid sample; finally, the obtained solid sample was placed in a vacuum drying oven and dried at 75 °C for 5 h to obtain a Bi4Ti3O 12 / BaTiS3 composite material with a molar ratio of perovskite oxide to perovskite sulfide of about 3:1.
[0107] Example 14
[0108] First, 0.221 g of Bi(NO3)3·5H2O, 0.037 g of Fe(NO3)3·9H2O and 0.094 g of tetrabutyl titanate were weighed and dissolved in 5 mL of HNO3 (4 mol / L) and stirred for 20 min to form a transparent solution. Then, 1.6 mol / L NaOH solution was added to the above solution until the total volume reached 40 mL. A yellow suspension was formed. After stirring for 2 h, the suspension was transferred to a 50 mL Teflon-lined stainless steel autoclave, and the hydrothermal reaction conditions were set to react at 200 °C for 24 h. After the reaction was completed, the autoclave was naturally cooled to room temperature. Finally, the precipitate was washed three times with deionized water and ethanol respectively. The final nanoparticles Bi5FeTi3O were obtained after drying at 70 °C for 12 h. 15 。
[0109] 0.013 g of Ba(NO3)2 and 0.018 g of L-cysteine were weighed and placed in an 80 mL beaker, and 22 mL of ethylene glycol was added. After stirring for 1.5 h, a mixed solution A was obtained; 0.019 g of Hf(SO4)2 was weighed and placed in a double-jacketed beaker in a cell disruptor, and then 22 mL of ethylene glycol and 100 μL of hydrazine hydrate were added. After mixing and treating for 35 min, a mixed solution B was obtained; then the whole mixed solution B was added to the mixed solution A and mixed evenly to obtain a mixed solution C; and then 0.223 g of the above-obtained Bi5FeTi3O 15 powder was added to the mixed solution C. After stirring for 1.5 h, the uniformly dispersed mixture was transferred into a 100 mL polytetrafluoroethylene reaction inner liner and placed in a constant-temperature drying oven for hydrothermal reaction at 220 °C for 24 h. After the reaction was completed, the obtained product was washed with deionized water at a rotation speed of 6000 rpm until the upper-layer liquid became clear, then centrifugally washed with absolute ethanol 6 times, and then the mixture was filtered by suction to obtain a solid sample; finally, the obtained solid sample was placed in a vacuum drying oven and dried at 75 °C for 5 h to obtain a Bi5FeTi3O with a molar ratio of perovskite oxide to perovskite sulfide of about 3:1. 15 / BaHfS3 composite material.
[0110] Example 15
[0111] Weigh 0.073 g of tetrabutyl titanate, 0.243 g of Bi(NO3)3·5H2O and 0.087 g of Fe(NO3)3·9H2O and place them in a 50 mL beaker. Add 5 mL of HNO3 (4 mol / L) and then stir magnetically for 30 min until all the raw materials are dissolved. Then add 10 mL of NaOH (1.6 mol / L) and pour all of it into a 50 mL polytetrafluoroethylene inner liner for hydrothermal reaction. The blast drying oven is set at 200 °C for 24 h. After the reaction is completed, wash it twice with deionized water and ethanol respectively, and dry it to obtain Bi7Fe3Ti3O 21 powder.
[0112] Weigh 0.013 g of Ba(NO3)2 and 0.006 g of L-cysteine and place them in an 80 mL beaker. Add 22 mL of ethylene glycol and stir for 1.5 h to obtain a mixed solution A. Weigh 0.016 g of ZrOCl2·8H2O and 0.013 g of thiourea and place them in a double-jacketed beaker in a cell crusher. Then add 22 mL of ethylene glycol and 100 μL of hydrazine hydrate, and mix and process for 35 min to obtain a mixed solution B. Then add all of the mixed solution B to the mixed solution A, mix evenly to obtain a mixed solution C. Then weigh 0.317 g of the Bi7Fe3Ti3O 21 powder obtained above and add it to the mixed solution C. After stirring for 1.5 h, transfer the uniformly dispersed mixture to a 100 mL polytetrafluoroethylene reaction inner liner and place it in a constant temperature drying oven for hydrothermal reaction at 220 °C for 24 h. After the reaction is completed, wash the obtained product with deionized water at a rotation speed of 6000 rpm until the upper liquid becomes clear, then wash it by centrifugation with absolute ethanol 6 times, and then filter the mixture by suction to obtain a solid sample. Finally, place the obtained solid sample in a vacuum oven and dry it at 75 °C for 5 h to obtain a Bi7Fe3Ti3O 21 / BaZrS3 composite material.
[0113] Comparative Example 1
[0114] Weigh 2.50 g of Bi2O3, 0.24 g of TiO2, 0.50 g of Nb2O5, 10.50 g of NaCl, 10.30 g of KCl and 2 ml of absolute ethanol and place them in a ball milling jar. Grind them on a ball mill clockwise and counterclockwise for 2 h each to obtain a mixture; then transfer the obtained mixture to an oven and dry it at 60 °C for 10 h to obtain a mixed powder; then put the obtained mixed powder into a crucible and place it in a muffle furnace. Heat it to 850 °C at a heating rate of 5 °C / min and calcine it at this temperature for 6 h. Finally, wash the calcined solid powder with deionized water until there is no Cl - , after drying, the Bi3TiNbO9 material is obtained, denoted as BTNO.
[0115] Comparative Example 2
[0116] Weigh 0.079 g of C6H8O7·H2O and 0.728 g of Bi(NO3)3·5H2O and place them in a 50 mL beaker. Then add 0.425 mL of tetrabutyl titanate, 4 mL of DMF, 6 mL of absolute ethanol and stir until the solution becomes clear. After that, add 1.0 g of polyvinylpyrrolidone (PVP) and stir to dissolve to obtain a mixture. Then dry the obtained mixture in a vacuum oven at 65 °C for 12 h to obtain a mixed powder. Then put the obtained mixed powder into a crucible and place it in a muffle furnace. Heat it to 650 °C at a heating rate of 8 °C / min and calcine it at this temperature for 4 h to obtain the Bi4Ti3O 12 material.
[0117] Comparative Example 3
[0118] Mix the BaCO3 powder and ZrO2 powder evenly. Place the powder mixture in a high-temperature reaction furnace, evacuate the reaction furnace to make the background vacuum degree < 0.1 Pa; then introduce CS2 vapor under vacuum conditions for temperature-raising sulfidation reaction; heat the high-temperature reaction furnace to 1000 °C, adjust the pressure in the high-temperature reaction furnace to 30 Pa, keep it warm for 1 h, and then cool it to room temperature. After the sulfidation reaction, the BaZrS3 powder is obtained, denoted as BZS.
[0119] Comparative Example 4
[0120] Weigh 0.027 g of the Bi3TiNbO9 powder obtained in Comparative Example 1 and place it in an 80 mL beaker. Add 20 mL of H2O and stir magnetically for 1 h. Then weigh 0.003 g of the BaZrS3 powder obtained in Comparative Example 3 and add it to this beaker and stir for 4 h to obtain a physically mixed Bi3TiNbO9+BaZrS3 composite material. Among them, the molar ratio of the oxide perovskite to the sulfide perovskite is 3:1, denoted as BTNO+BZS(3:1).
[0121] Comparative Example 5
[0122] Weigh 0.136 g of the Bi3TiNbO9 powder obtained in Comparative Example 1 and disperse it in 15 mL of N,N-dimethylformamide solution. Add 0.068 g of ZnCl2, and ultrasonically disperse for 10 min. Then add 0.029 g of InCl3·4H2O, continue ultrasonic treatment for 10 min, and then add 0.015 g of thioacetamide, and continue ultrasonic treatment for 5 min. Add 3 mL of glycerol to the above mixed solution, and ultrasonically treat for 5 min. Then transfer it to a reaction kettle and react at 200 °C for 24 h. After cooling the obtained product to room temperature, perform suction filtration, and then dry at 70 °C for 6 h to obtain a Bi3TiNbO9 / ZnIn2S4 composite material with a molar ratio of Bi3TiNbO9 to ZnIn2S4 of about 3:1.
[0123] Application Example 1
[0124] Photocatalytic preparation of H2O2:
[0125] Weigh 0.01 g of the materials prepared in Examples 1-15 and Comparative Examples 1-5 respectively and place them in different beakers. Then add 15 ml of deionized water respectively. After being dispersed evenly, pass dry air through them and stir for 1 h. Finally, place the obtained mixture under simulated sunlight for photocatalytic reaction. After the reaction is completed, filter the mixed solution with a filter head and collect the filtrate. Then measure 1 ml of the filtrate and place it in a centrifuge tube. Then use a pipette to transfer 3 ml of cerium sulfate solution with a concentration of 0.001 mol / L and 7 ml of sulfuric acid solution with a concentration of 0.15 mol / L into the centrifuge tube for reaction. Finally, use a UV-visible spectrophotometer to detect the absorbance to measure the photocatalytic H2O2 production performance of the prepared materials.
[0126] Application Example 2
[0127] Photocatalytic degradation of tetracycline hydrochloride:
[0128] Weigh 0.01 g of the materials prepared in Examples 1-15 and Comparative Examples 1-5 respectively and place them in different photoreactors. Then add 20 mL of tetracycline hydrochloride solution respectively, stir and disperse evenly, stir for 1 h under dark conditions, and then turn on the xenon lamp power supply for photocatalytic reaction for 1 h. After the reaction is completed, filter the mixed solution with a filter head and collect the filtrate. Then measure 10 mL of the filtrate and place it in a centrifuge tube. Finally, use a UV-visible spectrophotometer to detect the absorbance to judge the photocatalytic degradation performance of the materials for tetracycline.
[0129] Application Example 3
[0130] Photocatalytic degradation of pesticide residues:
[0131] Weigh 0.01 g of each of the materials prepared in Examples 1-15 and Comparative Examples 1-5 in a photoreactor and place them in different reactors. Then add 20 mL of the glyphosate solution to be degraded. First, introduce air and stir magnetically for 1 h in the dark to form a uniform suspension system, and then turn on the light and react for 1 h under light conditions. After the reaction, take samples and place them in centrifuge tubes. Then place the centrifuge tubes in a centrifuge and centrifuge at 4000 rpm for 10 min. Finally, take 4.5 mL of the supernatant and transfer it to a 10 mL colorimetric tube, add 0.50 mL of the molybdenum antimony resistance reagent and shake well. After color development for 30 min, measure the absorbance at a wavelength of 710 nm using a UV-visible spectrophotometer.
[0132] The test results of Examples 1-3 are shown in the following table:
[0133]
[0134] Note: The above photocatalytic performance was tested without a sacrificial reagent.
Claims
1. A composite material of oxide perovskite / sulfide perovskite, characterized in that: The composite material includes an oxide perovskite material and a sulfide perovskite material epitaxially grown on the oxide perovskite material.
2. The composite material according to claim 1, characterized in that: The perovskite oxide materials are one or more of Bi2MoO6, Bi2WO6, Bi2CrO6, Bi3TiNbO9, Bi3Fe 0.5 Nb 1.5 O9, Bi4Ti3O 12 , Bi5FeTi3O 15 , Bi6Fe2Ti3O 18 , Bi7Fe3Ti3O 21 and preferably one or more of Bi2MoO6, Bi3TiNbO9, Bi4Ti3O 12 or Bi5FeTi3O 15 ; The sulfide perovskite material is one or more of CaZrS3, CaTiS3, CaHfS3, SrZrS3, SrTiS3, SrHfS3, BaZrS3, BaTiS3, BaHfS3, preferably CaZrS3, SrZrS3, SrTiS3 or BaZrS3.
3. The composite material according to claim 1 or 2, characterized in that: In the composite material, the molar ratio of the oxide perovskite material to the sulfide perovskite material is 0.5 - 10:1, preferably 1 - 8:1, more preferably 2 - 5:1; The particle size of the composite material is 0.1 - 5 μm, preferably 0.3 - 4 μm, more preferably 0.5 - 3 μm.
4. The composite material according to any one of claims 1-3, characterized in that: The composite material is one or more of Bi2MoO6 / CaZrS3, Bi2WO6 / SrZrS3, Bi2CrO6 / BaTiS3, Bi3TiNbO9 / BaZrS3, Bi3TiNbO9 / SrZrS3, Bi4Ti3O 12 / BaZrS3, Bi4Ti3O 12 / BaTiS3, Bi5FeTi3O 15 / SrTiS3, Bi5FeTi3O 15 / BaHfS3, Bi7Fe3Ti3O 21 / BaZrS3, preferably Bi2MoO6 / CaZrS3, Bi3TiNbO9 / BaZrS3, Bi3TiNbO9 / SrZrS3 or Bi4Ti3O 12 / BaZrS3.
5. A method for preparing a composite material of oxide perovskite / sulfide perovskite or a method for preparing a composite material of oxide perovskite / sulfide perovskite according to any one of claims 1-4, characterized in that, This method includes the following steps: 1) Mix at least two of a bismuth source, a molybdenum source, a tungsten source, a chromium source, a titanium source, a niobium source, and an iron source with a metal halide salt, optionally an auxiliary agent, and ethanol, first perform grinding or dissolution and dispersion treatment, and then perform calcination and / or drying treatment to obtain an oxide perovskite micro-nano material; 2) Mix at least one of a calcium source, a barium source, and a strontium source and at least one of a zirconium source, a hafnium source, and a titanium salt with a sulfur source, a reducing agent, and a solvent, or perform dissolution and dispersion to obtain a sulfide perovskite precursor solution; 3) Add the oxide perovskite micro-nano material to the sulfide perovskite precursor solution for hydrothermal reaction, and after the reaction is completed, obtain an oxide perovskite / sulfide perovskite composite material.
6. The method according to claim 5, characterized in that: In step 1), the bismuth source is one or more of Bi2O3, Bi(NO3)3·5H2O, BiBr3, BiCl3, C6H9BiO6, C6H5BiO7; In step 1), the molybdenum source is one or more of (NH4)6Mo7O 24 ·4H2O, Na2MoO4·2H2O, K2MoO4·2H2O; In step 1), the tungsten source is one or more of (NH4)6W7O 24 ·6H2O, Na2WO4·2H2O, and K2WO4·2H2O; In step 1), the chromium source is one or more of Na2CrO4, K2CrO4, MgCrO4; In step 1), the titanium source is one or more of TiO2, tetrabutyl titanate, titanium isopropoxide, potassium oxalate titanate; In step 1), the niobium source is one or more of Nb2O5, C 10 H 25 NbO5, NbCl5; In step 1), the iron source is one or more of Fe(NO3)3·9H2O, FeCl3·6H2O, Fe2O3, Fe2(SO4)3·7H2O; In step 1), the metal halide salt is one or more of NaCl, KCl, LiCl, NaBr, KBr, NaI, KI; In step 1), the auxiliary agent is one of citric acid monohydrate (C6H8O7·H2O), polyvinylpyrrolidone (PVP), acetic acid (CH3COOH); 7. The method according to claim 5 or 6, characterized in that: In step 2), the sulfur source is one or more of sulfur powder, thiourea, L-cysteine, methionine, CS2, (NH4)2S, CH3CSNH2, Na2S2O3; In step 2), the calcium source is one or more of Ca(NO3)2, CaCl2, CaI2, CaBr2, Ca(HSO3)2, Ca(ClO)2; In step 2), the zirconium source is one or more of Zr(SO4)2, Zr(NO3)4, ZrOCl2·8H2O, ZrCl4, and Zr(C6H5O7)2; In step 2), the barium source is one or more of Ba(NO3)2, BaCl2, BaS, and Ba(CH3COO)2; In step 2), the strontium source is one or more of Sr(NO3)2, SrCl2, SrBr2, and SrI2; In step 2), the hafnium source is one or more of HfOCl2·8H2O, Hf(SO4)2, and HfCl4; In step 2), the titanium salt is one or more of TiO2, tetrabutyl titanate, titanium isopropoxide, and potassium oxalate titanate; 8. The method according to any one of claims 5-7, characterized in that: In step 2), the reducing agent is one or more of hydrazine hydrate, Na2SO3, H2C2O4, FeSO4, NaBH4, and KBH4; In step 2), the solvent is one or more of ethylene glycol, DMF, deionized water, ethanol, and isopropanol; 9. The method according to any one of claims 5-8, characterized in that: In step 1), the temperature of the calcination treatment is 100 - 900 °C, preferably 120 - 850 °C, and the time of the calcination treatment is 1 - 12 h, preferably 3 - 10 h; In step 3), the temperature of the reaction is 100 - 250 °C, preferably 150 - 220 °C; the time of the reaction is 5 - 48 h, preferably 8 - 36 h; In step 3), the addition amounts of the oxide perovskite micro / nanomaterials and the sulfide perovskite precursor solution are such that the molar ratio of the oxide perovskite substances to the sulfide perovskite substances is 1 - 12:1, preferably 1.5 - 10:1, and more preferably 2 - 6:
1.
10. Use of an oxide perovskite / sulfide perovskite composite material, or use of an oxide perovskite / sulfide perovskite composite material according to any one of claims 1-4, or use of an oxide perovskite / sulfide perovskite composite material prepared by the method according to any one of claims 5-9, characterized in that: The oxide perovskite / sulfide perovskite composite material is used in the field of photocatalysis; Preferably, the oxide perovskite / sulfide perovskite composite material is used for photocatalytic synthesis of H2O2, photocatalytic production of H2, photocatalytic synthesis of ammonia, photocatalytic degradation of pesticide residues, or dye molecules.