Multifunctional carbon fiber lithium battery based on sulfide composite electrolyte membrane as well as preparation method and application of multifunctional carbon fiber lithium battery
By constructing a nitrogen phosphide interface layer on the surface of the sulfide electrolyte membrane and using carbon fiber braided fabric, the problem of unstable interface between the lithium metal negative electrode and the sulfide electrolyte is solved, and a carbon fiber lithium battery with high specific energy, lightweight and multifunctionality is achieved, which is suitable for a variety of high-performance energy storage occasions.
Patent Information
- Application Number
- CN202510604182.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-12
- Publication Date
- 2025-08-05
AI Technical Summary
The interface between the lithium metal negative electrode and the sulfide electrolyte is unstable, making dendrites easy to form, resulting in safety hazards. It is difficult for traditional batteries to have both structural bearing functions and cannot meet the needs of lightweight and multifunctionality.
The nitrogen phosphide electrolyte layer is combined with the sulfide electrolyte membrane, combined with carbon fiber and glass fiber braided fabric, forming a multifunctional carbon fiber lithium battery, and the nitrogen phosphide is used to generate stable phase products on the surface of the lithium negative electrode, inhibit dendrites' growth, and use carbon fiber to provide mechanical support and conductive functions.
It improves the stability of the interface between electrolyte and metal lithium, enhances the ionic conductivity and mechanical strength of the battery, realizes lightweight and versatile, and is suitable for aerospace, transportation and portable electronic devices.
Smart Images

Figure CN120432615A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium batteries and functional composite materials, and in particular to a multifunctional carbon fiber lithium battery based on a sulfide composite electrolyte membrane, and a preparation method and application thereof. Background Art
[0002] Lithium metal anodes, with their extremely high theoretical specific capacity and low electrochemical potential, are considered an important candidate anode material for next-generation high-energy-density batteries. However, the interface between lithium metal and most electrolytes is unstable, prone to dendrite formation and side reactions, which pose safety risks.
[0003] Sulfide solid electrolytes have attracted much attention due to their high room-temperature ionic conductivity and good process compatibility. However, when in direct contact with metallic lithium, they are prone to producing decomposition products and dendrite growth at the interface, seriously affecting the safety and cycle life of all-solid-state batteries. Therefore, how to improve the stability of the sulfide electrolyte-lithium interface is a key challenge that needs to be solved urgently for sulfide-based all-solid-state batteries.
[0004] On the other hand, traditional batteries are mostly used as simple energy storage devices in applications, making it difficult to combine them with structural load-bearing functions. With the increasing demand for lightweight, high specific energy, and multifunctionality, the concept of "structural energy storage" has gradually emerged. By integrating battery functions into structural support materials such as carbon fiber, the material and weight burden can be reduced and overall performance enhanced. In particular, the use of low-weight, ultra-thin fiber fabrics such as carbon fiber woven cloth and glass fiber woven cloth can achieve a reasonable ion channel design while ensuring a certain strength, combining conductivity and mechanical reinforcement, thereby obtaining an integrated multifunctional carbon fiber battery with both structural support and energy storage functions. Summary of the Invention
[0005] The purpose of the present invention is to provide a multifunctional carbon fiber lithium battery based on a sulfide composite electrolyte membrane and its preparation method and application, so as to solve the above technical problems.
[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0007] The present invention provides a multifunctional carbon fiber lithium battery based on a sulfide composite electrolyte membrane, which is composed of components including a positive electrode carbon fiber cloth, a negative electrode carbon fiber cloth, a separator and a composite sulfide electrolyte membrane;
[0008] The positive electrode carbon fiber cloth is a carbon fiber woven cloth coated with positive electrode material;
[0009] The negative electrode carbon fiber cloth is a carbon fiber woven cloth coated with a negative electrode material;
[0010] The diaphragm is a glass fiber woven cloth;
[0011] The composite sulfide electrolyte membrane has a nitrogen phosphide electrolyte layer on its surface;
[0012] The positive electrode material is a mixture of a nickel-rich ternary material, a sulfide electrolyte powder and a conductive agent, wherein the nickel-rich ternary material comprises one or more of NCM811, LiFePO4 and LiMn2O4;
[0013] The negative electrode material is a mixture of a conductive carbon material, a sulfide electrolyte powder and a conductive agent. The conductive carbon material includes one or more of soft carbon, hard carbon, a silicon-carbon composite and graphite.
[0014] Furthermore, the coating amount of the positive electrode material on the positive electrode carbon fiber cloth is 5 to 20 mg / cm 2 ;
[0015] The coating amount of the negative electrode material on the negative electrode carbon fiber cloth is 5 to 20 mg / cm 2 ;
[0016] The surface density of the glass fiber woven cloth is 5 to 30 g / m 2 ;
[0017] The surface density of the carbon fiber woven cloth is 10 to 120 g / m 2 .
[0018] Furthermore, the composite sulfide electrolyte membrane is prepared by the following steps:
[0019] Step 1) mixing sulfide electrolyte powder and a binder, ball milling the mixture, and then rolling the mixture to obtain a sulfide electrolyte layer;
[0020] Step 2) dispersing the nitrogen phosphide electrolyte in an organic solvent to obtain a spraying solution, spraying the solution on the surface of the sulfide electrolyte layer, and drying the solution to obtain a sulfide composite electrolyte membrane.
[0021] Furthermore, in step 1), the sulfide electrolyte powder is obtained by ball milling the sulfide electrolyte, and the sulfide electrolyte includes one or more of argyrodite type, lithium germanium phosphorus sulfur type, Li2S-P2S5 type and thio-LISICON type electrolyte.
[0022] Furthermore, the ball milling speed is 5 to 500 rpm, the time is 6 to 10 hours, and the ball-to-material ratio is 5 to 12:1.
[0023] Furthermore, in step 1), the mass of the binder is 0.1 to 0.5 wt% of the sulfide electrolyte powder;
[0024] The binder includes one or more of polytetrafluoroethylene, polyvinylidene fluoride and thermoplastic elastomer;
[0025] After adding the binder, ball milling is performed, the ball milling speed is 5-500 rpm, the ball-to-material ratio is 5-12:1, and the ball milling time is 0.5-2 hours.
[0026] Furthermore, in step 2), the nitrogen phosphide electrolyte includes Li 10 P4N 10 and / or Li 13 P4N 10 X3, wherein X is selected from one of Cl, Br, and F;
[0027] The organic solvent includes one or more of xylene, n-hexane and anisole;
[0028] Furthermore, in step 2), the concentration of the spraying solution is 0.1 to 0.5 mg / mL;
[0029] The thickness of the sprayed layer on the surface of the sulfide composite electrolyte membrane is 5 to 20 μm.
[0030] The present invention provides a method for preparing the above-mentioned multifunctional carbon fiber lithium battery based on sulfide composite electrolyte membrane, wherein a glass fiber woven cloth is laminated to the sulfide composite electrolyte membrane, and then laminated between the positive electrode carbon fiber cloth and the negative electrode carbon fiber cloth, and then a multifunctional carbon fiber lithium battery based on the sulfide composite electrolyte membrane is obtained by lamination and pressing or hot pressing process.
[0031] The present invention also provides an application of a multifunctional carbon fiber lithium battery based on a sulfide composite electrolyte membrane in aerospace, transportation or portable electronic devices.
[0032] Beneficial effects of the present invention:
[0033] 1) Improved interface stability:
[0034] Since nitrogen phosphide or its halogen-doped derivatives can decompose in situ at the potential of the metallic lithium negative electrode to generate stable phase products such as Li3N, Li3P, LiF, LiCl, and LiBr, a uniform SEI layer that is conducive to ion conduction is formed, which effectively inhibits dendrite growth.
[0035] 2) High ionic conductivity of composite electrolyte membrane:
[0036] By combining sulfide electrolyte with nitrogen phosphide electrolyte, the high ionic conductivity of sulfide and the high chemical stability and good interface affinity of nitrogen phosphide are taken into consideration, so that the electrolyte membrane can obtain 4.2×10 -4 ~6.5×10 -3 S / cm ionic conductivity.
[0037] 3) Lightweight multifunctional structural battery:
[0038] Using carbon fiber woven cloth and glass fiber woven cloth as composite reinforcement inside the battery can simultaneously give the battery mechanical support and conductive (or isolation) functions, realizing a multifunctional carbon fiber lithium battery with integrated structural energy storage and excellent specific energy and specific strength.
[0039] 4) Wide applicability:
[0040] The technical concept of the present invention can be extended to a variety of nitrogen phosphide derivatives or other stability-modified materials, and is also compatible with different sulfide electrolyte systems. It is also applicable to other structural components such as lithium cobalt oxide, lithium iron phosphate and other positive electrode materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Figure 1 Schematic diagram of the preparation of the sulfide composite electrolyte membrane of the present invention;
[0042] Figure 2 This is a comparison chart of the ionic conductivity of the composite electrolyte membrane after using different nitrogen phosphide spray layers in the present invention. DETAILED DESCRIPTION
[0043] The present invention provides a multifunctional carbon fiber lithium battery based on a sulfide composite electrolyte membrane, which is composed of components including a positive electrode carbon fiber cloth, a negative electrode carbon fiber cloth, a separator and a composite sulfide electrolyte membrane;
[0044] The positive electrode carbon fiber cloth is a carbon fiber woven cloth coated with positive electrode material;
[0045] The negative electrode carbon fiber cloth is a carbon fiber woven cloth coated with a negative electrode material;
[0046] The diaphragm is a glass fiber woven cloth;
[0047] The composite sulfide electrolyte membrane has a nitrogen phosphide electrolyte layer on its surface;
[0048] The positive electrode material is a mixture of a nickel-rich ternary material, a sulfide electrolyte powder and a conductive agent, wherein the nickel-rich ternary material comprises one or more of NCM811, LiFePO4 and LiMn2O4;
[0049] The negative electrode material is a mixture of a conductive carbon material, a sulfide electrolyte powder and a conductive agent. The conductive carbon material includes one or more of soft carbon, hard carbon, a silicon-carbon composite and graphite.
[0050] In the present invention, the nickel-rich ternary material is preferably NCM811 and / or LiFePO4, and more preferably NCM811 and LiFePO4.
[0051] In the present invention, the conductive carbon material preferably includes one or more of soft carbon, silicon-carbon composite and graphite, and more preferably is a mixture of soft carbon, silicon-carbon composite and graphite.
[0052] In the present invention, the coating amount of the positive electrode material on the positive electrode carbon fiber cloth is 5 to 20 mg / cm 2 , preferably 10 to 15 mg / cm 2 ;
[0053] The coating amount of the negative electrode material on the negative electrode carbon fiber cloth is 5 to 20 mg / cm 2 , preferably 8 to 12 mg / cm 2 ;
[0054] The surface density of the glass fiber woven cloth is 5 to 30 g / m 2 , preferably 8 to 25 g / m 2 , more preferably 10 to 20 g / m 2 ;
[0055] The surface density of the carbon fiber woven cloth is 10 to 120 g / m 2 . Preferably 20 to 100 g / m 2 , more preferably 25 to 50 g / m 2 .
[0056] In the present invention, the composite sulfide electrolyte membrane is prepared by the following steps:
[0057] Step 1) mixing sulfide electrolyte powder and a binder, ball milling the mixture, and then rolling the mixture to obtain a sulfide electrolyte layer;
[0058] Step 2) dispersing the nitrogen phosphide electrolyte in an organic solvent to obtain a spraying solution, spraying the solution on the surface of the sulfide electrolyte layer, and drying the solution to obtain a sulfide composite electrolyte membrane.
[0059] In the present invention, in step 1), the sulfide electrolyte powder is obtained by ball milling the sulfide electrolyte, and the sulfide electrolyte includes one or more of argyrodite type, lithium germanium phosphorus sulfur type, Li2S-P2S5 type and thio-LISICON type electrolyte, preferably one or more of lithium germanium phosphorus sulfur type, Li2S-P2S5 type, thio-LISICON type electrolyte, and further preferably Li6PS5Cl, Li6PS5Br or Li7P3S 11 .
[0060] In the present invention, the rotation speed of the ball mill is 5 to 500 rpm, preferably 15 to 300 rpm, and more preferably 30 to 200 rpm;
[0061] The ball milling time is 6 to 10 hours, preferably 8 hours;
[0062] The ball-to-material ratio of the ball mill is 5 to 12:1, preferably 7 to 10:1, and more preferably 8:1.
[0063] In the present invention, in step 1), the mass of the binder is 0.1 to 0.5 wt% of the sulfide electrolyte powder, preferably 0.3 wt%;
[0064] The binder comprises one or more of polytetrafluoroethylene, polyvinylidene fluoride and thermoplastic elastomer, preferably polytetrafluoroethylene, polyvinylidene fluoride or thermoplastic elastomer, more preferably polytetrafluoroethylene;
[0065] After adding the binder, ball milling is performed, the ball milling speed is 5-500rpm, preferably 15-300rpm, and more preferably 30-200rpm; the ball-to-material ratio is 5-12:1, preferably 7-10:1, and more preferably 8:1; the ball milling time is 0.5-2h, preferably 0.8-1.5h, and more preferably 1.2h.
[0066] In the present invention, in step 2), the nitrogen phosphide electrolyte includes Li 10 P4N 10 and / or Li 13 P4N 10 X3, preferably Li 10 P4N 10 He Li 13 P4N 10 X3;
[0067] In the present invention, when the nitrogen phosphide electrolyte contains Li 13 P4N 10 When X3, X is selected from one of Cl, Br, and F, preferably Cl or Br, more preferably Cl;
[0068] The organic solvent comprises one or more of xylene, n-hexane and anisole, preferably xylene and / or n-hexane, more preferably xylene and n-hexane;
[0069] In the present invention, in step 2), the concentration of the spraying solution is 0.1 to 0.5 mg / mL, preferably 0.2 to 0.4 mg / mL, and more preferably 0.3 mg / mL;
[0070] The thickness of the sprayed layer on the surface of the sulfide composite electrolyte membrane is 5 to 20 μm, preferably 10 to 18 μm, and more preferably 15 μm;
[0071] In the present invention, the thickness of the sulfide composite electrolyte membrane is 50 to 150 μm, preferably 80 to 120 μm, and more preferably 100 μm.
[0072] In the present invention, the spraying is performed under an inert atmosphere to prevent the material from being affected by moisture or oxidation.
[0073] In the present invention, the sprayed sulfide composite electrolyte membrane is dried to allow the nitrogen phosphide electrolyte layer to be tightly bonded to the surface of the sulfide electrolyte membrane and to remove the solvent.
[0074] In the present invention, the drying temperature is 60-80° C., preferably 70° C., and the drying time is 10-24 h, preferably 15-20 h, and more preferably 18 h.
[0075] The present invention provides a method for preparing the above-mentioned multifunctional carbon fiber lithium battery based on sulfide composite electrolyte membrane, wherein a glass fiber woven cloth is laminated to the sulfide composite electrolyte membrane, and then laminated between the positive electrode carbon fiber cloth and the negative electrode carbon fiber cloth, and then a multifunctional carbon fiber lithium battery based on the sulfide composite electrolyte membrane is obtained by lamination and pressing or hot pressing process.
[0076] In the present invention, as a preferred embodiment, one side of the negative electrode first contacts the nitrogen phosphide spray layer.
[0077] The present invention also provides an application of a multifunctional carbon fiber lithium battery based on a sulfide composite electrolyte membrane in aerospace, transportation or portable electronic devices.
[0078] The technical solutions provided by the present invention are described in detail below with reference to the embodiments, but they should not be construed as limiting the scope of protection of the present invention.
[0079] Example 1
[0080] 5000 mg of Li6PS5Cl sulfide electrolyte was placed in a zirconia ball mill and ball-milled at a ball-to-material ratio of 10:1 and a rotation speed of 400 rpm in an argon atmosphere for 8 h. The sulfide electrolyte powder was then mixed with 5 mg of polytetrafluoroethylene and ball-milled for another 1 h. The mixture was then rolled into a sulfide electrolyte membrane with a thickness of 100 μm in an inert atmosphere glove box.
[0081] Weigh 10 mg of Li 10 P4N 10 Dispersed in 50 mL of xylene, it was sprayed onto the sulfide electrolyte membrane using a spraying process to make the thickness of the nitrogen phosphide electrolyte layer 10 μm, and then dried at 80°C for 8 hours to obtain a composite sulfide electrolyte membrane;
[0082] The positive electrode material was prepared according to the mass ratio of NCM811, Li6PS5Cl and conductive carbon black of 55:40:5, and 15 mg / cm of positive electrode material was taken. 2 Coated on a surface density of 25g / m 2 The positive electrode carbon fiber cloth was obtained after drying; the negative electrode material was prepared according to the mass ratio of soft carbon, Li6PS5Cl and conductive carbon black of 55:40:5, and 15mg / cm 2 The negative electrode material is coated on a surface with a density of 25g / m 2 The negative electrode carbon fiber cloth is obtained after drying on the ultra-thin carbon fiber woven cloth;
[0083] With a surface density of 10g / m 2 The low-weight ultra-thin glass fiber woven cloth is used as the separator, and the positive electrode carbon fiber cloth, composite sulfide electrolyte membrane (nitrogen phosphide electrolyte layer facing the negative electrode side), glass fiber woven cloth and negative electrode carbon fiber cloth are stacked in sequence and pressurized to assemble into a battery.
[0084] 1. Test method for ionic conductivity of electrolyte membrane
[0085] The ionic conductivity of the electrolyte membrane can be measured by electrochemical impedance spectroscopy (EIS). The specific method is as follows:
[0086] Sample preparation: The prepared sulfide composite electrolyte membrane was cut into circular pieces with a diameter of 10 mm.
[0087] Test equipment: Use an electrochemical workstation (such as BioLogic VSP-300, Autolab PGSTAT, etc.) and an impedance analysis system with stainless steel or aluminum electrodes.
[0088] Test conditions: The electrolyte membrane is placed between stainless steel electrodes, and an AC signal with a frequency range of 0.1 Hz to 7 MHz and a disturbance voltage of 10 mV is used.
[0089] Test steps:
[0090] The tests were carried out at room temperature (25 °C), electrochemical impedance spectroscopy (EIS) was used for measurement, and the ionic conductivity was calculated based on the Nyquist plot (the relationship between the real and imaginary impedances).
[0091] 2. Charge and discharge performance test method
[0092] Battery testing equipment: Use a battery tester (such as Arbin Instruments, LAND, etc.) to perform constant current charge and discharge tests.
[0093] Test conditions:
[0094] The charge and discharge current is set to 0.5C (where C is the theoretical capacity of the battery, in mAh / g), that is, the charge and discharge current per hour is 50% of the battery capacity.
[0095] The charge cut-off voltage is set to 4.3V and the discharge cut-off voltage is set to 2.8V.
[0096] The test temperature is 25℃.
[0097] Test steps:
[0098] The charge and discharge tests were carried out at room temperature, with constant current charging during the charging process and constant current discharging during the discharging process.
[0099] Record the voltage, current, capacity and time of each cycle of the battery during the charge and discharge process.
[0100] For each test cycle, the charge and discharge curves were recorded and the discharge capacity of each cycle was calculated.
[0101] Data recording: The capacity retention rate is calculated after 100 cycles. In addition, the charge and discharge curves and efficiency are recorded to calculate the first discharge efficiency.
[0102] 3. Cyclic performance test method
[0103] Cycle test equipment: Also use a battery tester to perform constant current charge and discharge tests.
[0104] Test conditions:
[0105] The battery charge and discharge rate is set to 0.5C, that is, the charge and discharge current per hour is 50% of the battery capacity.
[0106] The number of cycles is 100, the charge cut-off voltage is 4.3V, and the discharge cut-off voltage is 2.8V.
[0107] The test temperature was 25°C and the cycles were performed at room temperature.
[0108] Test steps:
[0109] The battery was subjected to 100 charge and discharge cycles.
[0110] Record the charge and discharge process of each cycle, including current, voltage, capacity and time.
[0111] The capacity was measured after every 10 cycles, and the capacity retention and Coulombic efficiency were calculated.
[0112] Monitor battery voltage fluctuations during cycling, especially polarization and voltage decay during battery charge and discharge.
[0113] Data Records:
[0114] Cycle performance curve: records the relationship between the battery's charge and discharge capacity and the number of cycles, and evaluates its capacity retention rate.
[0115] The capacity retention after 100 cycles was recorded.
[0116] The multifunctional carbon fiber lithium battery based on the sulfide composite electrolyte membrane obtained in Example 1 was subjected to constant current charge and discharge tests at room temperature. The initial capacity was 152 mAh / g, and the capacity retention rate reached 92.5% after 100 cycles. The coulombic efficiency was >99%. The ionic conductivity of the sulfide composite electrolyte membrane at room temperature was 4.2×10 -3 S / cm.
[0117] Example 2
[0118] 4000 mg of Li7P3S 11 The Cl sulfide electrolyte was placed in a zirconia ball mill and ball-milled for 8 h at a ball-to-material ratio of 10:1 and a rotation speed of 350 rpm in an argon atmosphere. The sulfide electrolyte powder was then mixed with 8 mg of polyvinylidene fluoride and ball-milled for another 1 h. The mixture was then rolled into a sulfide electrolyte membrane with a thickness of 70 μm in an inert atmosphere glove box.
[0119] Weigh 10 mg of Li 13 P4N 10 Cl3 was dispersed in 60 mL of n-hexane and sprayed onto the sulfide electrolyte membrane using a spraying process to make the thickness of the nitrogen phosphide electrolyte layer 5 μm. The membrane was then dried at 70°C for 10 h to obtain a composite sulfide electrolyte membrane.
[0120] According to LiFePO4, Li7P3S 11 The mass ratio of conductive carbon fiber to positive electrode material is 50:45:5, and the positive electrode material is 8 mg / cm 2 Coated on a surface density of 25g / m 2 The ultra-thin carbon fiber woven cloth is dried to obtain the positive electrode carbon fiber cloth; according to the silicon-carbon composite material, Li7P3S 11 The mass ratio of conductive carbon black to negative electrode material is 55:40:5, and 8mg / cm 2 The negative electrode material is coated on a surface with a density of 25g / m 2 The negative electrode carbon fiber cloth is obtained after drying on the ultra-thin carbon fiber woven cloth;
[0121] With a surface density of 8g / m 2The low-weight ultra-thin glass fiber woven cloth is used as the separator, and the positive electrode carbon fiber cloth, composite sulfide electrolyte membrane (nitrogen phosphide electrolyte layer facing the negative electrode side), glass fiber woven cloth and negative electrode carbon fiber cloth are stacked in sequence and pressurized to assemble into a battery.
[0122] At room temperature, the multifunctional carbon fiber lithium battery based on the sulfide composite electrolyte membrane obtained in Example 2 was subjected to constant current charge and discharge tests at a rate of 0.2C. The initial capacity was 144 mAh / g, and the capacity retention rate reached 90% after 150 cycles. The interface impedance increased relatively slowly.
[0123] Example 3
[0124] 5000 mg of Li6PS5Br sulfide electrolyte was placed in a zirconia ball mill and ball-milled at a ball-to-material ratio of 8:1 and a rotation speed of 400 rpm in an argon atmosphere for 6 h. The sulfide electrolyte powder was then mixed with 5 mg of polytetrafluoroethylene and ball-milled for another 1 h. The mixture was then rolled into a sulfide electrolyte membrane with a thickness of 120 μm in an inert atmosphere glove box.
[0125] Weigh 15 mg of Li 13 P4N 10 F3 was ultrasonically dispersed in 70 mL of anisole and sprayed onto the sulfide electrolyte membrane using a spraying process to make the thickness of the nitrogen phosphide electrolyte layer 20 μm. It was then dried at 90°C for 6 h to obtain a composite sulfide electrolyte membrane.
[0126] The positive electrode material was prepared according to the mass ratio of NCM811, Li6PS5Br and carbon black conductive agent of 60:35:5, and the positive electrode material was 18 mg / cm 2 Coated on a surface density of 25g / m 2 The positive electrode carbon fiber cloth was obtained after drying; the negative electrode material was prepared according to the mass ratio of soft carbon, Li6PS5Br and acetylene black of 50:45:5, and 18mg / cm 2 The negative electrode material is coated on a surface with a density of 25g / m 2 The negative electrode carbon fiber cloth is obtained after drying on the ultra-thin carbon fiber woven cloth;
[0127] With a surface density of 12g / m 2 The low-weight ultra-thin glass fiber woven cloth is used as the separator, and the positive electrode carbon fiber cloth, composite sulfide electrolyte membrane (nitrogen phosphide electrolyte layer facing the negative electrode side), glass fiber woven cloth and negative electrode carbon fiber cloth are stacked in sequence and pressurized to assemble into a battery.
[0128] At room temperature, the room temperature ionic conductivity of the sulfide composite electrolyte membrane obtained in Example 3 reached 6.5×10 -3S / cm, and the limiting current density is about 0.7 mA / cm 2 , the capacity retention rate is still higher than 95% after 50 cycles.
[0129] Example 4
[0130] 4500 mg of Li6PS5Cl, 500 mg of Li 10 P4N 10 The sulfide electrolyte was placed in a zirconia ball mill and ball-milled for 10 h in an argon atmosphere at a ball-to-material ratio of 5:1 and a rotation speed of 400 rpm. The sulfide electrolyte powder was then mixed with 10 mg of polytetrafluoroethylene and ball-milled for another 1 h. The mixture was then rolled into a sulfide electrolyte membrane with a thickness of 80 μm in an inert atmosphere glove box.
[0131] The positive electrode material is prepared according to the mass ratio of NCM811, sulfide electrolyte and conductive carbon black of 55:40:5, and the positive electrode material is 12 mg / cm 2 Coated on a surface density of 25g / m 2 The positive electrode carbon fiber cloth was obtained after drying; the negative electrode material was prepared according to the mass ratio of hard carbon, sulfide electrolyte and conductive carbon black of 55:40:5, and 12 mg / cm 2 The negative electrode material is coated on a surface with a density of 25g / m 2 The negative electrode carbon fiber cloth is obtained after drying on the ultra-thin carbon fiber woven cloth;
[0132] With a surface density of 10g / m 2 The low-weight ultra-thin glass fiber woven cloth is used as the separator, and the positive electrode carbon fiber cloth, sulfide electrolyte membrane (nitrogen phosphide electrolyte layer faces the negative electrode side), glass fiber woven cloth and negative electrode carbon fiber cloth are stacked in sequence and pressurized to assemble into a battery.
[0133] At room temperature, the multifunctional carbon fiber lithium battery based on the sulfide composite electrolyte membrane obtained in Example 4 has an initial capacity of 145 mAh / g, a capacity retention rate of 91.2% after 200 cycles, and small polarization.
[0134] Example 5
[0135] A total mass of 6000 mg of a Li2S-P2S5 system with a molar ratio of 70:30 was taken and ball milled at a ball-to-material ratio of 12:1 and a rotation speed of 450 rpm under an argon atmosphere for 9 hours. After adding 18 mg of polyvinylidene fluoride, the ball milling was continued for 1 hour. The mixture was then roller-pressed into a sulfide electrolyte membrane with a thickness of 100 μm in an inert atmosphere glove box.
[0136] Weigh 10 mg of Li 13 P4N 10F3 and 5 mg of LiF were mixed and dispersed in 80 mL of anisole to obtain a mixed spray solution. This solution was then sprayed onto the sulfide electrolyte membrane to a thickness of 15 μm. The membrane was then dried at 90°C for 10 h to obtain a composite surface with both fluoride and nitride characteristics.
[0137] The positive electrode material is prepared according to the mass ratio of LiMn2O4, Li2S-P2S5 and carbon black of 60:35:5, and the positive electrode material is 10 mg / cm 2 Coated on a surface density of 25g / m 2 The positive electrode carbon fiber cloth was obtained after drying; the negative electrode material was prepared according to the mass ratio of hard carbon, Li2S-P2S5 and conductive carbon black of 50:45:5, and 10mg / cm 2 The negative electrode material is coated on a surface with a density of 25g / m 2 The negative electrode carbon fiber cloth is obtained after drying on the ultra-thin carbon fiber woven cloth;
[0138] With a surface density of 8g / m 2 The low-weight ultra-thin glass fiber woven cloth is used as the separator, and the positive electrode carbon fiber cloth, composite sulfide electrolyte membrane (nitrogen phosphide electrolyte layer facing the negative electrode side), glass fiber woven cloth and negative electrode carbon fiber cloth are stacked in sequence and pressurized to assemble into a battery.
[0139] The sulfide composite electrolyte membrane obtained in Example 5 was tested at room temperature, and its ionic conductivity at room temperature was about 5.2×10 -3 S / cm, and the capacity retention rate of the obtained battery reached about 93.5% after 100 cycles at a charge and discharge rate of 0.5C.
[0140] It can be seen from the above embodiments that the present invention provides a multifunctional carbon fiber lithium battery based on a sulfide composite electrolyte membrane, and a preparation method and application thereof.
[0141] Figure 1 Schematic diagram of the preparation of the sulfide composite electrolyte membrane in the present invention, Figure 2 This is a comparison chart of the ionic conductivity of the composite electrolyte membrane after using different nitrogen phosphide spray layers in the present invention.
[0142] As can be seen from the figure, the ionic conductivity of the composite electrolyte membranes prepared in Examples 1 to 5 at room temperature (25°C) is 4.2×10 -3 ~6.5×10 -3 The S / cm values vary slightly depending on the nitrogen phosphide content and the type of halogen doping. Nitrogen phosphide derivatives or their mixtures can in-situ form Li3N, Li3P, LiF, LiCl, and other components on the lithium anode side, helping to further reduce interfacial impedance.
[0143] The prepared composite electrolyte membrane was sandwiched between lithium metal symmetrical electrodes to conduct limiting current density tests. The composite electrolyte membranes prepared in Examples 1 to 5 reached a limiting current density of 0.7 to 0.9 mA / cm 2 The current can flow without any obvious short circuit or excessive polarization.
[0144] The carbon fiber batteries of Examples 1 to 5 were subjected to long-term cycling at room temperature. Examples 1 and 3 exhibited excellent cycling stability using the NCM811 system, with capacity retention exceeding 90% after 100 cycles. Good cycling performance was also achieved using the LiMn2O4 positive electrode in Example 5.
[0145] Because carbon fiber woven fabric and glass fiber woven fabric work together to strengthen and support the battery, they can reduce the current collector and housing requirements in the battery system to a certain extent, thereby achieving lightweighting. The carbon fiber network also provides additional conductive paths and mechanical support, maintaining structural stability during battery deformation.
[0146] In summary, the present invention optimizes the interface between sulfide electrolyte and nitrogen phosphide electrolyte, combines carbon fiber woven cloth and glass fiber woven cloth, and successfully prepares an integrated multifunctional carbon fiber lithium battery with high ionic conductivity, high interface stability and mechanical reinforcement. The present invention improves the interface stability between sulfide electrolyte and metallic lithium, inhibits the formation of lithium dendrites; provides a composite electrolyte-carbon fiber integrated battery that can have both structural support and energy storage functions, achieving lightweight and high safety; the present invention improves the comprehensive performance of the electrolyte (including ionic conductivity, stability, processability, etc.) by combining nitrogen phosphide electrolyte or its halogen-doped derivatives with sulfide electrolyte, and can be further extended to other similar material systems. The present invention is of great significance.
[0147] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A multifunctional carbon fiber lithium battery based on a sulfide composite electrolyte membrane, characterized in that: It is composed of components including positive electrode carbon fiber cloth, negative electrode carbon fiber cloth, separator and composite sulfide electrolyte membrane; The positive electrode carbon fiber cloth is a carbon fiber woven cloth coated with positive electrode material; The negative electrode carbon fiber cloth is a carbon fiber woven cloth coated with a negative electrode material; The diaphragm is a glass fiber woven cloth; The composite sulfide electrolyte membrane has a nitrogen phosphide electrolyte layer on its surface; The positive electrode material is a mixture of a nickel-rich ternary material, a sulfide electrolyte powder and a conductive agent, wherein the nickel-rich ternary material comprises one or more of NCM811, LiFePO4 and LiMn2O4; The negative electrode material is a mixture of a conductive carbon material, a sulfide electrolyte powder and a conductive agent. The conductive carbon material includes one or more of soft carbon, hard carbon, a silicon-carbon composite and graphite.
2. A multifunctional carbon fiber lithium battery based on a sulfide composite electrolyte membrane according to claim 1, characterized in that: The coating amount of the positive electrode material on the positive electrode carbon fiber cloth is 5 to 20 mg / cm 2 ; The coating amount of the negative electrode material on the negative electrode carbon fiber cloth is 5 to 20 mg / cm 2 ; The surface density of the glass fiber woven cloth is 5 to 30 g / m 2 ; The surface density of the carbon fiber woven cloth is 10 to 120 g / m 2 .
3. A multifunctional carbon fiber lithium battery based on a sulfide composite electrolyte membrane according to claim 2, characterized in that: The composite sulfide electrolyte membrane is prepared by the following steps: Step 1) mixing sulfide electrolyte powder and a binder, ball milling the mixture, and then rolling the mixture to obtain a sulfide electrolyte layer; Step 2) dispersing the nitrogen phosphide electrolyte in an organic solvent to obtain a spraying solution, spraying the solution on the surface of the sulfide electrolyte layer, and drying the solution to obtain a sulfide composite electrolyte membrane.
4. A multifunctional carbon fiber lithium battery based on a sulfide composite electrolyte membrane according to claim 3, characterized in that: In step 1), the sulfide electrolyte powder is obtained by ball milling the sulfide electrolyte, and the sulfide electrolyte includes one or more of argyrodite type, lithium germanium phosphorus sulfur type, Li2S-P2S5 type and thio-LISICON type electrolyte.
5. The multifunctional carbon fiber lithium battery based on sulfide composite electrolyte membrane according to claim 4, characterized in that: The ball milling speed is 5-500 rpm, the time is 6-10 hours, and the ball-to-material ratio is 5-12:
1.
6. A multifunctional carbon fiber lithium battery based on a sulfide composite electrolyte membrane according to claim 3 or 4, characterized in that: In step 1), the mass of the binder is 0.1 to 0.5 wt% of the sulfide electrolyte powder; The binder includes one or more of polytetrafluoroethylene, polyvinylidene fluoride and thermoplastic elastomer; After adding the binder, ball milling is performed, the ball milling speed is 5-500 rpm, the ball-to-material ratio is 5-12:1, and the ball milling time is 0.5-2 hours.
7. The multifunctional carbon fiber lithium battery based on sulfide composite electrolyte membrane according to claim 3, characterized in that: In step 2), the nitrogen phosphide electrolyte includes Li 10 P4N 10 and / or Li 13 P4N 10 X3, wherein X is selected from one of Cl, Br, and F; The organic solvent includes one or more of xylene, n-hexane and anisole.
8. A multifunctional carbon fiber lithium battery based on a sulfide composite electrolyte membrane according to claim 3 or 7, characterized in that: In step 2), the concentration of the spraying solution is 0.1 to 0.5 mg / mL; The thickness of the sprayed layer on the surface of the sulfide composite electrolyte membrane is 5 to 20 μm.
9. The method for preparing a multifunctional carbon fiber lithium battery based on a sulfide composite electrolyte membrane according to any one of claims 1 to 8, characterized in that: The glass fiber woven cloth is laminated to the sulfide composite electrolyte membrane, and then laminated between the positive electrode carbon fiber cloth and the negative electrode carbon fiber cloth. After that, a multifunctional carbon fiber lithium battery based on the sulfide composite electrolyte membrane is obtained through a lamination pressurization or hot pressing process.
10. Use of a multifunctional carbon fiber lithium battery based on a sulfide composite electrolyte membrane according to any one of claims 1 to 8 in aerospace, transportation or portable electronic devices.
Citation Information
Cited By
Composite solid electrolyte diaphragm, preparation method and all-solid-state battery
CN121054967A
Composite solid electrolyte separator, method of preparation and all-solid-state battery
CN121054967B