Ternary positive electrode material, preparation method thereof, positive electrode and battery
By adopting a self-supported microcage structure design in the high-nickel ternary positive electrode material, the structural expansion problem caused by lithium ions precipitation and dissolution of the material during charging and discharging is solved, and the circulation performance of the battery and the stability of the material are significantly improved.
Patent Information
- Application Number
- CN202510668521.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-23
- Publication Date
- 2025-06-20
- Estimated Expiration
- 2045-05-23
AI Technical Summary
During the charging and discharging process, the high-nickel ternary cathode material causes structural expansion due to lithium ions precipitation and dissolution, which accelerates material deterioration and affects the cycling performance of the battery.
The high-nickel ternary cathode material is designed with a self-supported microcage structure. The microcage structure has a cavity inside and is filled with conductive agent. Through this structural design, the volume expansion or contraction of the material is effectively suppressed, structural changes are reduced, and material stability is improved.
Through the microcage structure design, the cycling performance of the battery is significantly improved, the structural changes of the material and the attenuation of battery capacity are reduced, and the stability and conductivity of the material are enhanced.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present application relates to the field of batteries, and particularly to a ternary cathode material, a preparation method thereof, a cathode and a battery. Background Art
[0002] With the rapid development of electric vehicles and energy storage technologies, higher requirements are put forward for the energy density, cycle life and safety performance of lithium-ion batteries. Due to its relatively high specific capacity, the high-nickel ternary cathode material has become one of the key materials to improve the energy density of batteries.
[0003] When using traditional high-nickel ternary cathode materials, during the charge and discharge process, lithium ions enter and leave the high-nickel ternary cathode material, resulting in the expansion and contraction of its structure, and then causing the rupture or distortion of the crystal structure of the high-nickel ternary cathode material. Each expansion and contraction will accelerate the deterioration of the material, resulting in the attenuation of battery capacity and affecting the cycle performance of the battery.
[0004] Therefore, how to improve the structural stability of high-nickel ternary cathode materials is an urgent problem to be solved. Summary of the Invention
[0005] The present application provides a ternary cathode material, a preparation method thereof, a cathode and a battery, which are used to improve the structural expansion caused by the precipitation and dissolution of lithium ions during the charge and discharge process of high-nickel ternary materials, and improve the cycle performance of the battery.
[0006] In a first aspect, the present application provides a ternary cathode material, which includes a self-supporting micro-cage structure. The material of the micro-cage structure is a high-nickel ternary material. There is a cavity inside the micro-cage structure, and a part of the cavity inside the micro-cage structure is filled with a conductive agent.
[0007] Further, the micro-cage structure in the ternary cathode material is a single-layer structure.
[0008] Further, the micro-cage structure in the ternary cathode material is a multi-layer structure.
[0009] Further, a part of the cavity inside the micro-cage structure is filled with a conductive agent.
[0010] Further, the volume ratio of the conductive agent filled in the micro-cage structure to the volume of the micro-cage structure is less than 70%.
[0011] Further, the micro-cage structure is spherical, and the diameter of the micro-cage structure is 50-500 nm; and / or the thickness of the cage wall structure is 5-50 nm.
[0012] Further, the surface of the micro-cage structure is coated with a heterojunction thin film of a fast ion conductor.
[0013] Further, the thickness of the heterojunction film of the fast ion conductor is 5 - 15 nm.
[0014] Further, the heterojunction film of the fast ion conductor comprises Li3PO4 and LiNbO3, and the molar ratio of Li3PO4 to LiNbO3 is 1:1 - 4:1.
[0015] Further, the conductive agent is one or more of carbon nanotubes, graphene, graphite, and carbon black.
[0016] Further, the conductive agent is filled between adjacent micro - cage structures.
[0017] Further, the chemical formula of the high - nickel ternary material is LiNi x Co y Mn z O2, where 0.8 ≤ x < 1, 0 < y < 0.3, 0 < z < 0.3, and x + y + z = 1.
[0018] In a second aspect of the present application, a preparation method of a ternary cathode material is provided. The preparation method is used to prepare the ternary cathode material according to any one of the first aspect, and the preparation method includes:
[0019] Uniformly disperse polystyrene nanospheres on a substrate to form a closely - arranged polystyrene nanosphere template;
[0020] Deposit a soluble salt solution on the surface of the polystyrene nanosphere template to form a precursor coating layer. The soluble salt solution includes nickel ions, cobalt ions, and manganese ions prepared according to a preset stoichiometric ratio;
[0021] Perform a lithiation reaction on the precursor coating layer with a lithium source to convert the precursor into a high - nickel ternary material;
[0022] Remove the polystyrene nanosphere template by calcination or dissolution with an organic solvent to obtain a self - supported high - nickel ternary cathode material with a micro - cage structure;
[0023] Impregnate a dispersion of the conductive agent into the pores of the micro - cage structure of the high - nickel ternary cathode material, and form a conductive network by high - temperature carbonization.
[0024] Further, the preparation method further includes:
[0025] Coat a fast ion conductor on the surface of the micro - cage structure by a sol - gel method to form a heterojunction film.
[0026] In a third aspect of the present application, a cathode is provided. The cathode includes the ternary cathode material according to any one of the first aspect, or includes the ternary cathode material prepared by the preparation method according to any one of the second aspect.
[0027] The fourth aspect of the present application provides a battery, which includes the ternary cathode material described in any item of the first aspect, or includes the ternary cathode material prepared by the preparation method described in any item of the second aspect.
[0028] The present application provides a ternary cathode material, its preparation method, a cathode and a battery. The ternary cathode material includes a self-supporting microcage structure, the material of the microcage structure is a high-nickel ternary material, and there is a cavity inside the microcage structure. The microcage structure has an internal cavity that can accommodate the entry and exit of lithium ions. Through this structural design, the volume expansion or contraction of the high-nickel ternary material during charge and discharge can be effectively inhibited, the structural change of the material can be reduced, the stability of the high-nickel ternary material can be improved, and thus the cycle performance of the battery can be enhanced. In addition, due to the special design of the microcage structure, the direct contact area between the solid electrolyte and the high-nickel ternary material can be reduced, and the interfacial compatibility between the high-nickel ternary material and the solid electrolyte can be improved, thereby avoiding the performance degradation caused by the interfacial reaction. Detailed Embodiments
[0029] To make the objectives, technical solutions and advantages of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are some, but not all, of the embodiments of the present invention. All other embodiments obtained by those of ordinary skill in the art based on the embodiments of the present invention without creative efforts shall fall within the protection scope of the present invention.
[0030] The high-nickel ternary cathode material is a type of cathode material for lithium-ion batteries and belongs to a kind of ternary cathode material. The high-nickel ternary cathode material contains three metal elements: nickel (Ni), cobalt (Co), and manganese (Mn), and the content of nickel is relatively high, usually exceeding 60%.
[0031] The nickel element has a relatively high specific capacity and can store more lithium ions, thereby providing a higher energy density. Therefore, the high-nickel ternary material provides a higher energy density than traditional materials and is particularly suitable for applications that require long-term operation and large-capacity energy storage, such as electric vehicles and large-scale energy storage systems. However, during charge and discharge, as lithium ions precipitate and dissolve on the surface of the high-nickel ternary cathode material, it will cause the expansion and contraction of the material structure, which may further lead to the rupture or distortion of the crystal structure of the high-nickel ternary cathode material. Each expansion and contraction will accelerate the deterioration of the material, resulting in capacity decay and affecting the cycle performance of the battery.
[0032] In view of the above problems, in this application, a high-nickel ternary material is fabricated into a self-supporting microcage structure, which has an internal space to accommodate the ingress and egress of lithium ions. Through this structure, the volume expansion or contraction of the high-nickel ternary material during charge and discharge can be effectively inhibited, the structural changes of the material can be reduced, the stability of the high-nickel ternary material can be improved, and thus the cycle performance of the battery can be enhanced.
[0033] Based on this, in the first aspect of this application, a ternary cathode material is provided. This ternary cathode material includes a self-supporting microcage structure. The material of the microcage structure is a high-nickel ternary material. There is a cavity inside the microcage structure, and part of the cavity inside the microcage structure is filled with a conductive agent.
[0034] Among them, the chemical formula of the high-nickel ternary material is LiNi x Co y Mn z O2, where 0.8 ≤ x < 1, 0 < y < 0.3, 0 < z < 0.3, and x + y + z = 1.
[0035] The high-nickel ternary material in this embodiment adopts a self-supporting design of the microcage structure, and includes a cavity structure inside. The cavity structure can accommodate more lithium ions to enter and exit during charge and discharge, alleviating the volume expansion problem of the electrode material and further enhancing the stability of the material. Due to the special design of the microcage structure, the direct contact area between the solid electrolyte and the high-nickel ternary material can be reduced, improving the interfacial compatibility, thereby avoiding the performance degradation caused by interfacial reactions. Filling the conductive agent can improve the electron transport ability inside the microcage, reduce the internal resistance, and increase the charge and discharge rate of the material.
[0036] In some embodiments, the microcage structure is a circular microcage structure or an approximately circular microcage structure.
[0037] In some embodiments, the microcage structure is a rectangular microcage structure or an approximately rectangular microcage structure.
[0038] In some embodiments, the microcage structure in the ternary cathode material is a single-layer structure.
[0039] The single-layer structure means that there is only one layer of microcage structure in the ternary cathode material. Lithium ions can enter and exit the microcage structure of the high-nickel ternary material relatively freely. The lithium ion transmission path is shorter, enabling rapid response to the ingress and egress of ions during charge and discharge and optimizing the ion transmission path.
[0040] In some embodiments, the microcage structure in the ternary cathode material is a multi-layer structure.
[0041] The microcage structure is multi-layered, indicating that multiple microcage structures are stacked together. Specifically, it can be 2 layers, 3 layers, 4 layers, 5 layers, 10 layers, etc. The sizes of the microcage structures in different layers can be the same or different. For example, the ternary cathode material includes two continuously arranged microcage structures that are superimposed on each other. Another example is that the ternary cathode material includes three continuously arranged microcage structures that are superimposed on each other.
[0042] The multi-layer structure can effectively disperse the stress generated during charge and discharge, avoiding problems such as cracking or shedding caused by insufficient stress dispersion that may occur in a single-layer structure. However, its lithium-ion transport path is longer compared to the single-layer structure.
[0043] In some embodiments, the volume of the conductive agent filled in the microcage structure accounts for 0%-70% of the volume of the microcage structure.
[0044] In this embodiment, space needs to be reserved inside the microcage structure for the precipitation of lithium ions. Therefore, the filled conductive agent cannot completely fill the inside of the microcage structure. Exemplarily, the proportion of the volume of the conductive agent to the volume of the microcage structure can be 0%, 10%, 20%, 30%, 40%, 50%, 60%, 70%, or a range composed of any two of the above values.
[0045] When the proportion of the volume of the conductive agent to the volume of the microcage structure is 0%, it means that no conductive agent is filled inside the microcage structure. The microcage structure itself has sufficient conductivity, and it is necessary to maximize the space for lithium ions to ensure efficient lithium-ion migration.
[0046] The proportion of the filled conductive agent should be adjusted according to actual application requirements. A lower proportion (such as 0%-30%) is suitable for use when a higher lithium-ion migration space is required, while a higher proportion (such as 40%-70%) is suitable for applications with higher requirements for conductivity. However, it should be noted that the effective space for lithium-ion precipitation in the microcage cannot be affected. The volume of lithium-ion precipitation can be calculated based on the battery's capacitance to estimate the amount of lithium ions involved and then estimate the volume of lithium-ion precipitation. Ensure that the reserved space inside the microcage structure is larger than the volume of lithium-ion precipitation.
[0047] In some embodiments, the microcage structure is spherical, and the inner diameter of this microcage structure is 50-500 nm. Exemplarily, the inner diameters of the microcage structures are 50 nm, 100 nm, 150 nm, 200 nm, 250 nm, 300 nm, 350 nm, 400 nm, 450 nm, 500 nm, or a range composed of any two of the above values.
[0048] In some embodiments, the thickness of the cage wall structure is 5 - 50 nm. Exemplarily, the thickness of the micro-cage structure is 5 nm, 10 nm, 15 nm, 20 nm, 25 nm, 30 nm, 35 nm, 40 nm, 50 nm, or a range composed of any two of the above values.
[0049] In some embodiments, the surface of the micro-cage structure is coated with a heterojunction thin film of a fast ion conductor.
[0050] The heterojunction thin film refers to a thin film structure composed of two or more different fast ion conductor materials. The heterojunction thin film of the fast ion conductor can reduce the interfacial impedance between the ternary material and the electrolyte, improve the interfacial compatibility, and improve the charge and discharge efficiency of the battery by providing a more uniform and efficient conductive interface. Coating a layer of the heterojunction thin film of the fast ion conductor on the surface of the micro-cage structure can effectively prevent the direct contact between the high-nickel ternary material and the solid electrolyte, thereby avoiding the incompatibility or reaction between the electrolyte and the cathode material. In addition, the coating of the heterojunction thin film of the fast ion conductor can further optimize the ionic conductivity, ensure that lithium ions can move efficiently and stably in the cathode material, and improve the safety of the battery.
[0051] The fast ion conductor can be selected from the following material combinations: Li3PO4 / LiNbO3, Li3BO4 / Li3PO4, Li2B4O7 / Li3PO4, Li3BO3 / LiNbO3, Li2B4O7 / LiNbO3, Li4Ti5O 12 / LiNbO3, Li 1.5 Al 0.5 Ti 1.5 (PO4)3 / Li3PO4, LiLaTiO3 / Li3PO4, Li7La3Zr2O 12 / LiNbO3, Li2O / TiO2, Li2S / P2S5, or a combination of multiple of the above materials.
[0052] In a specific implementation, the heterojunction thin film of the fast ion conductor includes Li3PO4 and LiNbO3, and the molar ratio of Li3PO4 to LiNbO3 is 1:1 - 4:1.
[0053] Lithium phosphate Li3PO4 is a commonly used lithium ion conductor with high chemical stability and low ionic migration energy barrier, and can be used as an electrolyte material; the main advantage of LiNbO3 is that it can form a relatively stable charge transport path. The heterojunction thin film of Li3PO4 and LiNbO3 combines the advantages of both and can provide a more efficient ionic conduction path between the micro-cage structure and the electrolyte.
[0054] The interfacial structure formed by Li3PO4 and LiNbO3 materials can reduce the interfacial impedance and decrease the electrochemical reaction loss between the electrolyte and the electrode material. The combination of Li3PO4 and LiNbO3 can help improve the migration rate of lithium ions in the battery by forming an excellent conductive network, enabling more efficient ion transport during the charge and discharge processes of the battery.
[0055] Exemplarily, the molar ratio of Li3PO4 to LiNbO3 can be 1:1, 2:1, 3:1, 4:1, or a range composed of any two of the above ratios.
[0056] In some embodiments, the thickness of the heterojunction thin film of the fast ion conductor is 5 - 15 nm. Exemplarily, the thickness can be 5 nm, 7 nm, 9 nm, 10 nm, 11 nm, 13 nm, 14 nm, 15 nm, or a range composed of any two of the above values.
[0057] In some embodiments, the conductive agent filled in the microcage structure is one or more of carbon nanotubes, graphene, graphite, carbon black, carbon fiber, conductive polymers (polyaniline, polypyrrole, polythiophene), and metal nanomaterials.
[0058] In some embodiments, the space between adjacent microcage structures is also filled with a conductive agent.
[0059] The conductive agent between the microcage structures can improve the interfacial connectivity between the microcage structures and reduce the interfacial impedance. The conductive agent is filled between the microcages to optimize the current conduction between adjacent microcages and improve the overall battery or capacitor performance. Especially during the charge and discharge processes, it can transfer charges more efficiently. The conductive agent filled between the microcage structures can also help enhance the physical contact and stability between the microcage structures. Especially during multiple cycles of charge and discharge, it can prevent the separation or damage of the microcage structures due to expansion and contraction or thermal stress, thereby improving the mechanical stability of the material.
[0060] In addition, the filling of the conductive agent helps reduce the internal resistance of the material. Especially when a conductive network is formed between adjacent microcages, it can significantly reduce the internal resistance of the battery.
[0061] The second aspect of this application provides a preparation method for a ternary cathode material. This preparation method is used to prepare the ternary cathode material as described in any one of the above, and this preparation method includes:
[0062] Step 1: Uniformly disperse polystyrene nanospheres on a substrate to form a closely arranged polystyrene nanosphere template.
[0063] The polystyrene (PS) nanosphere template is to disperse PS nanospheres on a substrate to construct a template with a regularly arranged nanostructure. The PS nanospheres can be uniformly dispersed on the substrate by self-assembly or spin coating, and a monolayer or multilayer arrangement of PS nanosphere structures can be formed by photolithography or other microfabrication methods.
[0064] In one implementation, the PS nanosphere template is prepared by spin coating, and the PS nanospheres are uniformly distributed on the substrate surface. Specifically, PS nanospheres of appropriate size can be selected, which can be purchased on the market or synthesized by polymerization. Then, surface treatment is carried out on the substrate. For example, plasma treatment (such as oxygen plasma) is used to clean the substrate and enhance its surface hydrophilicity. The PS nanospheres are dissolved in a suitable solvent (such as water or an organic solvent), and then this solution is uniformly coated on the substrate surface. A certain amount of PS nanosphere solution is dropped onto the substrate, and then the substrate is rotated at high speed. During the spin coating process, due to the action of centrifugal force, the PS nanospheres will be uniformly dispersed on the substrate surface, and finally a monolayer or multilayer nanosphere array is formed. Multiple layers of PS spheres can be stacked by repeating spin coating or the alternate dipping method. To improve the stability of the PS nanosphere template, the substrate can be slightly heat-treated to help the PS nanospheres better adhere to the substrate surface.
[0065] In one implementation, the dispersion and arrangement of PS nanospheres on the substrate surface can be controlled by the self-assembly method. Specifically, the PS nanospheres are dispersed in a suitable solvent, and the substrate is surface-modified, such as by oxygen plasma treatment or silanization treatment, to enhance its hydrophilicity or selectivity so that the nanospheres can adhere uniformly. The PS nanosphere solution is dropped onto the substrate. Through the evaporation or diffusion effect of the solvent, the PS nanospheres will naturally self-assemble into an ordered structure on the substrate surface. By adjusting parameters such as the solution concentration and evaporation rate, a more compact and ordered nanosphere array can be obtained.
[0066] In one implementation, polystyrene (PS) nanospheres are dispersed in water. A surfactant is added to the water, which can help the PS nanospheres disperse on the water surface and avoid aggregating with each other. Surfactant molecules usually attach to the surface of the nanospheres, enabling the nanospheres to stably exist on the water surface. The solution containing the PS nanospheres is dropped onto the water surface. On the water surface, with the help of the surfactant, the PS nanospheres will naturally arrange into an ordered monolayer or multilayer structure through the self-assembly phenomenon. Due to the interaction between the nanospheres, they will spontaneously organize into a closely packed array. After the PS nanospheres self-assemble into an ordered array on the water surface, a substrate (such as a silicon wafer or glass) is immersed in the water, and the nanosphere array will adhere to the surface of the substrate. By slowly lifting the substrate, the PS nanosphere array will be transferred from the water surface to the substrate surface. After the transfer, the water is removed by drying, and the nanosphere array will be firmly fixed on the substrate, forming a stable polystyrene template.
[0067] Step 2: Deposit a soluble salt solution onto the surface of the polystyrene nanosphere template to form a precursor coating layer. The soluble salt solution includes nickel ions, cobalt ions, and manganese ions prepared according to a preset stoichiometric ratio.
[0068] In this step, soluble salts of metals such as nickel, cobalt, and manganese (such as nitrates, chlorides, etc.) are formulated into a mixed solution according to the stoichiometric ratio. The solution contains the metal components required in the ternary material. Chemical bath deposition or atomic layer deposition can be used to uniformly deposit the metal precursor on the surface of the PS nanospheres.
[0069] In one implementation, metal ions are deposited by chemical bath deposition. Specifically, the prepared precursor solution is immersed or sprayed onto the surface of the PS nanospheres, and the chemical reaction in the solution is used to deposit the metal precursor on the template surface, forming a uniform metal coating layer.
[0070] In one implementation, metal ions are deposited by atomic layer deposition. Specifically, by precisely controlling the gas reaction, a thin and uniform metal film is deposited by the precursor on the template surface.
[0071] Step 3: Perform a lithiation reaction on the precursor coating layer with a lithium source to convert the precursor into a high-nickel ternary material. Among them, the chemical formula of the high-nickel ternary material is LiNi x Co y Mn z O2, 0.8 ≤ x < 1, 0 < y < 0.3, 0 < z < 0.3, and x + y + z = 1.
[0072] The PS template deposited with the metal precursor is mixed with a lithium source (such as lithium carbonate, lithium hydroxide, etc.). The lithium source reacts with the precursor at high temperature to form lithium nickel cobalt manganese oxide (LiNi xCo y Mn z (O2), that is, high-nickel ternary material.
[0073] The lithium source and the precursor undergo a thermal reaction at a temperature above 800 °C to complete the transformation of the precursor into the high-nickel ternary material.
[0074] Step 4: Remove the polystyrene nanosphere template by calcination or dissolution in an organic solvent to obtain a high-nickel ternary cathode material with a self-supporting microcage structure.
[0075] In one implementation, the polystyrene nanosphere template is heated to a relatively high temperature (the temperature is between 500 °C and 700 °C), and the PS nanospheres burn off at high temperature, leaving an oxide with a microcage structure.
[0076] In one implementation, a solvent (such as dichloromethane, etc.) is used to dissolve the PS nanospheres, leaving a microcage structure of nickel cobalt manganese oxide.
[0077] By removing the PS template, a self-supporting microcage structure is obtained, which is hollow inside. This structure provides a high specific surface area and good porosity.
[0078] Through the above steps, a high-nickel ternary all-solid-state cathode material with a self-supporting microcage structure can be prepared. There is a hollow space inside the microcage structure. During charging, lithium ions can precipitate inside the microcage structure, avoiding damage caused by structural expansion. The inside of the microcage structure can be filled with a conductive agent, and the space between the microcage structures can be filled with a conductive agent.
[0079] After the above step 4, in some embodiments, to improve the conductivity and stability of the ternary cathode material, the following step 5 is also required.
[0080] Step 5: Impregnate the dispersion of the conductive agent into the pores of the microcage structure of the high-nickel ternary cathode material and form a conductive network through high-temperature carbonization.
[0081] Under an inert atmosphere (such as nitrogen or argon), the dispersion of the conductive agent is impregnated into the microcage structure. The conductive agent will disperse between the microcage structures and into the internal space of the microcage structure. The microcage structure impregnated with the conductive agent is heated to a relatively high temperature (the temperature range is between 800 °C and 1000 °C) to carbonize the conductive agent in the microcage pores, forming a stable conductive network. An efficient conductive network is formed to enhance the conductivity of the microcage structure and improve the overall performance of the battery or capacitor.
[0082] Among them, the conductive agent can be selected from one or more of carbon nanotubes, graphene, graphite, and carbon black.
[0083] To regulate the volume of the conductive agent in the microcage structure, the total amount of the dispersant can be controlled. The amount of the dispersant directly determines the filling amount of the conductive agent inside the microcage structure. By controlling the total amount of the dispersant, the filling rate of the conductive agent in the microcage structure can be precisely controlled.
[0084] The total amount of the dispersant for controlling the filling can be achieved by any of the following methods:
[0085] 1. Concentration control of the dispersant: The dispersant is the dissolution medium of the conductive agent, and usually a liquid (such as water, alcohols or other solvents) is used as the dispersant. During impregnation, the concentration of the conductive agent in the solution can be adjusted. A low-concentration dispersion liquid will result in less conductive agent being impregnated into the microcage structure, while a high-concentration dispersion liquid may cause overfilling of the conductive agent.
[0086] 2. Impregnation time control: In addition to the control of the amount of the dispersant, the impregnation time also affects the adsorption amount of the conductive agent. A shorter impregnation time may result in the conductive agent not fully filling the pores of the microcage, while an overly long impregnation time may cause an excessive amount of the conductive agent.
[0087] 3. Solution amount control: During the impregnation process of the dispersion liquid, if too much solution is used, the conductive agent may penetrate outside the microcage or even overflow, affecting its volume ratio. By controlling the volume of the dispersion liquid, the filling amount of the conductive agent inside the microcage can be restricted.
[0088] In addition to the method of regulating the total amount of the dispersant, the proportion of the conductive agent filled inside the microcage structure can also be controlled by adjusting the particle size of the conductive agent. The pores on the wall of the microcage structure have a certain size, and the conductive agent with a smaller particle size can better penetrate into the pores of the microcage, thereby filling the microcage structure. While a larger particle size may not be effectively filled due to pore limitations. Therefore, a variety of conductive materials are mixed in the filled conductive agent, and the particle sizes of the various conductive materials are different. The conductive agent with a smaller particle size is used to fill into the microcage structure, and the conductive agent with a larger particle size can only be filled between two microcage structures or cannot be filled. In this way, by controlling the number of the filled conductive agent with a smaller particle size, the volume of the conductive agent inside the microcage structure is controlled.
[0089] In some embodiments, the volume of the conductive agent filled in the microcage structure accounts for 0%-60% of the volume of the microcage structure
[0090] Optionally, to further improve the interfacial compatibility between the solid electrolyte and the high-nickel ternary material and reduce the interfacial resistance, after the above step 4 or step 5, step 6 is further included.
[0091] Step 6: Coating a fast ion conductor on the surface of the microcage structure by the sol-gel method to form a heterojunction thin film.
[0092] According to the fast ion conductor to be used (such as Li3PO4 / LiNbO3), the corresponding metal salt or metal organic compound is selected as the precursor. For example, the precursors of Li3PO4 can be lithium dihydrogen phosphate (LiH2PO4) and lithium chloride (LiCl); the precursors of LiNbO3 can be lithium chloride (LiCl) and niobium chloride (NbCl5). The selected precursors are dissolved in a solvent (usually an alcohol solvent such as isopropyl alcohol or ethanol) or water to prepare a sol. An appropriate amount of stabilizer (such as an alcohol surfactant, an acidic solution, etc.) is added to maintain the stability of the sol and prevent the precursors from aggregating or precipitating. According to the thickness of the final film and the required conductive performance, the concentration of the sol is adjusted. If the sol concentration is too low, the film may be too thin; if the concentration is too high, precipitation may occur. The sol is uniformly coated on the surface of the microcage. Common coating methods include dip coating, spin coating, and drop coating. The coated microcage is placed at a temperature of 50 - 100 °C for drying to remove the solvent and transform the sol from a liquid state into a solid gel. During the drying process, the sol gradually transforms into a gel, forming a film. To make the film more stable and improve the conductivity of the film, the dried gel is heat-treated (sintered), which helps to form a crystalline structure and remove organic residues. During the sintering process, the film will be further densified, and a heterojunction film with higher conductivity will be formed. The sintering temperature varies depending on the different fast ion conductor materials selected. Exemplarily, the sintering temperature of Li3PO3 / LiNbO3 can be selected between 700 - 1000 °C.
[0093] Through the above step 6, a uniform heterojunction film can be effectively formed on the surface of the microcage structure, providing good conductive performance and stability, and effectively isolating the high-nickel ternary material and the solid electrolyte.
[0094] The third aspect of the present application provides a positive electrode, which includes any one of the ternary positive electrode materials in the first aspect above, or includes the ternary positive electrode materials prepared by any one of the preparation methods in the second aspect. For the preparation method of the positive electrode sheet, the above ternary positive electrode material can be prepared on the surface of the aluminum foil current collector to obtain the positive electrode sheet. Or the above-prepared ternary positive electrode material can be transferred onto the aluminum foil current collector to form the positive electrode sheet.
[0095] The fourth aspect of the present application provides a battery, which includes any one of the ternary positive electrode materials in the first aspect above, or includes the ternary positive electrode materials prepared by any one of the preparation methods in the second aspect. For the preparation method of the positive electrode sheet, the positive electrode sheet containing the positive electrode material, the solid electrolyte, and the negative electrode sheet containing the negative electrode material are assembled into an all-solid-state lithium-ion battery.
[0096] Hereinafter, the present invention will be further introduced through specific examples.
[0097] Example 1
[0098] 1. Template Preparation: A PS nanosphere template with a diameter of 300 nm was prepared by the sol - gel method. The PS nanospheres were dispersed on a glass substrate, and a uniform multi - layer PS nanosphere template was formed by spin - coating.
[0099] 2. Precursor Deposition: A mixed solution was prepared by mixing nickel sulfate, cobalt sulfate, and manganese sulfate according to the stoichiometric ratio of LiNi 0.85 Co 0.1 Mn 0.05 O₂. Using atomic layer deposition, the mixed solution was deposited on the surface of the PS nanosphere template at 80 °C for 50 cycles, forming a precursor coating layer with a thickness of about 40 nm.
[0100] 3. Lithiation Treatment: The template deposited with the precursor was mixed with lithium hydroxide in a molar ratio of 1:1.3 and calcined at 850 °C for 8 hours in an oxygen atmosphere to convert the precursor into the high - nickel ternary material LiNi 0.85 Co 0.1 Mn 0.05 O₂.
[0101] 4. Template Removal: The lithiated sample was immersed in toluene solution for 24 hours to remove the PS nanosphere template, obtaining a self - supported micro - cage - structured high - nickel ternary all - solid - state cathode material.
[0102] Example 2
[0103] The difference from Example 1 is that a single - layer PS nanosphere template was prepared by spin - coating.
[0104] Example 3
[0105] 1. Template Preparation: PS nanospheres with a diameter of 200 nm were dispersed on a silicon wafer substrate, and a closely packed single - layer PS nanosphere template was formed by centrifugation and self - assembly.
[0106] 2. Precursor Deposition: A mixed solution was prepared by mixing nickel nitrate, cobalt nitrate, and manganese nitrate according to the stoichiometric ratio of LiNi 0.85 Co 0.1 Mn 0.05 O₂. Using chemical bath deposition, the mixed solution was deposited on the surface of the PS nanosphere template at 50 °C for 2 hours, forming a precursor coating layer with a thickness of about 30 nm.
[0107] 3. Lithiation Treatment: The template deposited with the precursor was mixed with lithium carbonate in a molar ratio of 1:1.2 and calcined at 800 °C for 10 hours in an oxygen atmosphere to convert the precursor into the high - nickel ternary material LiNi 0.85 Co 0.1 Mn 0.05O2.
[0108] 4. Template removal: The lithiated sample was calcined at 500 °C for 2 hours to remove the PS nanosphere template, obtaining a self-supporting microcage-structured high-nickel ternary all-solid-state cathode material.
[0109] 5. Composite conductive network: In an inert atmosphere, the carbon nanotube / graphene dispersion was impregnated into the microcage pores, with the impregnation amount of the conductive agent being 2 wt%, the carbonization temperature being 800 °C, and calcined for 2 hours.
[0110] The self-supporting microcage-structured high-nickel ternary all-solid-state cathode material obtained above was impregnated, and the volume ratio of the conductive agent impregnated into the microcage structure to the volume of the microcage structure was 30%.
[0111] Example 4
[0112] The difference from Example 3 is that the volume ratio of the conductive agent impregnated into the microcage structure to the volume of the microcage structure is 10%.
[0113] Example 5
[0114] The difference from Example 3 is that the volume ratio of the conductive agent impregnated into the microcage structure to the volume of the microcage structure is 50%.
[0115] Example 6
[0116] The difference from Example 3 is that the volume ratio of the conductive agent impregnated into the microcage structure to the volume of the microcage structure is 70%.
[0117] Example 7
[0118] The difference from Example 3 is that after forming the composite conductive network, a heterojunction thin film of Li3PO4 / LiNbO3 fast ion conductor was coated on the microcage surface by the sol-gel method, with the coated Li3PO4 / LiNbO3 (molar ratio 3:1) and a thickness of 10 nm.
[0119] Comparative Example 1
[0120] The high-nickel ternary cathode material LiNi 0.85 Co 0.1 Mn 0.05O2 does not have a self-supporting micro-cage structure. Nickel chloride, cobalt chloride, and manganese chloride are dissolved in deionized water in a certain molar ratio (Ni:Co:Mn = 0.85:0.1:0.05) and stirred until completely dissolved to form a metal salt solution. In another container, lithium hydroxide (LiOH) is dissolved in deionized water to form a lithium hydroxide solution. The metal salt solution and the lithium hydroxide solution are mixed and continuously stirred. Ammonia water is slowly added dropwise to the mixed solution, and the pH value is controlled between 8 and 11. Metal hydroxide precursors (Ni(OH)2, Co(OH)2, Mn(OH)2) are formed. The precipitate is filtered through filter paper to remove impurities in the solution, and then the precipitate is repeatedly washed with deionized water to remove ions dissolved in the precipitate, such as chloride ions, ammonium ions, etc., until the pH value of the washing solution is close to neutral. The dried precursor is calcined at high temperature in a tubular furnace. It is calcined in an oxygen atmosphere at a calcination temperature of 700 °C to form an oxide structure (LiNi 0.85 Co 0.1 Mn 0.05 O2). The cooled product is taken out and crushed to the required particle size using a grinder or a ball mill.
[0121] Comparative Example 2
[0122] The difference from Example 3 is that the volume ratio of the conductive agent impregnated into the micro-cage structure to the volume of the micro-cage structure is 85%.
[0123] Comparative Example 3
[0124] The difference from Example 3 is that the volume ratio of the conductive agent impregnated into the micro-cage structure to the volume of the micro-cage structure is 99%.
[0125] Test Example
[0126] Charge and Discharge Test
[0127] The above-prepared cathode material is assembled with a sulfide solid electrolyte and a silicon-based anode material into a all-solid-state lithium-ion battery, and charge and discharge tests are carried out at room temperature. A battery tester is used to set appropriate charge and discharge currents and charging voltage ranges. Usually, the upper charging limit of the battery is 4.2 V, and the lower discharge limit is 2.5 V. It is charged at a certain current (such as 0.1 C) until the battery voltage reaches the upper limit of 4.2 V. After being fully charged, a discharge test is carried out until the battery voltage drops to the lower limit of 2.5 V. During discharge, the tester records the discharge curve and current of the battery. According to the discharge current and discharge time of the battery, the total capacity during the discharge process is calculated, and the specific capacity (mAh / g) between the discharge capacity and the mass of the cathode material is calculated.
[0128] Perform multiple charge-discharge cycles. The conditions (current, time, upper and lower voltage limits) for each charge-discharge cycle should be the same. After each charge-discharge cycle, record the discharge capacity and calculate the capacity retention rate.
[0129] Porosity test
[0130] First, prepare the electrode material sample to be tested. Use a densitometer or gas adsorption method (such as the BET method) to measure the total volume of the sample. Determine the porosity of the sample through techniques such as gas adsorption / desorption or mercury intrusion method.
[0131] The initial discharge specific capacity and capacity retention rate data of the above examples and comparative examples are shown in Table 1.
[0132] Table 1 Charge-discharge test data
[0133]
[0134] From the above data, the initial discharge specific capacity of Example 1 reached 190 mAh / g, and after 100 cycles, the capacity retention rate was 82%. For the traditional high-nickel ternary material in Comparative Example 1, the initial discharge specific capacity was 180 mAh / g, and after 100 cycles, the capacity retention rate was 70%. Compared with the traditional high-nickel ternary material, the initial discharge specific capacity of Example 1 increased, and the capacity cycle retention rate increased by 12%. Through the above comparison, it is proved indirectly that through the design of the microcage structure, the volume expansion or contraction of the high-nickel ternary material during the charge-discharge process can be effectively inhibited, the structural change of the material can be reduced, the stability of the high-nickel ternary material can be improved, and thus the cycle performance of the battery can be improved.
[0135] By comparing Example 1 and Example 2, it is proved by data that the design of the single-layer microcage structure can improve the discharge specific capacity and capacity retention rate compared with the multi-layer structure.
[0136] By comparing Example 3 and Example 7, it is proved by data that adding a heterojunction thin film of fast ion conductor can increase the stability of the high-nickel ternary material, and thus improve the cycle performance of the battery.
[0137] From the data of Example 2 - Example 6, and Comparative Example 2 and Comparative Example 3, it is proved by data that after the proportion of the conductive agent inside the microcage structure exceeds 70%, the improvement effect decreases because the insufficient internal space will cause lithium ions to precipitate outside, resulting in volume change and instability of the structure of the high-nickel ternary material, and the capacity cycle retention rate decreases.
[0138] In addition, the battery interface resistance of Example 7 is < 30 Ω·cm², no binder is used, the electrode porosity > 40%, the lithium ion transmission rate is increased by 50% compared with Example 2, at a rate of 0.1C, the initial discharge specific capacity is as high as 230 mAh / g, and after 200 cycles, the capacity retention rate is 96%.
[0139] Finally, it should be noted that: those skilled in the art will readily conceive of other embodiments of the present invention after considering the specification and practicing the invention disclosed herein. The present invention is intended to cover any variations, uses, or adaptations of the present invention, which follow the general principles of the present invention and include the common general knowledge or conventional technical means in the technical field not disclosed in the present invention, and various modifications and changes can be made without departing from its scope. The scope of the present invention is only limited by the appended claims.
Claims
1. A ternary cathode material, characterized in that, The ternary cathode material includes a self-supporting microcage structure, the material of the microcage structure is a high-nickel ternary material, there is a cavity inside the microcage structure, and a part of the cavity inside the microcage structure is filled with a conductive agent.
2. The ternary cathode material according to claim 1, characterized in that, The microcage structure in the ternary cathode material is a monolayer structure.
3. The ternary cathode material according to claim 1, characterized in that, The microcage structure in the ternary cathode material is a multilayer structure.
4. The ternary cathode material according to claim 1, characterized in that, The volume ratio of the conductive agent filled in the microcage structure to the volume of the microcage structure is less than 70%.
5. The ternary cathode material according to any one of claims 1 to 4, characterized in that, The microcage structure is spherical; the diameter of the microcage structure is 50 - 500 nm, and / or the wall thickness of the microcage structure is 5 - 50 nm.
6. The ternary cathode material according to any one of claims 1 to 4, characterized in that, The surface of the microcage structure is coated with a heterojunction film of a fast ion conductor.
7. The ternary cathode material according to claim 6, characterized in that, The thickness of the heterojunction film of the fast ion conductor is 5 - 15 nm.
8. The ternary cathode material according to claim 7, characterized in that, The heterojunction film of the fast ion conductor includes Li3PO4 and LiNbO3, and the molar ratio of Li3PO4 to LiNbO3 is 1:1 - 4:
1.
9. The ternary cathode material according to any one of claims 1 to 4, characterized in that, The conductive agent is one or more of carbon nanotubes, graphene, graphite, and carbon black.
10. The ternary cathode material according to any one of claims 1 to 4, characterized in that, The conductive agent is filled between adjacent microcage structures.
11. The ternary cathode material according to any one of claims 1 to 4, characterized in that, The chemical formula of the high-nickel ternary material is LiNi x Co y Mn z O2, where 0.8 ≤ x < 1, 0 < y < 0.3, 0 < z < 0.3, and x + y + z = 1.
12. A method for preparing a ternary cathode material, characterized in that, The preparation method is used to prepare the ternary cathode material according to any one of claims 1 - 11, and the preparation method includes: Uniformly disperse polystyrene nanospheres on a substrate to form a closely arranged polystyrene nanosphere template; Deposit a soluble salt solution on the surface of the polystyrene nanosphere template to form a precursor coating layer, and the soluble salt solution includes nickel ions, cobalt ions, and manganese ions prepared according to a preset stoichiometric ratio; Perform a lithiation reaction on the precursor coating layer and a lithium source to convert the precursor into a high-nickel ternary material; Remove the polystyrene nanosphere template by calcination or dissolution with an organic solvent to obtain a high-nickel ternary cathode material with a self-supporting microcage structure; Impregnate the dispersion of the conductive agent into the pores of the microcage structure of the high-nickel ternary cathode material, and form a conductive network by high-temperature carbonization.
13. The preparation method according to claim 12, characterized in that, The preparation method further includes: Coat a fast ion conductor on the surface of the microcage structure by a sol-gel method to form a heterojunction film.
14. A cathode, characterized in that, The cathode includes the ternary cathode material according to any one of claims 1 - 11, or includes the ternary cathode material prepared by the preparation method according to claim 12 or 13.
15. A battery, characterized in that, Includes the ternary cathode material according to any one of claims 1 - 11, or includes the ternary cathode material prepared by the preparation method according to claim 12 or 13.
Citation Information
Patent Citations
Method for preparing positive material of high-power lithium ion battery
CN102938459A
Lithium nickel cobalt manganate hollow sphere as well as preparation method and application thereof
CN104241630A
Preparation method of high-rate lithium ion ternary cathode material
CN109346720A
High-nickel ternary positive electrode material coated with fast ion conductor, preparation method thereof, and lithium ion battery prepared from material
CN109879331A
Ternary positive electrode material doped, coated and modified by fast ion conductor and preparation method of material
CN112599756A
Cited By
Ternary high-nickel positive electrode material with hollow structure, preparation method of ternary high-nickel positive electrode material and lithium ion battery
CN121405151A
Positive electrode material and preparation method thereof, positive plate and lithium ion battery
CN121726402A
A positive electrode material, a preparation method thereof, a positive electrode sheet, and a lithium ion battery
CN121726402B