Diaphragm, preparation method thereof and battery
By using a functional coating of carbon material with through-holes and ceramic particles on the lithium battery separator, the problem of insufficient pore size and porosity of the existing lithium battery separator is solved, and the performance improvement of the battery in long cycles and fast charging is achieved.
Patent Information
- Application Number
- CN202510161998.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-02-13
- Publication Date
- 2025-06-20
AI Technical Summary
The pore size and porosity of the existing lithium battery separators are limited, which is difficult to meet the demand for fast charging of batteries, and the capacity retention rate is poor under long cycles.
A functional coating composed of carbon material with through-holes and ceramic particles is adopted to absorb and store the electrolyte more effectively through the through-pore capillary action of the carbon material, thereby improving the capacity retention rate of the battery under long cycles.
It effectively improves the life problem of the battery during long-cycle cycling, improves the safety and cycle life of the battery, and improves the fast charging performance of the battery.
Smart Images

Figure CN120184514A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the technical field of batteries, and particularly to diaphragms, their preparation methods, and batteries. Background Art
[0002] Lithium batteries mainly consist of a positive electrode, a negative electrode, a diaphragm, and an electrolyte. In the current situation where the performance requirements for the actual use of lithium batteries are getting higher and higher, the demand for diaphragms is no longer just to block the direct contact between the positive and negative electrodes. Various functional diaphragms have emerged, providing more choices for lithium-ion batteries. In addition to higher safety requirements, better electrolyte wettability and ion permeability have also become a development direction for functional diaphragms.
[0003] Existing lithium-ion battery diaphragms are generally made of polyolefin materials. Limited by the structure of the material itself, their pore size and porosity are limited. And in order to improve the high-temperature resistance of the base material, a ceramic layer is usually coated on the surface of the base material, further blocking the ion transport channels. At present, with the increasing requirements for fast charging of batteries, it can no longer meet the needs.
[0004] CN106299222A discloses a method of using carbon materials as ceramic coating additives. By using carbon materials, the electronic conductivity of the diaphragm can be improved, and the electrolyte absorption capacity of the coating film can be further improved, enhancing the performance of the battery core. However, the capacity retention rate under long cycles of this solution is poor. Summary of the Invention
[0005] In view of this, the present invention provides a diaphragm, its preparation method, and a battery. The functional coating of the diaphragm includes carbon materials with through holes and ceramic particles. While ensuring its original heat resistance performance, more pores are added on the surface of the functional coating. Through the capillary action of the through holes in the carbon materials, the electrolyte can be more effectively absorbed and retained, which can improve the capacity retention rate of the battery under long cycles, effectively improve the life problem in the long-cycle rate cycling process, and enhance the safety and cycle life of the battery.
[0006] To achieve the above-mentioned invention purposes, the present invention provides the following technical solutions:
[0007] In a first aspect, the present invention provides a diaphragm, which includes a base material and a functional coating provided on at least one surface of the base material;
[0008] The functional coating includes carbon materials and ceramic particles. The carbon materials have a spherical structure, and the spherical structure is provided with through holes penetrating the spherical structure.
[0009] Preferably, the average particle diameter D of the carbon materials 50 is 1.5 - 6 μm.
[0010] Preferably, the diameter of the through holes is 0.2 - 2 μm.
[0011] Preferably, the mass ratio of the carbon material to the ceramic particles is (4.7 to 28):(66 to 90).
[0012] Preferably, the single-sided thickness of the functional coating is 2 to 10 μm.
[0013] In the embodiment of the present invention, the functional coating further includes a binder.
[0014] Preferably, the mass ratio of the carbon material, the ceramic particles, and the binder is (4.7 to 28):(66 to 90):(1 to 8).
[0015] In a second aspect, the present invention provides a method for preparing the above diaphragm, including the following steps:
[0016] S1. Provide a carbon material, the carbon material has a spherical structure, and the spherical structure is provided with through holes penetrating the spherical structure;
[0017] S2. Mix the carbon material, the ceramic particles, the binder, the dispersant, the thickener, the wetting agent, and water evenly to obtain a functional coating slurry;
[0018] S3. Coat the functional coating slurry on at least one surface of the substrate, and obtain a diaphragm after drying treatment.
[0019] In the embodiment of the present invention, the preparation method of the carbon material includes the following steps:
[0020] S11. Dissolve the first polymer in the first solvent to obtain an inner layer solution;
[0021] Dissolve the second polymer in the second solvent to obtain an outer layer solution;
[0022] S12. Make the inner layer solution and the outer layer solution into fiber filaments with a core-shell structure by coaxial electrospinning;
[0023] S13. Add the fiber filaments to the third solvent for dissolution treatment, filter and dry to obtain a carbon sphere precursor with a hollow structure;
[0024] S14. Perform pre-sintering treatment on the carbon sphere precursor in an air atmosphere, and then perform carbonization treatment in an inert gas atmosphere to obtain a carbon material.
[0025] In step S11 of the present invention:
[0026] In the embodiment of the present invention, the first polymer includes at least one of polymethyl methacrylate, polyethylene, polystyrene, and polyvinyl acetate.
[0027] In an embodiment of the present invention, the second polymer includes at least one of polyamide, polyacrylonitrile, polyvinyl alcohol, and polyvinyl chloride.
[0028] In an embodiment of the present invention, the first solvent and the second solvent independently include at least one of N,N-dimethylformamide, dimethylfuran, dimethyl sulfoxide, and N-methylpyrrolidone.
[0029] Preferably, the concentration of the inner layer solution is 7 wt% to 20 wt%.
[0030] Preferably, the concentration of the outer layer solution is 7 wt% to 30 wt%.
[0031] In step S12 of the present invention:
[0032] Preferably, the voltage of the coaxial electrospinning is 10 to 30 kV, the advancing rate of the inner layer solution is 20 to 500 mL / min, the advancing rate of the outer layer solution is 25 to 250 mL / min, the ratio of the advancing rate of the inner layer solution to the advancing rate of the outer layer solution is 0.2 to 2.0, and the electrode distance is 15 to 30 cm.
[0033] In step S13 of the present invention:
[0034] In an embodiment of the present invention, the third solvent includes at least one of toluene, tetrahydrofuran, xylene, and amyl acetate.
[0035] In step S14 of the present invention:
[0036] Preferably, the temperature of the pre-sintering treatment is 200 to 400 °C, and the heat preservation time of the pre-sintering treatment is 1 to 5 h.
[0037] Preferably, the temperature of the carbonization treatment is 1200 to 1500 °C, and the heat preservation time of the carbonization treatment is 1 to 6 h.
[0038] In a third aspect, the present invention provides a battery, which includes the above-mentioned separator, and / or a separator prepared by the above-mentioned preparation method.
[0039] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0040] 1. The functional coating of the separator of the present invention includes a carbon material (porous carbon spheres) with through holes and ceramic particles. While ensuring its original heat resistance performance, more pores are added on the surface of the functional coating. Through the capillary action of the through holes of the porous carbon spheres, the electrolyte can be more effectively absorbed and stored, thereby improving the capacity retention rate of the battery under long cycles, effectively improving the life problem in the long-cycle rate cycling process, and enhancing the safety and cycle life of the battery.
[0041] 2. The separator of the present invention can construct more lithium-ion channels on the surface layer of the separator, improve the penetration ability of lithium ions between the separators, improve the lithium plating situation caused by the aggregation of lithium ions on the surface layer, shorten the lithium-ion transmission distance, and improve the fast charging performance of the battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] Figure 1 It is a schematic structural diagram of the carbon material (porous carbon sphere) of the present invention from the first perspective.
[0043] Figure 2 It is a schematic structural diagram of the carbon material (porous carbon sphere) of the present invention from the second perspective. DETAILED DESCRIPTION OF THE INVENTION
[0044] The present invention discloses a separator, a preparation method thereof and a battery. Those skilled in the art can draw on the content of this article and appropriately improve the process parameters to achieve it. It should be particularly noted that all similar substitutions and modifications are obvious to those skilled in the art, and they are all regarded as included in the present invention. The method and application of the present invention have been described through preferred embodiments. Those skilled in the art can obviously make changes or appropriate changes and combinations to the methods and applications described in this article without departing from the content, spirit and scope of the present invention to implement and apply the technology of the present invention.
[0045] In the description of the present invention, it should be noted that the terms "first", "second", etc. are only used for descriptive purposes and do not indicate or imply relative importance.
[0046] In the description of the present invention, the list of items connected by the term "at least one of" or other similar terms may mean any combination of the listed items. For example, if items A and B are listed, then the phrase "at least one of A and B" means only A; only B; or A and B. In another example, if items A, B, and C are listed, then the phrase "at least one of A, B, and C" means only A; or only B; only C; A and B (excluding C); A and C (excluding B); B and C (excluding A); or all of A, B, and C. Item A may include a single element or multiple elements. Item B may include a single element or multiple elements. Item C may include a single element or multiple elements.
[0047] In the ranges disclosed herein, the endpoints and any values are not limited to the exact ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, between the endpoint values of each range, between the endpoint values of each range or individual point values, and between individual point values, they can be combined with each other to obtain one or more new numerical ranges, and these numerical ranges should be regarded as specifically disclosed herein.
[0048] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form new technical solutions.
[0049] Unless otherwise specified, all technical features and optional technical features of the present application can be combined with each other to form new technical solutions.
[0050] Unless otherwise specified, the terms "comprising" and "including" mentioned in the present application mean open-ended, and can also be closed-ended. For example, the said "comprising" and "including" can mean that other components not listed can also be included, or it can only include the components listed.
[0051] Specifically, the present invention adopts the following technical solutions:
[0052] In a first aspect, the present invention provides a separator, which includes a substrate and a functional coating provided on at least one surface of the substrate;
[0053] The functional coating includes a carbon material and ceramic particles. The carbon material has a spherical structure, and the spherical structure is provided with through holes penetrating the spherical structure.
[0054] The functional coating of the separator of the present invention includes carbon materials (porous carbon spheres) with through holes and ceramic particles. While ensuring its original heat resistance, more pores are added to the surface of the functional coating. Through the capillary action of the through holes of the porous carbon spheres, the electrolyte can be more effectively absorbed and stored, thereby improving the capacity retention rate of the battery under long cycles, effectively improving the life problem during the long-cycle rate cycling process, and enhancing the safety and cycle life of the battery. At the same time, the separator of the present invention can construct more lithium-ion channels on the surface layer of the separator, improve the penetration ability of lithium ions between the separators, improve the lithium plating situation caused by the aggregation of lithium ions on the surface layer, shorten the lithium-ion transmission distance, and improve the fast charging performance of the battery.
[0055] Preferably, the average particle size D of the carbon material 50 is 1.5 to 6 μm. Exemplarily, the average particle size D of the carbon material 50 is any value among 1.5 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm or any value within the range formed by any two of the above values. When the average particle size of the carbon material is within this range, it can be adapted to the existing inorganic coating formula and process of the separator, ensure good dispersion and coating effect of the slurry, and meet the requirements of the common coating thickness. When the average particle size is too large, the particles are prone to sedimentation, and the coating thickness is uncontrollable; when the average particle size is too small, the pore structure is not easy to play a role, affecting the transmission effect.
[0056] Preferably, the diameter of the through-holes is 0.2 to 2 μm. Exemplarily, the diameter of the through-holes is any value among 0.2 μm, 0.4 μm, 0.6 μm, 0.8 μm, 1 μm, 1.2 μm, 1.4 μm, 1.6 μm, 1.8 μm, 2 μm or any value within the range formed by any two of the above values. When the diameter of the through-holes is within this range, the electrolyte can be absorbed and stored more effectively, thereby improving the capacity retention rate of the battery under long-term cycling, effectively improving the life problem during the long-term rate cycling process, enhancing the safety and cycle life of the battery; more lithium-ion channels can be constructed on the surface layer of the separator, enhancing the penetration ability of lithium ions between the separators, improving the lithium deposition caused by the aggregation of lithium ions on the surface layer, shortening the lithium-ion transmission distance, and enhancing the fast charging performance of the battery.
[0057] In the embodiments of the present invention, the ceramic particles are at least one of alumina, boehmite, barium titanate, calcium oxide, magnesium oxide, zinc oxide, zirconia, and silica.
[0058] Preferably, the average particle size D of the ceramic particles 50 is 0.3 to 1.5 μm. Exemplarily, the average particle size D of the ceramic particles 50 is any value among 0.3 μm, 0.5 μm, 0.7 μm, 0.9 μm, 1 μm, 1.3 μm, 1.5 μm or any value within the range formed by any two of the above values. Within the above average particle size range, the functional coating can be made denser, play a better role in supporting the separator at high temperatures, and endow the separator with high-temperature resistance.
[0059] Preferably, the mass ratio of the carbon material to the ceramic particles is (4.7 to 28):(66 to 90). Exemplarily, the mass ratio of the carbon material to the ceramic particles is any value among 4.7:90, 9:85, 19:76, 20:71, 25:68, 28:66 or any value within the range formed by any two of the above values. When the mass ratio of the carbon material to the ceramic particles is within this range, the liquid absorption and retention effect of the pore structure of the carbon material on the electrolyte can be better exerted, the ion transport ability can be improved, and at the same time, the sufficient support of the coating for the separator can be ensured without having a negative impact on the thermal performance of the separator.
[0060] Preferably, the single-sided thickness of the functional coating is 2 to 10 μm. Exemplarily, the single-sided thickness of the functional coating is any value among 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm or any value within the range formed by any two of the above values.
[0061] In the embodiments of the present invention, the functional coating further includes a binder.
[0062] In an embodiment of the present invention, the binder includes at least one of polyacrylic acid, polyacrylate, polytetrafluoroethylene, styrene-butadiene rubber, polyacrylonitrile, and polyvinyl alcohol.
[0063] Preferably, the mass ratio of the carbon material, ceramic particles, and binder is (4.7 to 28):(66 to 90):(1 to 8). Exemplarily, the mass ratio of the carbon material, ceramic particles, and binder is any value among 4.7:90:4, 9:85:4, 19:76:4, 20:71:8, 25:68:5, 28:66:1 or any value within the range formed by any two of the above values.
[0064] In an embodiment of the present invention, the functional coating may further include at least one of a dispersant, a thickener, and a wetting agent.
[0065] In an embodiment of the present invention, the dispersant includes at least one of polyether silane, polyacrylate, and polyacrylate salts.
[0066] In an embodiment of the present invention, the thickener includes at least one of polyvinyl alcohol, sodium carboxymethyl cellulose, polyurethane, acrylate, and sodium polyacrylate.
[0067] In an embodiment of the present invention, the wetting agent includes at least one of polyether-modified silicone, modified succinic acid, and polyether-modified polydimethylsiloxane.
[0068] In an embodiment of the present invention, the substrate includes at least one of polypropylene, polyethylene, polypropylene / polyethylene / polypropylene, polyvinyl chloride, polyamide, and glass fiber.
[0069] Preferably, the thickness of the substrate is 4 to 20 μm. Exemplarily, the thickness of the substrate is any value among 4 μm, 6 μm, 8 μm, 10 μm, 12 μm, 14 μm, 16 μm, 18 μm, 20 μm or any value within the range formed by any two of the above values.
[0070] In a second aspect, the present invention provides a method for preparing the above diaphragm, including the following steps:
[0071] S1, providing a carbon material, the carbon material having a spherical structure, and the spherical structure being provided with through holes penetrating the spherical structure;
[0072] S2, mixing the carbon material, ceramic particles, binder, dispersant, thickener, wetting agent, and water evenly to obtain a functional coating slurry;
[0073] S3, coating the functional coating slurry on at least one surface of the substrate, and performing a drying treatment to obtain the diaphragm.
[0074] Preferably, the mass ratio of the carbon material, ceramic particles, binder, dispersant, thickener, and wetting agent is (4.7 to 28):(66 to 90):(1 to 8):(0.1 to 4):(0.1 to 4):(0.03 to 1.5). Exemplarily, the mass ratio of the carbon material, ceramic particles, binder, dispersant, thickener, and wetting agent is any value among 4.7:90:4:0.46:1:0.09, 9:85:4:0.46:1:0.09, 19:76:4:0.46:1:0.09, 20:71:8:0.1:4:0.03, 25:68:5:2:2:1, 28:66:1:4:0.1:1.5 or any value within the range formed by any two of the above values.
[0075] In the embodiment of the present invention, the preparation method of the carbon material includes the following steps:
[0076] S11, dissolving a first polymer in a first solvent to obtain an inner layer solution;
[0077] Dissolving a second polymer in a second solvent to obtain an outer layer solution;
[0078] S12, forming a core-shell structured fiber by coaxial electrospinning of the inner layer solution and the outer layer solution;
[0079] S13, adding the fiber into a third solvent for dissolution treatment, filtering and drying to obtain a carbon sphere precursor with a hollow structure;
[0080] S14, pre-sintering the carbon sphere precursor in an air atmosphere and then performing carbonization treatment in an inert gas atmosphere to obtain the carbon material.
[0081] In step S11 of the present invention:
[0082] In the embodiment of the present invention, the first polymer includes at least one of polymethyl methacrylate, polyethylene, polystyrene, and polyvinyl acetate.
[0083] In the embodiment of the present invention, the second polymer includes at least one of polyamide, polyacrylonitrile, polyvinyl alcohol, and polyvinyl chloride.
[0084] In the embodiment of the present invention, the first solvent and the second solvent independently include at least one of N,N-dimethylformamide, dimethylfuran, dimethyl sulfoxide, and N-methylpyrrolidone.
[0085] Preferably, the concentration of the inner layer solution is 7 wt% to 20 wt%. Exemplarily, the concentration of the inner layer solution is any value among 7 wt%, 8 wt%, 10 wt%, 12 wt%, 14 wt%, 16 wt%, 18 wt%, 20 wt% or any value within the range formed by any two of the above values.
[0086] Preferably, the concentration of the outer layer solution is 7 wt% to 30 wt%. Exemplarily, the concentration of the outer layer solution is any value among 7 wt%, 8 wt%, 10 wt%, 12 wt%, 14 wt%, 16 wt%, 18 wt%, 20 wt%, 22 wt%, 24 wt%, 26 wt%, 28 wt%, 30 wt% or any value within the range formed by any two of the above values.
[0087] In step S12 of the present invention:
[0088] Preferably, the voltage for coaxial electrospinning is 10 - 30 kV, the feeding rate of the inner layer solution is 20 - 500 mL / min, the feeding rate of the outer layer solution is 25 - 250 mL / min, the ratio of the feeding rate of the inner layer solution to the feeding rate of the outer layer solution is 0.2 - 2.0, and the electrode distance is 15 - 30 cm. The above technical parameters of electrospinning are conventional parameters, and those skilled in the art can select them according to needs. Among them, the ratio of the feeding rate of the inner layer solution to the feeding rate of the outer layer solution will affect the proportion of the second polymer in the outer layer solution. The larger this proportion is, the smaller the pore size, the less the active surface, and the better the cycling performance.
[0089] In step S13 of the present invention:
[0090] In the embodiment of the present invention, the third solvent includes at least one of toluene, tetrahydrofuran, xylene, and amyl acetate. Since the shell layer of the core-shell structure is insoluble in the third solvent while the core is soluble in the third solvent, the core in the sphere will be dissolved by the third solvent, leaving a hollow pore.
[0091] In step S14 of the present invention:
[0092] Preferably, the temperature for pre-sintering treatment is 200 - 400 °C, and the heat preservation time for pre-sintering treatment is 1 - 5 h. Exemplarily, the temperature for pre-sintering treatment is any value among 200 °C, 220 °C, 240 °C, 260 °C, 280 °C, 300 °C, 320 °C, 340 °C, 360 °C, 380 °C, 400 °C or any value within the range formed by any two of the above values, and the heat preservation time for pre-sintering treatment is any value among 1 h, 2 h, 3 h, 4 h, 5 h or any value within the range formed by any two of the above values. The pre-sintering treatment can prevent the second polymer from sintering into blocks during the sintering process.
[0093] Preferably, the temperature of the carbonization treatment is 1200-1500 °C, and the heat preservation time of the carbonization treatment is 1-6 h. Exemplarily, the temperature of the carbonization treatment is any value among 1200 °C, 1250 °C, 1300 °C, 1350 °C, 1400 °C, 1450 °C, 1500 °C or any value within the range value composed of any two of the above values, and the heat preservation time of the carbonization treatment is any value among 1 h, 2 h, 3 h, 4 h, 5 h, 6 h or any value within the range value composed of any two of the above values. In the carbonization treatment, the second polymer should be completely carbonized. If the temperature is too low or the time is too short, incomplete carbonization will occur, affecting the electrical conductivity of the material.
[0094] Thirdly, the present invention provides a battery, which includes the above-mentioned separator and / or the separator prepared by the above-mentioned preparation method.
[0095] In the embodiments of the present invention, the battery structure includes but is not limited to coin cells, soft-pack batteries, cylindrical batteries, etc.
[0096] The present application has no special restrictions on the positive electrode sheet, negative electrode sheet, and electrolyte in the battery. Those skilled in the art can select according to actual needs as long as the purpose of the present application can be achieved.
[0097] The reagents, instruments, materials, etc. used in the present invention can all be obtained through commercial channels.
[0098] The following further elaborates the present invention in conjunction with embodiments:
[0099] Example 1
[0100] 1. Preparation of porous carbon spheres:
[0101] (1) Poly(methyl methacrylate) was added to N,N-dimethylformamide and heated and stirred at 60 °C at a rate of 500 rpm for 60 min to prepare an inner layer solution with a concentration of 10 wt.%; polyamide was added to N,N-dimethylformamide and heated and stirred at 60 °C at a rate of 500 rpm for 60 min to prepare an outer layer solution with a concentration of 10 wt.%, and reserved;
[0102] (2) Using a coaxial electrospinning device, the voltage was set to 10 kV, the feeding rate of the inner layer solution was 50 mL / min, the feeding rate of the outer layer solution was 250 mL / min, and the ratio of the two feeding rates was controlled to 0.2, and the electrode distance was 30 cm; then, a core-shell structured fiber filament was prepared by coaxial electrospinning and reserved;
[0103] (3) Add the obtained fiber filaments to excessive toluene, mix at 100 °C at a rotation speed of 200 rpm for 1 h to dissolve the core, then filter with a suction filtration device and collect the filter cake. The filter cake is dried to obtain a carbon sphere precursor for standby;
[0104] (4) Under an air atmosphere, pre-sinter the obtained carbon sphere precursor at 200 °C for 5 h, and then calcine and carbonize it at 1200 °C for 6 h under nitrogen protection. After cooling, a porous carbon sphere is obtained. Its structural schematic diagram is as Figure 1 and Figure 2 shown. The average particle size D 50 is 1.8 μm, and the diameter of the through holes is 0.2 - 0.5 μm.
[0105] 2. Preparation of the functional coating separator:
[0106] Weigh 9.68 kg of alumina with D 50 being 0.8 μm, 0.51 kg of porous carbon spheres, 0.13 kg of ammonium polyacrylate (solid content 37%, actual addition amount 0.05 kg), and 17.73 kg of water and add them to the double planetary stirring tank body in sequence. Mix thoroughly to obtain a premix. Then weigh 2.96 kg of sodium carboxymethylcellulose solution (solid content 4%, actual addition amount 0.108 kg) and add it to the premix. Stir and disperse thoroughly to obtain a mixture slurry. Add the completely dispersed mixture slurry to a sand mill for sanding to obtain a semi-finished slurry. Then weigh 0.96 kg of polyacrylate (solid content 45%, actual addition amount 0.431 kg) and add it to the stirring tank containing the semi-finished slurry. After stirring and dispersing thoroughly, add 9.51 g of polyether-modified silicone for stirring to obtain a finished slurry. Finally, uniformly coat the finished slurry on one side of a 7-μm-thick polyethylene substrate by gravure coating. The coating thickness is 3 μm, and it is dried at 45 °C to obtain a functional coating separator.
[0107] Example 2
[0108] 1. Preparation of porous carbon spheres:
[0109] Same as Example 1.
[0110] 2. Preparation of the functional coating separator:
[0111] Weigh 9.93 kg of D 50Boehmite with a particle size of 1.0 μm, 0.52 kg of porous carbon spheres, 0.13 kg of sodium polyacrylate (solid content 37%, actual addition 0.05 kg), and 18.17 kg of water were successively added to the double planetary stirring tank body, and thoroughly mixed to obtain a premix. Then, 2.76 kg of sodium carboxymethyl cellulose solution (solid content 4%, actual addition 0.111 kg) was weighed and added to the premix, and thoroughly stirred and dispersed to obtain a mixture slurry. The completely dispersed mixture slurry was added to a sand mill for sanding to obtain a semi-finished slurry. Subsequently, 0.98 kg of polyacrylate (solid content 45%, actual addition 0.442 kg) was weighed and added to the stirring tank containing the semi-finished slurry. After thorough stirring and dispersion, 9.75 g of polyether-modified silicone was added and stirred to obtain a finished slurry. Finally, the finished slurry was evenly coated on one side of a 7-μm-thick polyethylene substrate by gravure coating, with a coating thickness of 2 μm, and dried at 45°C to obtain a functional coating separator.
[0112] Example 3
[0113] The difference between this example and Example 1 is that the addition amount of alumina is 9.17 kg, and the addition amount of porous carbon spheres is 1.02 kg.
[0114] Example 4
[0115] The difference between this example and Example 1 is that the addition amount of alumina is 8.15 kg, and the addition amount of porous carbon spheres is 2.04 kg.
[0116] Comparative Example 1
[0117] The difference between this comparative example and Example 1 is that the addition amount of alumina is 10.19 kg, and no porous carbon spheres are added.
[0118] Comparative Example 2
[0119] The difference between this comparative example and Example 2 is that commercial microporous carbon spheres (particle size D 50 is 0.5 μm, porosity is 60%) are used instead of porous carbon spheres.
[0120] Performance Test of the Separator
[0121] Test the coating air permeability and liquid absorption and retention performance of the separators in the examples and comparative examples.
[0122] (1) Test method for the coating air permeability of the separator:
[0123] Samples were cut from the separator along the TD direction, with a width of ≥5 cm, and 5 samples were taken for each group. Using a Gurley 4340CJ air permeability tester, the cut and flawless samples were placed into the sample port, and "ENTER" was pressed to start the test. The air permeability of the base film and the coated film was measured, and the difference between the two was the increased air permeability of the coating. The average value of all the increased air permeabilities of the coating was recorded as the air permeability of the separator coating.
[0124] (2) Test method for liquid absorption and retention performance:
[0125] The separator was cut into 100 mm×100 mm samples, and the mass m1 before the test was obtained by weighing using an electronic balance. Then the samples were completely immersed in a beaker filled with electrolyte, taken out after 2 h, wiped clean of the residual electrolyte on the surface, and weighed to obtain m2. After that, the samples were left standing for 1 h and weighed again to obtain m3.
[0126] Liquid absorption rate = (m2 - m1) / m1
[0127] Liquid retention rate = (m3 - m1) / m1
[0128] The test results are shown in Table 1.
[0129] Table 1
[0130]
[0131] Compared with Comparative Examples 1-2, Examples 1-4 have better air permeability and liquid absorption and retention performance.
[0132] From the above Examples 1 and Comparative Example 1, in the case of using pore carbon spheres in Example 1, the presence of through pores in the coating improves the air permeability of the separator, and the increase in capillary action and pores significantly improves the liquid absorption and retention performance.
[0133] From Examples 2 and Comparative Example 2, the microporous carbon spheres in Comparative Example 2 have no through pores in their structure, and the particle size is only about 0.5 μm. After addition, the air permeability of the separator increases more, but the air permeability becomes worse. The surface functional groups have a certain improvement in the infiltration of the electrolyte, but are not beneficial to the liquid retention.
[0134] Preparation and performance test of the battery
[0135] 1. Preparation of the battery:
[0136] The commercial positive electrode sheet, commercial negative electrode sheet, and separator (the separators prepared in the above examples and comparative examples) were wound to obtain a bare battery cell, the positive and negative electrode tabs were welded, the bare battery cell was installed in an aluminum plastic film battery case (or aluminum battery case / steel battery case / nickel-plated battery case), injected with electrolyte, encapsulated, left standing, formed, and capacity-divided to obtain a lithium-ion battery.
[0137] 2. Performance test of the battery:
[0138] (1) Test method for capacity retention rate after 1000 cycles:
[0139] In a constant-temperature test cabinet at 25°C, first charge at a constant current of 2C to 4.4V, then charge at a constant voltage of 4.4V until the current reaches 0.05C for cutoff, and then discharge at a constant current of 2C to 2.8V. Record the discharge capacity of the first cycle. This is one charge-discharge cycle. Repeat the above charge-discharge cycle 1000 times, and record the discharge capacity of the 1000th cycle. The formula for calculating the capacity retention rate is: (discharge capacity of the 1000th cycle / discharge capacity of the first cycle) * 100%.
[0140] (2) Test method for rate discharge retention rate:
[0141] In a constant-temperature test cabinet at 25°C, first discharge at a constant current of 1C to 2.8V, then charge at a constant current of 1C to 4.4V, and then discharge at a constant current of XC (XC is 1C, 2C, or 4C) to 2.8V. Record the discharge capacity at each rate. The formula for calculating the rate discharge retention rate is: (discharge capacity at XC / discharge capacity at 1C) * 100%
[0142] The results are shown in Table 2.
[0143] Table 2
[0144]
[0145] Compared with Comparative Examples 1-2, Examples 1-4 have better cycle performance and rate performance.
[0146] From the comparison between Example 1 and Comparative Example 1 above, in the case of using pore carbon spheres in Example 1, the presence of through pores in the coating improves the air permeability of the separator. The increase in capillary action and pores significantly improves the liquid absorption and retention performance. At the same time, both the rate discharge and the rate cycle retention rate are increased.
[0147] From the comparison between Example 2 and Comparative Example 2, since the microporous carbon spheres in Comparative Example 2 have no through pores in their structure and the particle size is only about 0.5μm, the addition increases the air permeability of the separator more. Its surface functional groups have a certain improvement in electrolyte wetting, but it is not beneficial to liquid retention. In addition, the retention rate is poor under long cycles.
[0148] The above are only the preferred embodiments of the present invention. It should be noted that for those of ordinary skill in the art, without departing from the principle of the present invention, several improvements and refinements can be made, and these improvements and refinements should also be regarded as the protection scope of the present invention.
Claims
1. A diaphragm, characterized in that: The diaphragm includes a substrate and a functional coating disposed on at least one surface of the substrate; The functional coating comprises a carbon material and ceramic particles, the carbon material is in a spherical structure, and the spherical structure is provided with a through hole penetrating the spherical structure.
2. The diaphragm according to claim 1, characterized in that The average particle size D of the carbon material 50 1.5~6μm; And / or, the diameter of the through hole is 0.2-2 μm.
3. The diaphragm according to claim 1, characterized in that The mass ratio of the carbon material to the ceramic particles is (4.7-28):(66-90).
4. The diaphragm according to claim 1, characterized in that The thickness of the functional coating on one side is 2-10 μm.
5. The diaphragm according to claim 1, characterized in that The functional coating further comprises a binder; The mass ratio of the carbon material, the ceramic particles and the binder is (4.7-28):(66-90):(1-8).
6. The method for preparing the diaphragm according to any one of claims 1 to 5, characterized in that: The steps include: S1, providing a carbon material, wherein the carbon material is in a spherical structure, and the spherical structure is provided with a through hole penetrating the spherical structure; S2, mixing the carbon material, ceramic particles, a binder, a dispersant, a thickener, a wetting agent and water to obtain a functional coating slurry; S3, coating the functional coating slurry on at least one surface of a substrate, and drying the slurry to obtain the diaphragm.
7. The preparation method according to claim 6, characterized in that: The method for preparing the carbon material comprises the following steps: S11, dissolving a first high molecular polymer in a first solvent to obtain an inner layer solution; dissolving the second high molecular weight polymer in the second solvent to obtain an outer layer solution; S12, preparing fiber filaments with a core-shell structure by coaxial electrospinning the inner layer solution and the outer layer solution; S13, adding the fiber filaments into a third solvent for dissolution treatment, filtering and drying to obtain a carbon sphere precursor with a hollow structure; S14, pre-sintering the carbon sphere precursor in an air atmosphere, and then carbonizing it in an inert gas atmosphere to obtain the carbon material.
8. The preparation method according to claim 7, characterized in that: In the step S11, The first high molecular polymer includes at least one of polymethyl methacrylate, polyethylene, polystyrene, and polyvinyl acetate; And / or, the second high molecular polymer includes at least one of polyamide, polyacrylonitrile, polyvinyl alcohol and polyvinyl chloride; and / or, the first solvent and the second solvent independently include at least one of N,N-dimethylformamide, dimethylfuran, dimethyl sulfoxide, and N-methylpyrrolidone; and / or, the concentration of the inner layer solution is 7wt% to 20wt%; and / or, the concentration of the outer layer solution is 7wt% to 30wt%; In the step S12, The voltage of the coaxial electrospinning is 10-30 kV, the propulsion rate of the inner layer solution is 20-500 mL / min, the propulsion rate of the outer layer solution is 25-250 mL / min, the propulsion rate ratio of the inner layer solution to the outer layer solution is 0.2-2.0, and the electrode distance is 15-30 cm.
9. The preparation method according to claim 7, characterized in that: In step S13, The third solvent includes at least one of toluene, tetrahydrofuran, xylene, and amyl acetate; In step S14, The temperature of the pre-sintering treatment is 200-400° C., and the holding time of the pre-sintering treatment is 1-5 hours; And / or, the temperature of the carbonization treatment is 1200-1500° C., and the insulation time of the carbonization treatment is 1-6 hours.
10. A battery, characterized in that: The battery comprises the separator according to any one of claims 1 to 5, and / or the separator prepared by the preparation method according to any one of claims 6 to 9.