Non-oriented electrical steel sheet and method for producing same

By adding a rapid annealing step to the hot-rolled plate process of the electrical steel plate, the grains of specific orientation are formed, and the problem of reducing the magnetic flux density of the existing electrical steel plate is solved, and the effect of uniform magnetic properties is achieved in all directions is excellent, which is suitable for the manufacturing of high-efficiency motor cores.

CN120187884APending Publication Date: 2025-06-20POHANG IRON & STEEL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380077661.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-11-18
Filing Date
2023-10-11
Publication Date
2025-06-20

AI Technical Summary

Technical Problem

After the existing electrical steel plates are added with high resistivity alloy elements, the magnetic flux density is reduced, making it difficult to meet the high-frequency and low iron loss requirements of electric vehicle drive motors. At the same time, the process of adding high aluminum also leads to increased surface defects and deterioration of motor axial characteristics.

Method used

In the process of pre-rolling and cold rolling of hot-rolled plates, rapid annealing is performed between pre-rolling and cold rolling to form grains with specific orientations, thereby achieving uniform magnetic properties throughout the direction.

Benefits of technology

It achieves excellent omnidirectional flux density and iron loss of electrical steel plates, and is suitable for the manufacture of environmentally friendly automobile motors, high-efficiency home appliance motors, and ultra-high-end motor cores.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

A non-oriented electrical steel sheet according to one embodiment of the present invention comprises, in weight%, Si: 2.5 to 4.0%, Al: 0.03 to 2.0%, and Mn: 0.03 to 2.0%, with the remainder comprising Fe and unavoidable impurities, lt; 111gt, 111gt; the area fraction of / ND crystal grains is 20% or less, lt; 100 gt; / ND grain area fraction and lt; 110gt, 110gt; the ratio of the area fraction / ND crystal grains is 1.01 or more.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] One embodiment of the present invention relates to a non-oriented electrical steel sheet and a method for manufacturing the same. Specifically, one embodiment of the present invention relates to a non-oriented electrical steel sheet and a method for manufacturing the same. In the process of pre-rolling and cold-rolling a hot-rolled sheet, annealing is performed between pre-rolling and cold-rolling, and the temperature is rapidly increased during annealing, thereby forming grains with a specific orientation and having excellent magnetic uniformity in the entire direction. Background Art

[0002] Recently, due to the increase in disasters caused by climate change, countries around the world have issued carbon neutral roadmaps for 2050. The total carbon emissions in 2020 reached 3.9 billion tons, of which the emissions from internal combustion engines accounted for 24%, reaching 940 million tons. Therefore, the demand for achieving carbon neutrality in this field through the electrification of internal combustion engines is very urgent. For this reason, in the field of mobility, the electrification process led by electric vehicles is rapidly advancing. The required characteristics of drive motors in new mobility are to increase the driving range and the maximum speed. This is directly related to the low iron loss characteristics of electrical steel sheets. If the iron loss of the electrical steel sheet is low, the efficiency can be further improved, thereby further increasing the driving range. Therefore, the high-frequency low iron loss characteristics of electrical steel sheets are essential. For this reason, electrical steel sheets usually contain a large amount of Si, and a large amount of elements such as Al, Mn, and Cr are added to ensure high-frequency low iron loss.

[0003] However, when a large amount of high-resistivity alloy elements such as Si, Al, Mn, and Cr are added, the problem of reduced magnetic flux density will occur. Especially, materials that continuously require lightweight in electric vehicle drive motors must use materials with high magnetic flux density.

[0004] For this reason, a method for improving characteristics by thinning the hot-rolled sheet has been proposed, and a method for improving magnetism by containing high aluminum and undergoing two annealings and two rollings has been proposed. In addition, a method for achieving hot-rolled thinning by a thin slab manufacturing method has been proposed.

[0005] However, for the method of reducing the thickness of the hot-rolled sheet, in the conventional hot-rolling process, due to the increase in rolling load, it is difficult to achieve mass production. And although the addition of high aluminum and the two annealing and two rolling processes have confirmed the improvement of magnetism to a certain extent, the {110}<001> Gaussian texture also develops simultaneously, so the axial characteristics of the motor deteriorate, and the surface defects caused by the addition of high aluminum also increase significantly. Summary of the Invention

[0006] (I) Technical Problems to be Solved

[0007] In one embodiment of the present invention, it aims to provide a non-oriented electrical steel sheet and a manufacturing method thereof. Specifically, in one embodiment of the present invention, it aims to provide a non-oriented electrical steel sheet and a manufacturing method thereof. In the processes of pre-rolling and cold-rolling a hot-rolled sheet, annealing is carried out between pre-rolling and cold-rolling, and the temperature is rapidly raised during annealing, thereby forming grains with a specific orientation and having excellent magnetic uniformity in the whole direction.

[0008] (II) Technical Solution

[0009] In the non-oriented electrical steel sheet according to one embodiment of the present invention, by weight%, the non-oriented electrical steel sheet contains Si: 2.5 to 4.0%, Al: 0.03 to 2.0%, and Mn: 0.03 to 2.0%, and the balance contains Fe and inevitable impurities. The area fraction of <111> / ND grains is 20% or less, and the ratio of the area fraction of <100> / ND grains to the area fraction of <110> / ND grains is 1.01 or more.

[0010] <100> / ND grains are grains in which the <100> axis of the grains is within a range of 15 degrees or less from the vertical axis (ND) of the steel sheet surface. <111> / ND grains represent grains in which the <111> axis of the grains is within a range of 15 degrees or less from the vertical axis (ND) of the steel sheet surface. <110> / ND grains represent grains in which the <110> axis of the grains is within a range of 15 degrees or less from the vertical axis (ND) of the steel sheet surface. The area fraction refers to the proportion of the area occupied by grains with a specific orientation in the total area of the steel sheet measured by electron backscatter diffraction (EBSD).

[0011] In the non-oriented electrical steel sheet according to one embodiment of the present invention, the area fraction of <100> / ND grains can be 10% or more.

[0012] In the non-oriented electrical steel sheet according to one embodiment of the present invention, it may further contain one or more of Cu: 0.005 to 0.2% by weight, Cr: 0.01 to 0.5% by weight, Ni: less than 0.05% by weight and excluding 0%, Zn: less than 0.01% by weight and excluding 0%.

[0013] In the non-oriented electrical steel sheet according to one embodiment of the present invention, it may further contain one or more of P: less than 0.1% and excluding 0%, C: less than 0.003% and excluding 0%, S: less than 0.004% and excluding 0%, Ti: less than 0.003% and excluding 0%, N: less than 0.003% and excluding 0%.

[0014] An non-oriented electrical steel sheet according to an embodiment of the present invention may further contain one or more of Mo: 0.03% by weight or less, excluding 0%, B: 0.0050% by weight or less, excluding 0%, V: 0.0050% by weight or less, excluding 0%, Ca: 0.0050% by weight or less, excluding 0%, Nb: 0.0050% by weight or less, excluding 0%, and Mg: 0.0050% by weight or less, excluding 0%.

[0015] An non-oriented electrical steel sheet according to an embodiment of the present invention may further contain one or two or more of Sn, Sb, Bi, Pb, Ge, and As, and the content of each or their total is 0.005 to 0.200% by weight.

[0016] An non-oriented electrical steel sheet according to an embodiment of the present invention may satisfy one or more of the following formulas 1 to 3.

[0017] [Formula 1]

[0018] (B50 L +B50 C ) / 2≥1.63

[0019] [Formula 2]

[0020] {(B50 L +B50 C+ B50 60 ) / 3} / {(B50 L +B50 C ) / 2}≥0.95

[0021] [Formula 3]

[0022] B50 60 / {(B50 L +B50 C ) / 2}≥0.90

[0023] Wherein, in Formulas 1 to 3, B50 L represents the magnetic flux density (B50, Tesla) measured in the rolling direction, B50 C represents the magnetic flux density (B50, Tesla) measured in the direction perpendicular to the rolling direction, and B50 60 represents the magnetic flux density (B50, Tesla) measured in the direction at an angle of 60 degrees with the rolling direction.

[0024] An non-oriented electrical steel sheet according to an embodiment of the present invention may satisfy the following formula 4.

[0025] [Formula 4]

[0026] (W10 / 400 L+W10 / 400 C ) / 2 ≤ 6.885×e (2.99×t)

[0027] Among them, in Equation 4, W10 / 400 L is the iron loss measured in the rolling direction (W10 / 400, W / kg), and W10 / 400 C is the iron loss measured in the direction perpendicular to rolling (W10 / 400, W / kg), e is the natural constant, and t represents the thickness of the electrical steel sheet (mm).

[0028] A method for manufacturing a non-oriented electrical steel sheet according to an embodiment of the present invention includes: a step of hot rolling a slab to manufacture a hot-rolled sheet, wherein, by weight%, the slab contains Si: 2.5 to 4.0%, Al: 0.03 to 2.0%, and MN: 0.03 to 2.0%, and the balance contains Fe and inevitable impurities; a step of pre-cold rolling the hot-rolled sheet at 20 to 80% to manufacture a pre-cold-rolled sheet; a heating step of heating the pre-cold-rolled sheet at a heating rate of 20°C / second (s) or more; an intermediate annealing step of annealing the pre-cold-rolled sheet; a step of cold rolling the annealed pre-cold-rolled sheet at a reduction rate of 30 to 80% to manufacture a cold-rolled sheet; and a cold-rolled sheet annealing step of annealing the cold-rolled sheet.

[0029] The step of manufacturing the hot-rolled sheet may include a step of finish rolling at a temperature of 850°C or higher.

[0030] The step of manufacturing the hot-rolled sheet may include a step of performing water cooling after 0.1 second or more has elapsed after finish rolling.

[0031] The step of manufacturing the hot-rolled sheet may include a step of coiling at a temperature of 600 to 800°C.

[0032] The slab may further contain one or more of Cu: 0.005 to 0.2% by weight, Cr: 0.01 to 0.5% by weight, Ni: less than 0.05% by weight and excluding 0%, Zn: less than 0.01% by weight and excluding 0%.

[0033] The slab may further contain one or more of P: less than 0.1% and excluding 0%, C: less than 0.003% and excluding 0%, S: less than 0.004% and excluding 0%, Ti: less than 0.003% and excluding 0%, N: less than 0.003% and excluding 0%.

[0034] The slab may further contain one or two or more of Sn, Sb, Bi, Pb, Ge, and As, and their respective or total contents are 0.005 to 0.200% by weight.

[0035] The slab may further contain one or more of Mo: not more than 0.03% by weight and excluding 0%, B: not more than 0.0050% by weight and excluding 0%, V: not more than 0.0050% by weight and excluding 0%, Ca: not more than 0.0050% by weight and excluding 0%, Nb: not more than 0.0050% by weight and excluding 0%, and Mg: not more than 0.0050% by weight and excluding 0%.

[0036] (III) Advantageous Effects

[0037] The non-oriented electrical steel sheet according to an embodiment of the present invention has excellent magnetic flux density and iron loss in all directions.

[0038] Ultimately, the non-oriented electrical steel sheet according to an embodiment of the present invention contributes to the manufacture of motors for environmentally friendly vehicles, motors for high-efficiency household appliances, and ultra-high-end motor cores. Detailed Embodiments

[0039] The terms first, second, third, etc. are used to describe each part, component, region, layer, and / or section, but these parts, components, regions, layers, and / or sections should not be limited by these terms. These terms are only used to distinguish one part, component, region, layer, or section from another part, component, region, layer, or section. Therefore, without departing from the scope of the present invention, the first part, component, region, layer, or section described below may also be described as the second part, component, region, layer, or section.

[0040] The terms used herein are only for describing specific embodiments and are not intended to limit the present invention. Unless the context clearly gives the opposite meaning, the singular forms used herein are also intended to include the plural forms. The term "comprising" used in the specification may specifically refer to a certain property, field, integer, step, action, element, and / or component, but does not exclude the existence or addition of other properties, fields, integers, steps, actions, elements, and / or components.

[0041] If a part is described as being on another part, there may be other parts directly on the other part or there may be other parts therebetween. When a part is described as being directly on another part, there are no other parts therebetween.

[0042] Although not otherwise defined, the meanings of all terms (including technical terms and scientific terms) used herein are the same as those commonly understood by those of ordinary skill in the art to which the present invention pertains. For terms defined in a dictionary, they should be interpreted as having a meaning consistent with the relevant technical literature and the content disclosed herein, and should not be interpreted in an idealized or overly formal sense.

[0043] In addition, unless otherwise specifically stated, % represents % by weight, and 1 ppm is 0.0001% by weight.

[0044] In one embodiment of the present invention, further comprising an additional element means that the additional element replaces the remaining iron (Fe), and the replacement amount is equivalent to the addition amount of the additional element.

[0045] Hereinafter, embodiments of the present invention will be described in detail so that those of ordinary skill in the art to which the present invention pertains can easily implement the present invention. However, the present invention can be implemented in various different ways and is not limited to the embodiments described herein.

[0046] An non-oriented electrical steel sheet according to an embodiment of the present invention, in weight %, the non-oriented electrical steel sheet contains Si: 2.5 to 4.0%, Al: 0.03 to 2.0%, and Mn: 0.03 to 2.0%, and the balance contains Fe and inevitable impurities.

[0047] First, the reasons for the composition limitations of the non-oriented electrical steel sheet will be described.

[0048] Si: 2.5 to 4.0 wt%

[0049] Silicon (Si) plays a role in increasing the resistivity of the material to reduce iron loss, so a relatively large amount needs to be added. If too little Si is added, the improvement effect on high-frequency iron loss may be negligible. If too much Si is added, the hardness of the material increases, resulting in poor productivity and blanking performance, so it is not advisable. More specifically, Si can contain 2.9 to 3.7 wt%.

[0050] Al: 0.03 to 2.0 wt%

[0051] Aluminum (Al) plays a role in increasing the resistivity of the material to reduce iron loss, so a large amount needs to be added. If too little Al is added, there is no effect on reducing high-frequency iron loss, fine nitrides are formed, and magnetic properties may deteriorate. If too much Al is added, there may be a problem of changing the physical properties of the mold powder during the continuous casting process, resulting in a significant decrease in productivity. More specifically, Al can contain 0.1 to 1.8 wt%, and further specifically, Al can contain 0.5 to 1.5 wt%.

[0052] Mn: 0.03 to 2.0 wt%

[0053] Manganese (Mn) plays a role in increasing the resistivity of the material to improve iron loss and forming sulfides. If too little Mn is added, fine precipitation of MnS may occur, resulting in magnetic property deterioration. If too much Mn is added, it promotes the formation of a <111> / ND texture that is unfavorable for magnetism, and the magnetic flux density may rapidly decrease. More specifically, Mn can contain 0.05 to 1.9 wt%.

[0054] An non-oriented electrical steel sheet according to an embodiment of the present invention may further contain one or more of Cu: 0.005 to 0.2 wt%, Cr: 0.01 to 0.5 wt%, Ni: less than 0.05 wt% and excluding 0%, Zn: less than 0.01 wt% and excluding 0%.

[0055] Cu: 0.005 to 0.200 wt%

[0056] Copper (Cu) plays a role in forming sulfides together with Mn. If too little Cu is added when further adding Cu, fine precipitation of (Cu·Mn)S may occur, which may lead to magnetic deterioration. If too much Cu is added, high-temperature brittleness occurs, and cracks may form during continuous casting or hot rolling. More specifically, Cu may contain 0.01 to 0.10 wt%.

[0057] Cr: 0.01 to 0.50 wt%

[0058] Chromium (Cr) plays a role in improving the resistivity to improve iron loss. If too little Cr is added, the effect of increasing the resistivity may be insufficient. If the Cr content is too high, the magnetic flux density may decrease. More specifically, Cr may contain 0.050 to 0.20 wt%.

[0059] Ni: less than 0.05 wt%

[0060] Nickel (Ni) reacts with impurity elements to form fine sulfides, carbides and nitrides, which may have an adverse effect on magnetism. More specifically, Ni may contain 0.001 to 0.03 wt%.

[0061] Zn: less than 0.01 wt%

[0062] For zinc (Zn), if the content is too high, it may cause magnetic deterioration as an impurity. Therefore, Zn can be further added within the aforementioned range. More specifically, Zn may contain 0.001 to 0.005 wt%.

[0063] An non-oriented electrical steel sheet according to an embodiment of the present invention may further contain one or more of P: less than 0.1% and excluding 0%, C: less than 0.003% and excluding 0%, S: less than 0.004% and excluding 0%, Ti: less than 0.003% and excluding 0%, N: less than 0.003% and excluding 0%.

[0064] P: less than 0.1 wt%

[0065] Phosphorus (P), as a grain boundary segregation element, can increase the magnetic flux density, but if too much is added, the brittleness of the steel sheet increases and the weldability deteriorates. More specifically, P may contain 0.0001 to 0.0500 wt%.

[0066] C: 0.003 wt% or less

[0067] Carbon (C) reacts with N, Ti, Nb, V, etc. to form fine carbides, thereby having an effect of hindering grain growth and magnetic domain movement, which may lead to magnetic deterioration. More specifically, C may contain 0.0001 to 0.0025 wt%.

[0068] S: 0.004 wt% or less

[0069] Sulfur (S) is an element that forms sulfides such as MnS, which inhibits grain growth and may lead to poor magnetic properties. More specifically, S may contain 0.0001 to 0.0030 wt%.

[0070] Ti: 0.003 wt% or less

[0071] Titanium (Ti) forms carbonitrides, thereby having an effect of hindering magnetic domain movement, so it can be limited. More specifically, Ti may contain 0.0001 to 0.0025 wt%.

[0072] N: 0.003 wt% or less

[0073] Nitrogen (N) combines with Ti, Nb, V to form nitrides, which may lead to a decrease in grain growth. More specifically, N may contain 0.0001 to 0.0025 wt%.

[0074] The non-oriented electrical steel sheet according to an embodiment of the present invention may further contain one or more of Sn, Sb, Bi, Pb, Ge, and As, and the content of each or their total is 0.005 to 0.200 wt%.

[0075] When the foregoing elements are further added, they segregate at grain boundaries, relieve stress concentration at grain boundaries during cold rolling, and inhibit the recrystallization of <111> / ND-oriented grains during subsequent process recrystallization annealing, thereby increasing the magnetic flux density. If these elements are added appropriately, the foregoing effects can be further obtained, while if the content is too much, a large amount of segregation occurs, which inhibits grain growth and may lead to deterioration of magnetic flux density and iron loss instead. More specifically, it may further contain one or more of Sn, Sb, Bi, Pb, Ge, and As, and the content of each or their total is 0.010 to 0.100 wt%.

[0076] The non-oriented electrical steel sheet according to an embodiment of the present invention may further contain one or more of Mo: 0.03 wt% or less, B: 0.0050 wt% or less, V: 0.0050 wt% or less, Ca: 0.0050 wt% or less, Nb: 0.0050 wt% or less, and Mg: 0.0050 wt% or less.

[0077] These elements react with inevitably included elements such as C, S, and N to form fine carbides, nitrides, or sulfides, which may have an adverse effect on magnetism. Therefore, the upper limit can be restricted as described above.

[0078] Other impurities

[0079] In addition to the aforementioned elements, inevitably mixed impurities can be included. Regarding the inevitable impurities, they are impurities mixed in the steelmaking step and the manufacturing process of the non-oriented electrical steel sheet, which are well-known in the art, so the specific description is omitted. In one embodiment of the present invention, in addition to the aforementioned alloy components, the addition of other elements is not excluded, and the inclusion method can be different within the scope that does not damage the technical idea of the present invention. If additional elements are further included, they replace a part of the remaining Fe.

[0080] For the non-oriented electrical steel sheet according to one embodiment of the present invention, the area fraction of <111> / ND grains is 20% or less, and the ratio of the area fraction of <100> / ND grains to the area fraction of <110> / ND grains is 1.01 or more.

[0081] Among them, <100> / ND grains are grains whose <100> axis of the grains is within the range of 15 degrees or less from the vertical axis (ND) of the steel sheet surface, <111> / ND grains indicate that the <111> axis of the grains is within the range of 15 degrees or less from the vertical axis (ND) of the steel sheet surface, and <110> / ND grains indicate that the <110> axis of the grains is within the range of 15 degrees or less from the vertical axis (ND) of the steel sheet surface. The area fraction refers to the proportion of the area occupied by grains with a specific orientation in the total area of the steel sheet measured by electron backscatter diffraction (EBSD). EBSD is usually installed on a scanning electron microscope (Scanning Electron Microscope), for example, it can be the EBSD measurement device of TSL Company on the JEOL JSM-7200F device. The range within 15 degrees means that the angle between the vertical axis of the steel sheet surface and any plane containing the corresponding orientation is within 15 degrees, and it can be measured by the EBSD crystal orientation analysis program (OIM) of TSL Company.

[0082] In this way, when the orientation of the grains is appropriately adjusted, the magnetism in the entire direction of the steel sheet can be further uniformly improved.

[0083] In one embodiment of the present invention, for the grain orientation and its area fraction, the steel sheet is cut parallel to the plate thickness direction, and the crystal orientation of the grains is analyzed by measuring the central part of the cut surface by electron backscatter diffraction (EBSD). The measurement interval is 2 μm, and the total measurement area is 3000 μm × 3000 μm.

[0084] The non-oriented electrical steel sheet has a body-centered cubic crystal structure as its basic crystal structure, and there is a crystal orientation that is prone to magnetization under an externally applied magnetic field. The results of measuring the magnetization characteristics for different crystal orientations show that when the crystal orientation is the <001> orientation, it is the easiest to magnetize, and when the crystal orientation is the <111> orientation, it is the most difficult to magnetize. That is to say, when the grain orientation is <100> / ND relative to <111> / ND, a higher magnetic flux density can be exhibited under the same applied magnetic field.

[0085] Therefore, if there are many <111> / ND grains in the steel sheet, magnetization is not likely to occur under an externally applied magnetic field, resulting in a poor magnetic flux density and an increase in iron loss, and the required motor efficiency cannot be met. Therefore, it is preferred to minimize the <111> / ND grains as much as possible. In the present invention, the area fraction of <111> / ND grains is 20% or less. More specifically, the area fraction of <111> / ND grains can be 15% or less. The smaller the fraction, the more beneficial it is for magnetism, so the lower limit is not restricted (except 0%). More specifically, the area fraction of <111> / ND grains can be 5 to 19%. Further specifically, the area fraction of <111> / ND grains can be 10 to 15%.

[0086] The ratio of the area fraction of <100> / ND grains to the area fraction of <110> / ND grains (<100> / <110>) can be 1.01 or more.

[0087] For <110> / ND grains, although they are not as difficult to magnetize as <111> / ND grains, there is a large magnetic deviation in the rolling direction and the direction perpendicular to rolling, which is not conducive to ensuring uniform magnetism in the entire direction of the steel sheet. However, compared with <111> / ND grains, <110> / ND grains are beneficial for ensuring the magnetic flux density and low iron loss characteristics, so it is necessary to control them to an appropriate fraction.

[0088] Therefore, in order to ensure uniform magnetism in the entire direction of the steel sheet, by increasing the proportion of <100> / ND grains and decreasing the proportion of <110> / ND grains, the magnetism can be further improved, and preferably the ratio of the area fraction of <100> / ND grains to the area fraction of <110> / ND grains (<100> / <110>) is 1.01 or more. More specifically, it can be 1.04 or more. The higher this ratio, the more beneficial it is for magnetism, so the upper limit is not restricted. More specifically, it can be 1.10 to 1.9.

[0089] If there are many <100> / ND grains in the steel sheet, high magnetic flux density and low iron loss characteristics can be exhibited by externally applying a magnetic field, and the efficiency of the motor can be greatly improved. In one embodiment of the present invention, the area fraction of <100> / ND grains can be 10% or more. More specifically, the area fraction of <100> / ND grains can be 20% or more, and the more, the more beneficial to magnetism, so there is no upper limit restriction. More specifically, the area fraction of <100> / ND grains can be 20% to 50%.

[0090] In one embodiment of the present invention, grains with a specific orientation are formed, and the magnetism is uniformly excellent in the whole direction.

[0091] Specifically, the non-oriented electrical steel sheet according to one embodiment of the present invention can satisfy one or more of the following formulas 1 to 3.

[0092] [Formula 1]

[0093] (B50 L +B50 C ) / 2≥1.63

[0094] [Formula 2]

[0095] {(B50 L +B50 C+ B50 60 ) / 3} / {(B50 L +B50 C ) / 2}≥0.95

[0096] [Formula 3]

[0097] B50 60 / {(B50 L +B50 C ) / 2}≥0.90

[0098] Among them, in Formulas 1 to 3, B50 L represents the magnetic flux density (B50, Tesla) measured in the rolling direction, B50 C represents the magnetic flux density (B50, Tesla) measured in the direction perpendicular to rolling, B50 60 represents the magnetic flux density (B50, Tesla) measured in the direction at an angle of 60 degrees to the rolling direction.

[0099] B50 refers to the magnetic flux density induced under a magnetic field of 5000 A / m.

[0100] Formula 1 is basically a conventional method for evaluating the magnetic flux density of non-oriented electrical steel sheets, and represents the average value of the magnetic flux density (B50) in the rolling direction (L) and the direction perpendicular to rolling (C).

[0101] Equation 2 represents the average value of the magnetic flux density (B50) measured in the rolling direction (L) of the steel sheet, the perpendicular direction (C), and the direction at a 60-degree angle relative to the rolling direction, divided by the average value of Equation 1, indicating that not only the known rolling direction (L) and perpendicular direction (C), but also the magnetic flux density in the direction at a 60-degree angle is excellent. That is, in the present invention, since the magnetism is excellent in the entire direction of the steel sheet, a high magnetic flux density (B50 60 ) is also exhibited in the 60-degree direction where the known magnetic flux density is the worst. Therefore, according to the present invention, the ratio of the average value of the magnetic flux density (B50 60 ) including the rolling direction, perpendicular direction, and 60-degree direction to the average value of the magnetic flux density in the rolling direction and perpendicular direction of the electrical steel sheet manufactured by the known method is higher.

[0102] Equation 3 is the value obtained by dividing the magnetic flux density (B50 60 ) of the steel sheet measured in the direction at a 60-degree angle by the average value of the magnetic flux density in the rolling direction (L) and its perpendicular direction (C) of the steel sheet. Since the magnetic flux density is high in the entire direction of the steel sheet, it represents a ratio higher than the magnetic flux density (B50 60 ) in the direction at a 60-degree angle of the steel sheet manufactured by the known method to Equation 1. By the known two-step annealing and two-step rolling methods, the {100}<001> exact Cube texture and the {110}<001> Gaussian texture are developed, so that only the magnetic flux density in the rolling direction and its perpendicular direction of the steel sheet is high, but the magnetic flux density in the direction at a 60-degree angle relative to the rolling direction is very poor. Therefore, it cannot be evaluated that the magnetic properties are excellent in the entire direction of the steel sheet. As described in the present invention, by using the optimal resistivity-increasing alloying elements for increasing the area fraction of <100> / ND grains in the steel sheet, hot rolling and coiling at high temperature, and the cold rolling reduction ratio and the rapid heating technology applied in the intermediate annealing in each step, an non-oriented electrical steel sheet for drive motors can be manufactured, which has excellent magnetic flux density not only in the rolling direction and its perpendicular direction of the steel sheet, but also in the 60-degree direction of the rolling direction.

[0103] In addition, the non-oriented electrical steel sheet according to an embodiment of the present invention can satisfy the following Equation 4.

[0104] [Equation 4]

[0105] (W10 / 400 L +W10 / 400 C ) / 2≤6.885×e (2.99×t)

[0106] Wherein, in Equation 4, W10 / 400 L is the iron loss (W10 / 400, W / kg) measured in the rolling direction, and W10 / 400 CW10 / 400 is the iron loss measured in the rolling vertical direction (W10 / 400, W / kg), e is the natural constant, and t represents the thickness of the electrical steel sheet (mm).

[0107] W10 / 400 is the iron loss when exciting a magnetic flux density of 1.0 T at a frequency of 400 Hz.

[0108] Equation 4 ensures excellent magnetic flux density in the entire direction of the steel sheet according to Equations 1 to 3, so that the iron loss is also greatly reduced, and the efficiency of the motor can be improved. This iron loss characteristic is not only affected by the magnetic flux density characteristic, but also greatly affected by the thickness of the steel sheet. Therefore, according to the thickness of the steel sheet, this means the iron loss that can be ensured on the steel sheet that exhibits excellent magnetic flux density in the entire direction of the steel sheet as in the present invention.

[0109] A method for manufacturing a non-oriented electrical steel sheet according to an embodiment of the present invention includes: a step of hot rolling a slab to manufacture a hot-rolled sheet, wherein, by weight%, the slab contains Si: 2.5 to 4.0%, Al: 0.03 to 2.0%, and MN: 0.03 to 2.0%, and the balance contains Fe and unavoidable impurities; a step of pre-rolling the hot-rolled sheet at 20 to 80% to manufacture a pre-rolled sheet; an intermediate annealing step of heating and annealing the pre-rolled sheet at a heating rate of 20 °C / second or more; a step of cold rolling the pre-rolled sheet after intermediate annealing at a reduction ratio of 30 to 80% to manufacture a cold-rolled sheet; and a cold-rolled sheet annealing step of annealing the cold-rolled sheet.

[0110] The following describes each step in detail.

[0111] First, a slab is manufactured. The reasons for restricting the addition ratios of the components in the slab are the same as the reasons for restricting the components of the non-oriented electrical steel sheet described above, so the repeated description is omitted. In the following manufacturing processes such as hot rolling, hot-rolled sheet annealing, pre-rolling, first annealing, cold rolling, and second annealing, the components of the slab will not substantially change, so the components of the slab are substantially the same as the components of the non-oriented electrical steel sheet.

[0112] Before the step of manufacturing the hot-rolled sheet, the slab can be heated to above 1100 °C. Specifically, the slab is loaded into a heating furnace and heated to 1100 to 1250 °C. When heated at a temperature exceeding 1250 °C, the precipitates redissolve, and thus fine precipitation will occur after hot rolling.

[0113] The heated slab is hot-rolled to 1.5 to 4.0 mm to form a hot-rolled sheet. In an embodiment of the present invention, since there is also a pre-rolling step before cold rolling, even if the thickness of the hot-rolled sheet is relatively thick, a non-oriented electrical steel sheet with an appropriate thickness can be manufactured. More specifically, the thickness of the hot-rolled sheet can be 1.5 to 3.5 mm.

[0114] The steps of manufacturing a hot-rolled sheet may include a step of finish rolling at a temperature above 850°C.

[0115] If the hot-rolling finish rolling temperature is too low, the rolling load increases and the hot-rolling workability decreases. In addition, a lot of deformed structures remain in the hot-rolled steel sheet, which also becomes a reason for the increase in the rolling load during the subsequent process of cold rolling. Furthermore, during intermediate annealing, recrystallization of <111> / ND-oriented grains is promoted from the deformed structure, resulting in a deterioration of the magnetic flux density. Therefore, the higher the hot-rolling finish rolling temperature, the better. More specifically, it is preferably finish rolled at a temperature of 860 to 1000°C.

[0116] The steps of manufacturing a hot-rolled sheet may include a step of performing water cooling after a time of 0.1 second or more has elapsed after finish rolling.

[0117] After finish rolling, cooling is performed for coiling. When water cooling is performed, if water cooling is directly performed after finish rolling (i.e., the time is shorter than 0.1 second), as the steel sheet is rapidly cooled, the steel sheet deforms and residual stress is generated, making coiling difficult. In addition, in terms of the fine structure, the deformed stress after finish rolling remains directly without being released, which may lead to an increase in the rolling load during the subsequent cold rolling step and the recrystallization of fine <111> / ND orientation. Therefore, maintaining for 0.1 second or more after hot-rolling finish rolling enables the recovery of the hot-rolled deformed structure and recrystallization to occur, which reduces the rolling load during subsequent cold rolling and suppresses the generation of <111> / ND-oriented recrystallized grains. More specifically, water cooling can be performed after 0.3 to 5.0 seconds, and further specifically, water cooling can be performed after 0.5 to 3.0 seconds.

[0118] The steps of manufacturing a hot-rolled sheet may include a step of coiling at a temperature of 600 to 800°C. Before the finish rolling step, a rough rolling step may also be included.

[0119] If the temperature in the coiling step is controlled too low, the recovery and recrystallization of the hot-rolled deformed structure will not proceed smoothly. In order to rapidly cool the steel sheet at a low temperature, the cooling load increases, and the supercooled coiled sheet is difficult to coil. On the other hand, if the temperature is too high, although the recovery and recrystallization can be promoted, additional oxidation caused by oxygen in the atmosphere occurs during coiling, which may form a thicker scale and cause problems of grain boundary oxidation. Grain boundary oxidation of the hot-rolled sheet promotes grain boundary corrosion during the subsequent pickling process, resulting in a higher possibility of surface stripe defects and severe wear of the rolling rolls. Therefore, the coiling temperature is preferably 600 to 800°C, and more specifically, coiling can be performed at 600 to 750°C.

[0120] After manufacturing the hot-rolled sheet, it is most preferable to directly perform pickling and pre-cold rolling. However, after the step of manufacturing the hot-rolled sheet, it may further include a step of annealing the hot-rolled sheet in a temperature range of 600 to 1100 °C. If the annealing temperature of the hot-rolled sheet is too low, no recrystallized structure or fine growth will be formed, and the effect of improving the magnetic flux density is small. If the annealing temperature is too high, the magnetic properties will instead deteriorate, and due to the deformation of the sheet shape, the rolling workability will become poor. More specifically, the temperature range may be 700 to 1050 °C.

[0121] For the annealing of the hot-rolled sheet, it is carried out as needed to increase the orientation favorable for magnetism, and it may also be omitted. The annealing form is not particularly limited, and batch or continuous annealing may be adopted.

[0122] For the hot-rolled sheet after hot rolling, pickling may be carried out as needed.

[0123] Next, the hot-rolled sheet is pre-cold rolled at 20 to 80% to manufacture a pre-cold rolled sheet.

[0124] For the pre-cold rolling, it is carried out in a PCM (Pickling&Cold rolling Mill, pickling and cold rolling mill) including a pickling process or a TCM (Tandem Cold rolling Mill, tandem cold rolling mill) that only performs cold rolling to improve the rolling productivity, and it is carried out in a reduction ratio range of 20 to 80% to improve the final cold rolling productivity and the <100> / ND grain fraction in the final product sheet. At the same time, if the rolling productivity is not considered, the pre-cold rolling may also be carried out in a reversible mill in the present invention.

[0125] The pre-cold rolling is different from the following cold rolling because the pre-cold rolling is a one-time rolling step of the following process: rolling to an intermediate thickness instead of the final product thickness, then performing intermediate annealing, and then cold rolling to the final product thickness.

[0126] For the reduction ratio of the pre-cold rolling, it can be obtained by (the thickness of the steel sheet before rolling - the thickness of the steel sheet after rolling) / the thickness of the steel sheet before rolling. If the reduction ratio in the pre-cold rolling step is too low, the rolling load will increase during the final cold rolling, resulting in a decrease in productivity, and the final reduction ratio will increase, and there may be a problem of promoting the recrystallization of fine <111> / ND orientation. On the other hand, if the reduction ratio is too high, the cold rolling load will increase, and the possibility of the sheet breaking will also become high.

[0127] Therefore, the reduction ratio in the pre-cold rolling step is preferably in the range of 20 to 80%. More specifically, the lower limit of the reduction ratio may be 20%, 30%, 40%, 50%, 60%, 70% or 80%. The upper limit of the reduction ratio may be 80%, 70%, 60%, 50%, 40%, 30% or 20%.

[0128] The steps of manufacturing the pre - cold - rolled sheet can be carried out at a temperature of 60 to 300 °C. At this temperature, due to the friction between the steel sheet and the rolling rolls, the temperature of the steel sheet naturally increases, or it can be increased by external heating. If the temperature is too low, the rolling load will increase significantly, and the steel sheet will slide between the rolling rolls instead of being rolled, and problems such as distortion may occur. If the temperature is too high, oxidation of Si and Al occurs on the surface of the steel sheet, the magnetic properties will deteriorate, and problems such as ignition of the rolling oil may occur. If the temperature is too high, oxidation of Si and Al occurs on the surface of the steel sheet, the magnetic properties will deteriorate, and problems such as ignition of the rolling oil may occur. More specifically, it is preferably carried out at a temperature of 70 to 250 °C.

[0129] Next, the pre - cold - rolled sheet is heated at a heating rate of 20 °C / second or more and then intermediate annealing is carried out. In one embodiment of the present invention, recrystallization of <100> / ND orientation is promoted by a higher heating rate, and finally the magnetic properties are improved. If the heating rate is too low, recrystallization of <111> / ND orientation is promoted, and it is difficult to fully obtain the above - mentioned effects. A heating rate of 500 °C / second or more is difficult to control, and the temperature rises to a temperature higher than the target annealing temperature, making it difficult to ensure a uniform fine structure. More specifically, heating can be carried out at 30 °C / second to 500 °C / second. For the above - mentioned heating rate, it can be measured in the temperature range from the starting temperature of 100 °C to the ending temperature of 600 °C.

[0130] For the above - mentioned heating rate, it can be measured in the temperature range from the starting temperature of 100 °C to the ending temperature of 600 °C.

[0131] Intermediate annealing can be carried out in the temperature range of 600 to 1100 °C. If the annealing temperature is too low, the grain size becomes fine, the grain boundaries increase, and finally, during final cold rolling, the number of recrystallization nuclei of <111> / ND orientation at the grain boundaries increases, and finally the magnetic flux density deteriorates. On the other hand, if the annealing temperature is too high, the grains increase significantly, and due to cracks at the grain boundaries generated during final cold rolling, there may be a problem of increased sheet breakage. Preferably, annealing can be specifically carried out at 750 to 1050 °C.

[0132] After intermediate annealing, if necessary, the annealed sheet can be pickled. The pickling method is well - known, so detailed description is omitted.

[0133] Next, the cold - rolling step is to cold - roll the pre - cold - rolled sheet after intermediate annealing at a reduction ratio of 30 to 80%.

[0134] If the reduction ratio is too low, the accumulated deformation energy on the rolled steel sheet is small, and recrystallization is difficult in the subsequent annealing process, resulting in the retention of the rolling texture, and there may be problems with the improvement of magnetic flux density and iron loss. On the other hand, if the reduction ratio is too high, the recrystallization of <111> / ND-oriented grains is promoted in the subsequent annealing process, and the grains also become fine, and there may be problems with the deterioration of magnetic flux density and the increase of iron loss. More specifically, the lower limit of the reduction ratio can be 30%, 40%, 50%, 60%, 70% or 80%. The upper limit of the reduction ratio can be 80%, 70%, 60%, 50%, 40% or 30%.

[0135] Next, the step of annealing the cold-rolled sheet can anneal the cold-rolled sheet in the temperature range of 600 to 1200 °C. If the annealing temperature is too low, the recrystallization of <111> / ND-oriented grains is promoted, and the grains also become fine, making it difficult to ensure excellent magnetic flux density characteristics. If the annealing temperature is too high, the grains grow coarsely, the iron loss increases, and due to the annealing ambient gas, an oxide layer or a nitride layer is generated on the surface of the steel sheet, and there is also a problem of increased iron loss. More specifically, annealing can be carried out at 750 to 1100 °C.

[0136] After the step of annealing the cold-rolled sheet, in order to ensure the insulation and corrosion resistance of the steel sheet, a step of forming an insulating coating film may also be included. The insulating coating film is well-known, so specific descriptions are omitted.

[0137] The preferred embodiments and comparative examples of the present invention are described below. However, the following embodiments are only a preferred embodiment of the present invention, and the present invention is not limited to the following embodiments.

[0138] Example 1

[0139] Manufacture a slab having the components shown in Table 1 below. Together with the components shown in Table 1, P: 0.01%, C: 0.0020%, S: 0.0025%, N: 0.0020%, Ti: 0.0025%, Cu: 0.02%, Cr: 0.04%, Ni: 0.02% (by weight) are added, and Zn, Mo, B, Ca, Mg, Nb, V, etc. are each added in an amount of 0.002% or less, and the balance is Fe.

[0140] The slab is heated to 1150°C, hot finish rolled at 920°C, water cooled after 1 second, and coiled at 650°C to produce a hot rolled sheet. Subsequently, pickling and pre cold rolling are performed on the hot rolled sheet. For the pre cold rolling, pre cold rolling is carried out at a reduction ratio shown in Table 1 at a temperature of 85°C, heated at a heating rate shown in Table 1 below, and then subjected to intermediate annealing at 1000°C for 30 seconds. The steel sheet after intermediate annealing is finally cold rolled at a secondary reduction ratio shown in Table 1 below, thereby manufacturing a cold rolled sheet with a thickness shown in Table 1. For the final annealing, it is carried out for 60 seconds in an environment of dry hydrogen and nitrogen at 950°C.

[0141] After annealing the cold rolled sheet, for the measurement of the grain orientation of the steel sheet, it is measured by electron backscatter diffraction (EBSD), and the fractions for each orientation are shown in Table 2 below.

[0142] For the magnetic properties, Epstein specimens at different angles are prepared and measured with an Epstein tester, and the results are shown in Table 2 and Table 3 below.

[0143] [Table 1]

[0144]

[0145] [Table 2]

[0146]

[0147] [Table 3]

[0148]

[0149] As shown in Tables 1 to 3, an example of appropriately adjusting the conditions of the pre cold rolling reduction ratio, heating rate, and final cold rolling reduction ratio is that the <100> / ND fraction is higher, and the <111> / ND and <110> / ND fractions are controlled, and it can be confirmed that the magnetic properties are uniformly excellent in the entire direction.

[0150] Example 2

[0151] Hot rolling was carried out on a slab having the same composition as No. 6 shown in Table 1 of Example 1. The slab was heated to 1200 °C, and hot-rolled sheets with a thickness of 3.0 mm were manufactured by changing the hot finish rolling temperature, the holding time before water cooling after finish rolling, and the coiling temperature. The hot-rolled sheet after hot rolling was pre-cold rolled to 0.7 mm at a reduction rate of 76.7% under the temperature condition of 100 °C. Then, after heating to 950 °C at a heating rate of 50 °C / second, intermediate annealing was carried out for 10 seconds. The steel sheet after intermediate annealing was finally cold rolled to a thickness of 0.25 mm at a secondary reduction rate of 64%. For the final annealing, after heating at a rate of 100 °C / second, final annealing was carried out at 1050 °C for 20 seconds. For the analysis of the magnetic properties and grain orientation fraction of the final product, it was carried out by the same method as in Example 1 and then shown in Tables 4 and 5.

[0152] [Table 4]

[0153]

[0154] [Table 5]

[0155]

[0156] As shown in Tables 4 and 5, the final hot rolling temperature should be 850 °C or higher and held for at least 0.1 second or more after rolling, so as to promote the recovery and recrystallization of the hot-rolled structure. As a result, the <111> / ND texture fraction in the final steel sheet after cold rolling decreases, ensuring excellent magnetic flux density characteristics in the entire direction of the steel sheet. In order to ensure such a recovered and recrystallized hot-rolled structure, it can be confirmed that the coiled sheet needs to be coiled in the temperature range of 600 to 800 °C.

[0157] The present invention can be implemented in various different ways and is not limited to the above embodiments. Those of ordinary skill in the technical field to which the present invention pertains can understand that the present invention can be implemented by other specific ways without changing the technical idea or essential features of the present invention. Therefore, it should be understood that the above embodiments are exemplary in all aspects and not restrictive.

Claims

1. An non-oriented electrical steel sheet, wherein, The non-oriented electrical steel sheet contains, by weight %, Si: 2.5 to 4.0%, Al: 0.03 to 2.0%, and Mn: 0.03 to 2.0%, with the balance containing Fe and inevitable impurities. The area fraction of <111> / ND grains is 20% or less. The ratio of the area fraction of <100> / ND grains to the area fraction of <110> / ND grains is 1.01 or more. Among them, <100> / ND grains are grains in which the <100> axis of the grains lies within a range of 15 degrees or less from the vertical axis (ND) of the steel sheet surface, <111> / ND grains represent grains in which the <111> axis of the grains lies within a range of 15 degrees or less from the vertical axis (ND) of the steel sheet surface, and <110> / ND grains represent grains in which the <110> axis of the grains lies within a range of 15 degrees or less from the vertical axis (ND) of the steel sheet surface.

2. The non-oriented electrical steel sheet according to claim 1, wherein, The area fraction of <100> / ND grains is 10% or more.

3. The non-oriented electrical steel sheet according to claim 1, wherein, The non-oriented electrical steel sheet further contains one or more of Cu: 0.005 to 0.2% by weight, Cr: 0.01 to 0.5% by weight, Ni: less than 0.05% by weight and excluding 0%, and Zn: less than 0.01% by weight and excluding 0%.

4. The non-oriented electrical steel sheet according to claim 1, wherein, The non-oriented electrical steel sheet further contains one or more of P: less than 0.1% by weight and excluding 0%, C: less than 0.003% by weight and excluding 0%, S: less than 0.004% by weight and excluding 0%, Ti: less than 0.003% by weight and excluding 0%, and N: less than 0.003% by weight and excluding 0%.

5. The non-oriented electrical steel sheet according to claim 1, wherein, The non-oriented electrical steel sheet further contains one or two or more of Sn, Sb, Bi, Pb, Ge, and As, and the content of each or their total is 0.005 to 0.200% by weight.

6. The non-oriented electrical steel sheet according to claim 1, wherein, The non-oriented electrical steel sheet further contains one or more of Mo: less than 0.03% by weight and excluding 0%, B: less than 0.0050% by weight and excluding 0%, V: less than 0.0050% by weight and excluding 0%, Ca: less than 0.0050% by weight and excluding 0%, Nb: less than 0.0050% by weight and excluding 0%, and Mg: less than 0.0050% by weight and excluding 0%.

7. The non-oriented electrical steel sheet according to claim 1, wherein, The non-oriented electrical steel sheet satisfies the following formula 1. [Formula 1] (B50 L +B50 C ) / 2 ≥ 1.63 Among them, in Formula 1, B50 L represents the magnetic flux density (B50, Tesla) measured in the rolling direction, and B50 C represents the magnetic flux density (B50, Tesla) measured in the direction perpendicular to rolling.

8. The non-oriented electrical steel sheet according to claim 1, wherein, The non-oriented electrical steel sheet satisfies the following formula 2. [Formula 2] {(B50 L +B50 C+ B50 60 ) / 3} / {(B50 L +B50 C ) / 2}≥0.95 Among them, in Formula 2, B50 L represents the magnetic flux density (B50, Tesla) measured in the rolling direction, B50 C represents the magnetic flux density (B50, Tesla) measured in the direction perpendicular to rolling, B50 60 represents the magnetic flux density (B50, Tesla) measured in the direction at a 60-degree angle to the rolling direction.

9. The non-oriented electrical steel sheet according to claim 1, wherein, The non-oriented electrical steel sheet satisfies the following formula 3. [Formula 3] B50 60 / {(B50 L +B50 C ) / 2}≥0.90 Among them, in Equation 3, B50 L represents the magnetic flux density (B50, Tesla) measured in the rolling direction, B50 C represents the magnetic flux density (B50, Tesla) measured in the direction perpendicular to rolling, B50 60 represents the magnetic flux density (B50, Tesla) measured in the direction at a 60-degree angle to the rolling direction.

10. The non-oriented electrical steel sheet according to claim 1, wherein, The non-oriented electrical steel sheet satisfies the following formula 4. [Formula 4] (W10 / 400 L +W10 / 400 C ) / 2 ≤ 6.885×e (2.99×t) Among them, in Formula 4, W10 / 400 L is the iron loss measured in the rolling direction (W10 / 400, W / kg), and W10 / 400 C is the iron loss measured in the direction perpendicular to rolling (W10 / 400, W / kg), e is the natural constant, and t represents the thickness of the electrical steel sheet (mm).

11. A method for manufacturing an non-oriented electrical steel sheet, comprising: A step of hot rolling a slab to manufacture a hot rolled sheet, wherein, by weight%, the slab contains Si: 2.5 to 4.0%, Al: 0.03 to 2.0% and Mn: 0.03 to 2.0%, and the balance contains Fe and inevitable impurities; A step of pre-cold rolling the hot rolled sheet at 20 to 80% to manufacture a pre-cold rolled sheet; An intermediate annealing step of heating and annealing the pre-cold rolled sheet at a heating rate of 20°C / second or more; A step of cold rolling the pre-cold rolled sheet after intermediate annealing at a reduction rate of 30 to 80% to manufacture a cold rolled sheet; and A cold rolled sheet annealing step of annealing the cold rolled sheet.

12. The method for manufacturing an non-oriented electrical steel sheet according to claim 11, wherein, The step of manufacturing the hot-rolled sheet includes a step of finish rolling at a temperature of 850 °C or higher.

13. The method for manufacturing an non-oriented electrical steel sheet according to claim 11, wherein, The step of manufacturing the hot-rolled sheet includes a step of performing water cooling after a time of 0.1 second or more after finish rolling.

14. The method for manufacturing an non-oriented electrical steel sheet according to claim 11, wherein, The step of manufacturing the hot-rolled sheet includes a step of coiling at a temperature of 600 to 800 °C.

15. The method for manufacturing an non-oriented electrical steel sheet according to claim 11, wherein, The slab further contains one or more of Cu: 0.005 to 0.2% by weight, Cr: 0.01 to 0.5% by weight, Ni: less than 0.05% by weight and excluding 0%, and Zn: less than 0.01% by weight and excluding 0%.

16. The method for manufacturing an non-oriented electrical steel sheet according to claim 11, wherein, The slab further contains one or more of P: 0.1% by weight or less, excluding 0%, C: 0.003% by weight or less, excluding 0%, S: 0.004% by weight or less, excluding 0%, Ti: 0.003% by weight or less, excluding 0%, and N: 0.003% by weight or less, excluding 0%.

17. The method for manufacturing an non-oriented electrical steel sheet according to claim 11, wherein, The slab further contains one or two or more of Sn, Sb, Bi, Pb, Ge, and As, and the content of each or their total is 0.005 to 0.200% by weight.

18. The method for manufacturing an non-oriented electrical steel sheet according to claim 11, wherein, The slab further contains one or more of Mo: 0.03% by weight or less, excluding 0%, B: 0.0050% by weight or less, excluding 0%, V: 0.0050% by weight or less, excluding 0%, Ca: 0.0050% by weight or less, excluding 0%, Nb: 0.0050% by weight or less, excluding 0%, and Mg: 0.0050% by weight or less, excluding 0%.