Method for improving metal punching efficiency through fusion splashing by using combined laser

By combining laser technology, the delayed output pulse laser spray is used to remove the melt after continuous laser pre-damage, which solves the problem of low efficiency in existing laser hole drilling technology and achieves an efficient and tool-free metal hole drilling effect.

CN120480443APending Publication Date: 2025-08-15NANJING UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510665255.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-22
Publication Date
2025-08-15

AI Technical Summary

Technical Problem

The existing laser hole drilling technology has problems such as low energy conversion efficiency, molten materials hinder further penetration, and long processing time when processing metals. It is especially difficult to efficiently form holes on thick metal sheets.

Method used

Using combined laser technology, pulsed laser is output by delayed output after continuous laser pre-damage, and the melt is sputtered by pulsed laser, and laser parameters are controlled in combination with the delay device to improve the removal rate and hole drilling efficiency of the melt.

Benefits of technology

It realizes efficient hole drilling without tool loss, improves metal hole drilling rate and quality, enhances laser ablation effect, and is suitable for processing under complex working conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120480443A_ABST
    Figure CN120480443A_ABST
Patent Text Reader

Abstract

The invention discloses a method for improving metal punching efficiency through fusion splashing by using combined laser, which comprises the following steps of: focusing continuous laser and millisecond pulse laser at one point on the surface of a metal material in an atmospheric environment; and single millisecond pulse laser is added at the end of continuous laser irradiation to evaporate the molten material or remove the molten material through back-flushing pressure splashing, so that the removal rate of the material is increased. The energy utilization rate and the machining efficiency are improved, the area of a recasting layer is greatly reduced, and the method is suitable for machining thick metal plates.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of laser processing and damage to metals, and in particular relates to a method for improving metal drilling efficiency through melt splashing by combining lasers. Background Art

[0002] With the globalization of manufacturing and fierce market competition, traditional metal component manufacturing methods often suffer from multiple steps, poor quality, high costs, low efficiency, and severe pollution, making them unable to meet the demands of rapidly responding to market demands for new products. The widespread adoption of laser processing methods in industry can significantly increase productivity, reduce production costs, improve product quality, and reduce environmental pollution. Laser processing has developed a variety of applications, among which laser drilling uses a laser beam to irradiate a material surface, heating and melting or vaporizing a localized area, thereby forming high-precision, high-quality holes. Laser drilling has become a key research technology for cutting-edge products in industries such as aviation, aerospace, machinery, optoelectronics, instrumentation, and metering. For example, parts such as turbine engine blades, gas turbine blades, and printed circuit boards require hundreds of holes to be machined. When perforating large targets, even when the beam energy deposited on the target reaches a certain level, continuous irradiation for several seconds is required to achieve effective perforation. To address the inherent limitations of continuous lasers, such as limited energy conversion efficiency and insufficient peak power output, combined laser irradiation technology has been proposed as a novel energy coupling solution. This technology achieves the synergistic effect of heat accumulation effect and transient impact effect by timing-controlled operation of different lasers and metals, breaking through the energy efficiency bottleneck of traditional single irradiation mode.

[0003] Combined lasers offer certain advantages in perforation. During the laser drilling process, the molten material from the continuous laser accumulates in the pits formed by the initial interaction, hindering further penetration. Some of the energy absorbed by the target material is not effectively used for perforation, and a longer exposure time is required to damage the metal. The molten material can be removed by evaporation caused by the pulsed laser or by splashing due to recoil pressure. Combining the two can achieve better damage effects under the same continuous and pulsed laser conditions, and can also achieve the same damage targets as using only one laser at a time using lower continuous laser power and pulsed laser energy. Summary of the Invention

[0004] The present invention aims to provide a method for improving the efficiency of metal drilling by combining laser with melt splashing, thereby increasing the removal rate of the melt during the laser drilling process.

[0005] To achieve the object of the present invention, the present invention provides a method for improving metal drilling efficiency by combined laser melting and sputtering, comprising the following steps:

[0006] Step 1: irradiate the metal material with a parallel beam formed by a continuous laser through an optical lens group, so that the parallel beam interacts with the metal material and causes pre-damage;

[0007] Step 2: Using a delay device to cause the pulsed laser to emit light after the continuous laser causes the pre-damage, and controlling the delay time of the two, so that a pulsed laser can be accurately emitted to form a parallel beam through the optical lens group to irradiate the surface of the metal material and drill a hole at the same location as the pre-damage;

[0008] Step 3: The continuous laser and the pulse laser stop emitting light at the same time, obtaining a blind hole or a through hole, and completing the drilling.

[0009] Furthermore, the metal material is one of aluminum alloy, titanium alloy and pure copper.

[0010] Furthermore, the wavelength of the continuous laser is 1064 nm.

[0011] Furthermore, the pulse width of the pulse laser is 10 ms.

[0012] Furthermore, the spot radius of the continuous laser is 5 mm, and the spot radius of the pulsed laser is 1 mm.

[0013] Furthermore, the delayed light emission time of the two in step 2 is 2s-4s.

[0014] Furthermore, the power density of the continuous laser and the energy density of the pulsed laser are both greater than the melting threshold of the metal material.

[0015] Furthermore, the spot centers of the continuous laser and the pulse laser coincide with a point on the metal material.

[0016] Furthermore, the optical lens group includes a first optical lens L1 and a second optical lens L2.

[0017] Compared with the prior art, the significant improvements of the present invention are: (1) the present invention is contactless processing, without tool wear, avoiding the problem of drill bit breakage during mechanical drilling, and can be processed in complex working conditions; (2) the present invention can remove the melt generated by continuous laser by pulse laser, thereby increasing the laser drilling rate; (3) the present invention improves the drilling quality by controlling parameters such as laser power and pulse width; (4) the present invention enhances the laser ablation drilling effect by combining the mechanical effects generated during the laser ablation process to peel off the target material below the melting point.

[0018] In order to more clearly illustrate the functional characteristics and structural parameters of the present invention, further description is given below with reference to the accompanying drawings and specific embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] The drawings described herein are used to provide a further understanding of the present invention and constitute a part of this application. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:

[0020] Figure 1 This is a schematic diagram of an experiment of punching a hole in a metal plate by combined laser irradiation according to the present invention;

[0021] Figure 2 The experimental results of the continuous laser and millisecond pulse laser acting on aluminum alloy are shown in the figure; (a) is the damage image of aluminum alloy after continuous laser acting on it for 3 s; (b) is the damage image of aluminum alloy after the energy density is 3980 J / cm 2 Figure 2. Pulse laser damage to aluminum alloy. (c) is the energy density of 5414 J / cm 2 Image of pulse laser damaging aluminum alloy;

[0022] Figure 3 This is a diagram showing the results of combined laser damage to aluminum alloy in Example 1 of the present invention;

[0023] Figure 4 1 is a diagram showing the damage and melt splashing of aluminum alloy by the combined laser according to Example 2 of the present invention; (a) is a diagram showing the damage of aluminum alloy by the combined laser; (b) is a diagram showing the melt splashing during the combined laser damage process;

[0024] Figure 5 This is a diagram showing the results of combined laser damage to aluminum alloy in Example 3 of the present invention. DETAILED DESCRIPTION

[0025] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments; based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0026] The present invention provides a method for improving metal drilling efficiency by combining laser melting and splashing. Figure 1 , for an aluminum alloy plate with a thickness of 1mm, the following steps are included:

[0027] Step 1: irradiate the aluminum alloy plate with a parallel beam formed by a continuous laser through an optical lens group to the surface of the metal material, so that the parallel beam interacts with the aluminum alloy plate and causes pre-damage;

[0028] Step 2: Using a delay device to cause the pulsed laser to emit light after the continuous laser causes the pre-damage, and controlling the delay time of the two, so that a pulsed laser can be accurately emitted to form a parallel beam through the optical lens group to irradiate the surface of the aluminum alloy plate, and to drill a hole at the same position as the pre-damage;

[0029] Step 3: The continuous laser and the pulse laser stop emitting light at the same time, obtaining a blind hole or a through hole, and completing the drilling.

[0030] Furthermore, the wavelength of the continuous laser is 1064 nm.

[0031] Furthermore, the pulse width of the pulse laser is 10 ms.

[0032] Furthermore, the spot radius of the continuous laser is 5 mm, and the spot radius of the pulsed laser is 1 mm.

[0033] Furthermore, the delayed light emission time of the two in step 2 is 2s-4s.

[0034] Furthermore, the power density of the continuous laser is 1723 W / cm 2 The energy density of the pulse laser is from 3980 J / cm 2 to 5414 J / cm 2

[0035] Furthermore, the spot centers of the continuous laser and the pulse laser coincide with a point on the metal material.

[0036] Further, combined Figure 2 (a), (b), and (c) Continuous laser exposure for 3 s did not cause the aluminum alloy to melt; the energy density was 3980 J / cm 2 The damage diameter of the pulse laser on aluminum alloy is 3.043mm; the energy density is 5414 J / cm 2 The damage diameter of the pulse laser on aluminum alloy is 3.330mm.

[0037] Example 1

[0038] For laser drilling of aluminum alloy plates with a side length of 5 cm and a thickness of 1 mm, the continuous laser is a 1064 nm point light source with a Gaussian distribution and a continuous laser power density of 1723 W / cm 2 The spot radius is 5 mm, the pulse width of the pulse laser is 10 ms, and the energy density of the pulse laser is 3980 J / cm 2, spot radius 1 mm; under the control of the delay device, a continuous laser is first output to cause pre-damage, and then a single pulse laser is output after a delay of 2 s, which acts on the surface of the pre-damaged aluminum alloy plate through the optical lens group, and the two laser beams stop emitting light at the same time.

[0039] The above embodiment 1 was tested and the test results were as follows. Figure 3 As shown in the figure, the combined laser has a better damage effect on aluminum alloy than a single laser, and the damage diameter reaches 4.738 mm. However, under this condition, the combined laser does not cause perforation on the 1 mm thick aluminum alloy plate.

[0040] Example 2

[0041] For laser drilling of an aluminum alloy plate with a side length of 5 cm and a thickness of 1 mm, the continuous laser is a 1064 nm point light source with a Gaussian distribution, the continuous laser power density is 1723 W / cm2, the spot radius is 5 mm, the pulse width of the pulsed laser is 10 ms, the energy density of the pulsed laser is 3980 J / cm2, and the spot radius is 1 mm; under the control of the delay device, the continuous laser is output to cause pre-damage, and then a single pulse laser is output after a delay of 4 s, which acts on the surface of the pre-damaged aluminum alloy plate through the optical lens group, and the two laser beams stop emitting light at the same time.

[0042] The above embodiment 2 was tested and the test results were as follows. Figure 4 As shown, Figure 4 (a) The combined laser has a better damage effect on aluminum alloy than a single laser. Under this condition, the combined laser can create a hole with a diameter of 1.652 mm in a 1 mm thick aluminum alloy plate. Figure 4 (b) is the result of the melt splashing on the aluminum alloy surface under the combined laser conditions. The aluminum alloy melt produced by the continuous laser can be removed by evaporation caused by the pulsed laser or splashing by the recoil pressure, which increases the amount of material removed and improves the material removal rate and laser processing efficiency.

[0043] Example 3

[0044] For laser drilling of an aluminum alloy plate with a side length of 5 cm and a thickness of 1 mm, the laser is a 1064 nm point light source with a Gaussian distribution, the continuous laser power density is 1723 W / cm2, the spot radius is 5 mm, the pulse width of the pulsed laser is 10 ms, the energy density of the pulsed laser is 5414 J / cm2, and the spot radius is 1 mm; under the control of the delay device, a continuous laser is output to cause pre-damage, and then a single pulse laser is output after a delay of 2 s, which acts on the surface of the pre-damaged aluminum alloy plate through the optical lens group, and the two laser beams stop emitting light at the same time.

[0045] The above embodiment 3 was tested and the test results were as follows. Figure 5As shown in the figure, the combined laser has a better damage effect on aluminum alloy than a single laser. Under this condition, the combined laser can cause a hole with a diameter of 1.315 mm in a 1 mm thick aluminum alloy plate. The continuous laser action does not melt the aluminum alloy. The mechanical effect generated during the pulsed laser ablation causes the material below the melting point to be peeled off, enhancing the laser ablation drilling effect.

[0046] The above embodiment is suitable for drilling a through hole with a radius less than 1 mm in an aluminum alloy plate with a thickness of 1 mm.

[0047] It should be noted that, in this document, relational terms such as first and second, etc., are used only to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any actual relationship or order between these entities or operations. Moreover, the terms "comprises," "comprising," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that includes a list of elements includes not only those elements but also other elements not explicitly listed, or elements inherent to such process, method, article, or apparatus.

[0048] While embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions, and variations may be made to these embodiments without departing from the principles and spirit of the invention, and that the scope of the invention is defined by the appended claims and their equivalents.

Claims

1. A method for improving metal drilling efficiency by combining laser with melt spraying, characterized in that: The following steps are involved: Step 1: irradiate the metal material with a parallel beam formed by a continuous laser through an optical lens group, so that the parallel beam interacts with the metal material and causes pre-damage; Step 2: Using a delay device to cause the pulsed laser to emit light after the continuous laser causes the pre-damage, and controlling the delay time of the two, so that a pulsed laser can be accurately emitted to form a parallel beam through the optical lens group to irradiate the surface of the metal material and drill a hole at the same location as the pre-damage; Step 3: The continuous laser and the pulse laser stop emitting light at the same time, obtaining a blind hole or a through hole, and completing the drilling.

2. The method for improving metal drilling efficiency by combined laser spraying according to claim 1, characterized in that: The metal material is one of aluminum alloy, titanium alloy and pure copper.

3. The method for improving metal drilling efficiency by combined laser melting and sputtering according to claim 1, characterized in that: The wavelength of the continuous laser is 1064 nm.

4. The method for improving metal drilling efficiency by combined laser melting and sputtering according to claim 1, characterized in that: The pulse width of the pulse laser is 10 ms.

5. The method for improving metal drilling efficiency by combined laser spraying according to claim 1, characterized in that: The spot radius of the continuous laser is 5 mm, and the spot radius of the pulsed laser is 1 mm.

6. The method for improving metal drilling efficiency by combined laser spraying according to claim 1, characterized in that: The delayed light emission time of the two in step 2 is 2s-4s.

7. The method for improving metal drilling efficiency by combined laser spraying according to claim 1, characterized in that: The power density of the continuous laser and the energy density of the pulsed laser are both greater than the melting threshold of the metal material.

8. The method for improving metal drilling efficiency by combined laser spraying according to claim 5, characterized in that: The spot centers of the continuous laser and the pulse laser coincide with a point on the metal material.

9. The method for improving metal drilling efficiency by combined laser spraying according to claim 1, characterized in that: The optical lens group includes a first optical lens L1 and a second optical lens L2.