Carbon fiber composite material with both interface performance and damping performance and preparation method thereof

Through the carbon fiber composite materials treated with specific composition and process, the problems of carbon fiber composite materials being prone to breakage and insufficient anti-aging in sports equipment are solved, and high-strength and high-damping interface performance is achieved, which is suitable for high-end competitive sports equipment.

CN120535910APending Publication Date: 2025-08-26SHANDONG UNIV +1

Patent Information

Application Number
CN202510932652.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-07-07
Publication Date
2025-08-26

AI Technical Summary

Technical Problem

The existing carbon fiber composite materials are prone to impact and fracture in sports equipment, have insufficient anti-aging performance, insufficient interlayer shear strength, and cannot have excellent interface performance and damping performance.

Method used

Using a combination of 65-75% carbon fiber, 25-35% modified butyl rubber resin matrix, 0.5-2% butyl rubber film and 0.1-0.5% silane coupling agent, the interface performance and damping performance are improved through specific process treatment, including the preparation of modified butyl rubber resin matrix and the surface treatment of carbon fiber, combining sandwich structure and curing process.

Benefits of technology

It significantly improves the shear strength of the fiber-resin interface, achieves excellent interface performance and damping performance, is suitable for the application needs of high-end competitive sports equipment, and has a performance loss of less than 15% after humidity and heat aging.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of composite materials, in particular to a carbon fiber composite material with both interface performance and damping performance and a preparation method of the carbon fiber composite material. The invention relates to a carbon fiber composite material with interfacial properties and damping properties. The carbon fiber composite material is prepared from the following components in percentage by weight: 65-75% of carbon fibers, 25-35% of a modified butyl rubber resin matrix, 0.5-2% of a butyl rubber film, 0.5-1% of a polyurethane-based sizing agent and 0.1-0.5% of a silane coupling agent, the in-situ growth CNTs technology is adopted, the shearing strength of a fiber-resin interface can be remarkably improved, meanwhile, the butyl rubber film is embedded into every two layers of carbon fiber prepreg of a sandwich structure, directional energy dissipation is achieved through controllable shearing deformation, excellent environmental stability is achieved, the damping performance and interface performance loss after damp-heat aging is lower than 15%, and the damping performance and the interface performance loss after damp-heat aging are lower than 15%. The industrial problem that a traditional carbon fiber composite material is strong but not tough and rigid but not soft is successfully solved, and the carbon fiber composite material is particularly suitable for application requirements of high-end competitive sports equipment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of composite materials, and in particular to a carbon fiber composite material having both interface properties and damping properties and a preparation method thereof. Background Art

[0002] Carbon fiber first came into being in the mid-20th century and was mainly used in the military and aerospace fields. The initial carbon fiber used petroleum-based fiber or coal-based fiber as raw materials, which generally had limited performance. With the advancement of technology, the continuous improvement of carbonization technology and pre-oxidation technology, the quality and performance of carbon fiber have been significantly improved. In recent years, carbon fiber composite materials, as a high-performance material, have been widely used in aerospace, automobile, wind power and sports equipment fields due to their excellent properties such as high strength, lightweight and corrosion resistance.

[0003] With the continuous advancement of modern sports technology, athletes are increasingly demanding on sports equipment, especially in terms of weight and performance. Lightweight equipment can help athletes improve their performance, reduce energy consumption, and thus enhance their performance. However, existing carbon fiber composite materials used in sports equipment are prone to fracture under impact, lack aging resistance, and have insufficient interlaminar shear strength. They are prone to delamination under impact or fatigue loads. Therefore, there is an urgent need for a carbon fiber composite material that combines interfacial properties and damping properties to support the performance leap and user experience upgrade of sports equipment.

[0004] In view of the above problems, the present invention provides a solution. Summary of the Invention

[0005] The object of the present invention is to provide a carbon fiber composite material having both interface properties and damping properties and a preparation method thereof, wherein the carbon fiber composite material has excellent interface properties and damping properties.

[0006] To achieve the above-mentioned object, the present invention adopts the following technical solution: a carbon fiber composite material having both interface properties and damping properties is composed of the following percentage components: 65-75% carbon fiber, 25-35% modified butyl rubber resin matrix, 0.5-2% butyl rubber film and 0.1-0.5% silane coupling agent; The preparation method of the modified butyl rubber resin matrix comprises the following steps: A1: Add butyl rubber to a crusher with a crushing size of 300 mesh. After crushing for 30 minutes, filter the crushed rubber through a 300-mesh filter screen to collect the sieved butyl rubber particles. Then, transfer the butyl rubber particles to a 20% acetone-butanone mixed solution. Set the stirrer speed to 600 rpm and stir at 60°C for 3-4 hours to dissolve the rubber. A2: Add maleic anhydride and dicumyl peroxide to the dissolved rubber, raise the temperature to 70-80°C, set the stirrer speed to 600 rpm, and mix and stir for 1.5-2 hours to obtain the grafted dissolved rubber; A3: Heat the epoxy resin to 50-60°C, then add the grafted dissolved rubber and carboxyl-terminated liquid butyl rubber, maintain the temperature, set the stirrer speed to 1200-1500 rpm and stir for 50-60 minutes, then transfer to an ultrasonic processor, set the ultrasonic frequency to 30-40 kHz, and ultrasonically disperse for 30 minutes to obtain the epoxy resin rubber pre-blend; A4: Transfer the epoxy resin rubber pre-blend to a vacuum distillation chamber, set the pressure of the vacuum distillation chamber to 10 kPa and the temperature to 80° C., and perform vacuum distillation until no bubbles escape from the epoxy resin rubber pre-blend to obtain an epoxy resin rubber blend; A5: Mix dicyandiamide powder and diurea-based accelerator and add them to a ball mill. Set the ball mill particle size to 4.5 μm. Ball mill mixing for 30-45 minutes. Then add them to the epoxy resin rubber blend. Set the stirrer speed to 300 rpm. Heat to 60°C and mix at low speed for 1-2 hours. After mixing, transfer to a vacuum deaerator and set the vacuum deaerator pressure to -0.095 MPa. Degas under vacuum for 30 minutes to obtain a dispersed epoxy resin rubber blend. A6: Heat the dispersed epoxy resin rubber blend to 80°C, pre-cure for 1 hour, then heat to 120°C for curing for 2 hours. After the curing is completed, heat to 150°C for repeated curing for 2 hours. After the repeated curing is completed, heat to 180°C for final curing for 1 hour. After the final curing is completed, naturally cool to room temperature to obtain a modified butyl rubber resin matrix.

[0007] Furthermore, the acetone-butanone mixed solution described in step A1 is a mixed solution of 20% acetone solution and 20% butanone solution, wherein the mass ratio of the acetone solution to the butanone solution is 1:1; the mass ratio of the butyl rubber particles described in step A1 to the 20% acetone-butanone mixed solution is 1:4; the mass ratio of the dissolved rubber, maleic anhydride, and diisopropyl peroxide in step A2 is 100:2:1; the mass ratio of the epoxy resin, the grafted dissolved rubber, and the carboxyl-terminated liquid butyl rubber in step A3 is 100:10:1; the mass ratio of the dicyandiamide powder, the diurea-based accelerator, and the epoxy resin rubber blend described in step A5 is 1:0.01:20; Furthermore, a method for preparing a carbon fiber composite material having both interface properties and damping properties comprises the following steps: B1: Immerse the carbon fiber completely in acetone for 8-12 hours. After immersion, remove it and transfer it to an ultrasonic cleaner with an ultrasonic frequency of 60kHz. After ultrasonic cleaning for 5-10 minutes, transfer it to an oven with a temperature of 80°C and a wind speed of 1.5m / s and dry it for 2 hours. B2: The dried carbon fiber was transferred to a 65% nitric acid solution and repeatedly soaked for 1-2 hours. After soaking, it was transferred to an oven, the oven temperature was set to 80°C, the wind speed was 1.5m / s, and the drying was carried out for 45 minutes. Subsequently, ferric nitrate was dissolved in ethanol to prepare an ethanolic ferric nitrate solution, and then the dried carbon fiber was immersed in the ethanolic ferric nitrate solution for 0.5-1 hour. After the immersion was completed, it was transferred to an oven, the oven temperature was set to 60°C, the wind speed was 1.5m / s, and the drying was carried out for 45 minutes to obtain the loaded carbon fiber; B3: Transfer the loaded carbon fibers to a tube furnace, seal it, and evacuate to 0.1 Pa. Then, introduce argon at a flow rate of 80 sccm. Control the heating rate at 10°C / min to raise the temperature to 250-300°C. Then, introduce hydrogen at a flow rate of 30 sccm and maintain for 4 h. B4: After the hydrogen is introduced, the heating rate is controlled to be 5°C / min, and the temperature is raised to 720°C. Then, acetylene and argon are introduced. The flow rate of argon as a load gas is 100 sccm, and the flow rate of acetylene as a carbon source gas is 40 sccm. The growth is carried out for 45-60 minutes. After the growth is completed, the acetylene inlet valve is closed, and argon is continued to be introduced to cool down. The cooling rate is controlled to be 5°C / min until it reaches room temperature to obtain modified carbon fibers; B5: The modified carbon fiber was impregnated with a polyurethane-based sizing agent at 50°C for 2 minutes. After impregnation, the carbon fiber was removed and transferred to a curing chamber for curing at 120°C for 30 minutes. The silane coupling agent was then dissolved in ethanol and sprayed onto the cured modified carbon fiber surface to a thickness of 2 mm. The carbon fiber was then transferred to an 80°C oven with a wind speed of 1.5 m / s and dried for 1 hour. B6: Butyl rubber film is placed between the dried modified carbon fiber layers, with one layer of butyl rubber film sandwiched between every two layers. It is then mixed with the modified butyl rubber resin matrix in a bath at 60°C. After the bath, the resin content is controlled to 25-35% by roller pressing. After roller pressing, the prepreg is transferred to a curing box at 80°C and pre-cured for 10 minutes to obtain a prepreg. B7: Heat the mold to 80℃, then load the prepreg, apply pressure of 0.5MPa to eliminate bubbles, and then transfer it to a curing box. Set the curing box temperature to 80℃ for initial curing for 1h. After the initial curing is completed, heat it to 120℃ for secondary curing for 2h. After the secondary curing is completed, heat it to 150℃ for tertiary curing for 2h. After the tertiary curing is completed, heat it to 180℃ for final curing for 1h. After the final curing is completed, control the cooling rate to 5℃ / min and cool it to room temperature. After cooling, a carbon fiber composite material with both interface properties and damping properties is obtained.

[0008] Furthermore, the concentration of the ferric nitrate ethanol solution in step B2 is 0.05 mol / L; and the mass ratio of the silane coupling agent to ethanol in step B5 is 1:9.

[0009] In summary, due to the adoption of the above technical scheme, the beneficial effect of the present invention is that the in-situ growth CNTs technology of the present invention can significantly improve the shear strength of the fiber-resin interface, and at the same time, a sandwich structure is used in which every two layers of carbon fiber prepreg are embedded in a butyl rubber film, and directional energy dissipation is achieved through controllable shear deformation. It also has excellent environmental stability, and the damping performance and interface performance loss after wet-heat aging are less than 15%, which successfully solves the industry problem of traditional carbon fiber composite materials being "strong but not tough, rigid but not flexible", and is particularly suitable for the application needs of high-end competitive sports equipment. DETAILED DESCRIPTION

[0010] In order to make the technical means, creative features, objectives and effects achieved by the present invention easier to understand, the present invention is further described below in conjunction with specific embodiments.

[0011] Unless otherwise specified, the experimental methods in the following examples are conventional methods and were performed according to the techniques or conditions described in literature in the field or according to product specifications. The materials and reagents used in the following examples are all commercially available unless otherwise specified.

[0012] Example 1: 100 g of butyl rubber was added to a crusher, the crushing particle size was set to 300 mesh, and after crushing for 30 minutes, the crushed particles were filtered through a 300-mesh filter sieve to collect the sieved butyl rubber particles. The butyl rubber particles were then transferred to 400 g of a 20% acetone-butanone mixed solution, the stirrer speed was set to 600 rpm, and the mixture was stirred and dissolved at 60° C. for 4 hours to obtain 500 g of dissolved rubber. 2: Add 10 g of maleic anhydride and 5 g of dicumyl peroxide to the dissolved rubber, raise the temperature to 80°C, set the stirrer speed to 600 rpm, and mix and stir for 2 h to obtain the grafted dissolved rubber; 3: Heat 1 kg of epoxy resin to 60°C, then add 100 g of grafted dissolved rubber and 10 g of carboxyl-terminated liquid butyl rubber, maintain the temperature constant, set the stirrer speed to 1500 rpm and mix and stir for 50-60 minutes, then transfer to an ultrasonic processor, set the ultrasonic frequency to 40 kHz, and ultrasonically disperse for 30 minutes to obtain an epoxy resin rubber pre-blend; 4: Transfer the epoxy resin rubber pre-blend to a vacuum distillation chamber, set the vacuum distillation chamber pressure to 10 kPa, the temperature to 80° C., and vacuum distill until no bubbles escape from the epoxy resin rubber pre-blend to obtain 800 g of epoxy resin rubber blend; 5: Mix 40g of dicyandiamide powder and 0.4g of diurea-based accelerator and add them to a ball mill. Set the ball mill particle size to 4.5μm. Ball mill mixing for 45min and then add them to the epoxy resin rubber blend. Set the stirrer speed to 300rpm, heat to 60℃, and mix at low speed for 2h. After mixing, transfer to a vacuum deaerator and set the vacuum deaerator pressure to -0.095MPa. Degas under vacuum for 30min to obtain a dispersed epoxy resin rubber blend. 6: Heat the dispersed epoxy resin rubber blend to 80°C, pre-cure for 1 hour, then heat to 120°C and cure for 2 hours. After the curing is completed, heat to 150°C and repeat cure for 2 hours. After the repeated curing is completed, heat to 180°C and finally cure for 1 hour. After the final curing is completed, naturally cool to room temperature to obtain 812 g of the modified butyl rubber resin matrix prepared in Example 1.

[0013] Table 1, parameter table of reagents used in Example 1 .

[0014] Example 2, 1: 100 g of butyl rubber was added to a crusher, the crushing particle size was set to 300 mesh, and after crushing for 30 minutes, the crushed rubber was passed through a 300-mesh filter sieve to collect the sieved butyl rubber particles. The butyl rubber particles were then transferred to a 20% acetone-butanone mixed solution, the stirrer speed was set to 600 rpm, and the mixture was stirred and dissolved at 60° C. for 3 hours to obtain dissolved rubber; 2: Add 10 g of maleic anhydride and 5 g of dicumyl peroxide to the dissolved rubber, raise the temperature to 70°C, set the stirrer speed to 600 rpm, and mix and stir for 1.5 h to obtain the grafted dissolved rubber; 3: Heat 1 kg of epoxy resin to 50°C, then add 100 g of grafted dissolved rubber and 10 g of carboxyl-terminated liquid butyl rubber, maintain the temperature constant, set the stirrer speed to 1200 rpm and mix for 50 minutes, then transfer to an ultrasonic processor, set the ultrasonic frequency to 30 kHz, and ultrasonically disperse for 30 minutes to obtain 800 g of epoxy resin rubber pre-blend; 4: Transfer the epoxy resin rubber pre-blend to a vacuum distillation chamber, set the pressure of the vacuum distillation chamber to 10 kPa and the temperature to 80° C., and perform vacuum distillation until no bubbles escape from the epoxy resin rubber pre-blend to obtain the epoxy resin rubber blend; 5: Mix 40g of dicyandiamide powder and 0.4g of diurea-based accelerator and add them to a ball mill. Set the ball mill particle size to 4.5μm and ball mill for 30min. Then add them to the epoxy resin rubber blend. Set the stirrer speed to 300rpm, heat to 60℃, mix at low speed for 1h. After mixing, transfer to a vacuum deaerator and set the vacuum deaerator pressure to -0.095MPa. Defoam in vacuum for 30min to obtain a dispersed epoxy resin rubber blend. 6: Heat the dispersed epoxy resin rubber blend to 80°C, pre-cure for 1 hour, then heat to 120°C and cure for 2 hours. After the curing is completed, heat to 150°C and repeat cure for 2 hours. After the repeated curing is completed, heat to 180°C and finally cure for 1 hour. After the final curing is completed, naturally cool to room temperature to obtain the modified butyl rubber resin matrix prepared in Example 2.

[0015] Table 2, parameters of reagents used in Example 2 .

[0016] Example 3, 1: 650g of carbon fiber was completely immersed in acetone for 12 hours. After immersion, it was removed and transferred to an ultrasonic cleaner with an ultrasonic frequency set to 60kHz. After ultrasonic cleaning for 10 minutes, it was transferred to an oven with an oven temperature set to 80°C and a wind speed of 1.5m / s and dried for 2 hours. 2: The dried carbon fiber was transferred to a 65% nitric acid solution and soaked repeatedly for 2 hours. After soaking, it was transferred to an oven, the oven temperature was set to 80 ° C, the wind speed was 1.5 m / s, and the drying was completed for 45 minutes. Subsequently, 0.05 mol of ferric nitrate was dissolved in 1 L of ethanol to prepare an ethanolic ferric nitrate solution. The dried carbon fiber was then immersed in the ethanolic ferric nitrate solution for 1 hour. After the immersion was completed, it was transferred to an oven, the oven temperature was set to 60 ° C, the wind speed was 1.5 m / s, and the loaded carbon fiber was dried for 45 minutes. 3: Transfer the loaded carbon fibers to a tube furnace, seal it, evacuate it to 0.1 Pa, then introduce argon, control the heating rate at 10°C / min, raise the temperature to 00°C, then introduce hydrogen and maintain for 4 hours; 4: After the hydrogen is introduced, the heating rate is controlled to be 5°C / min, and the temperature is raised to 720°C. Then, acetylene and argon are introduced, with argon as the load gas and acetylene as the carbon source gas. The growth is carried out for 60 minutes. After the growth is completed, the acetylene inlet valve is closed, and argon is continued to be introduced to cool down. The cooling rate is controlled to be 5°C / min until it reaches room temperature to obtain modified carbon fiber; 5: Impregnate the modified carbon fiber into the polyurethane-based sizing agent at a temperature of 50°C for 2 minutes. After impregnation, remove it and transfer it to a curing chamber for curing at 120°C for 30 minutes. Then, dissolve 5g of silane coupling agent in 45g of ethanol and spray the dissolved silane coupling agent on the surface of the cured modified carbon fiber to a thickness of 2mm. Then transfer it to an 80°C oven, set the oven wind speed to 1.5m / s, and dry it for 1 hour. 6: Butyl rubber film was laid between the dried modified carbon fiber layers, with one layer of butyl rubber film sandwiched between every two layers, wherein there were 4 layers of modified carbon fiber and 3 layers of butyl rubber film, with a total weight of 20 g of butyl rubber film. Subsequently, the modified butyl rubber resin matrix prepared in Example 1 was mixed by bathing at 60°C. After the bathing, the resin content was controlled by roller pressing to 350 g. After the rolling was completed, the prepreg was transferred to a curing box, the curing box temperature was set to 80°C, and pre-cured for 10 minutes to obtain a prepreg; 7: Heat the mold to 80°C, then load the prepreg, pressurize it to 0.5MPa to eliminate bubbles, and then transfer it to a curing box. Set the curing box temperature to 80°C for initial curing for 1 hour. After the initial curing is completed, heat it to 120°C for secondary curing for 2 hours. After the secondary curing is completed, heat it to 150°C for tertiary curing for 2 hours. After the tertiary curing is completed, heat it to 180°C for final curing for 1 hour. After the final curing is completed, control the cooling rate to 5°C / min and cool it to room temperature. After cooling, the carbon fiber composite material with both interface properties and damping properties prepared in Example 3 is obtained.

[0017] Table 3, parameter table of reagents used in Example 3 .

[0018] Example 4, 1: 750g of carbon fiber was completely immersed in acetone for 8h. After immersion, it was removed and transferred to an ultrasonic cleaner with an ultrasonic frequency set to 60kHz. After ultrasonic cleaning for 5min, it was transferred to an oven with an oven temperature set to 80°C and a wind speed of 1.5m / s and dried for 2h. 2: The dried carbon fiber was transferred to a 65% nitric acid solution and soaked repeatedly for 1 hour. After soaking, it was transferred to an oven, the oven temperature was set to 80 ° C, the wind speed was 1.5 m / s, and the drying was completed for 45 minutes. Subsequently, 0.05 mol of ferric nitrate was dissolved in 1 L of ethanol to prepare an ethanolic ferric nitrate solution. The dried carbon fiber was then immersed in the ethanolic ferric nitrate solution for 0.5 hours. After the immersion was completed, it was transferred to an oven, the oven temperature was set to 60 ° C, the wind speed was 1.5 m / s, and the loaded carbon fiber was dried for 45 minutes. 3: Transfer the loaded carbon fibers to a tube furnace, seal it, evacuate it to 0.1 Pa, then introduce argon, control the heating rate at 10°C / min, raise the temperature to 250°C, then introduce hydrogen and maintain it for 4 hours; 4: After the hydrogen is introduced, the heating rate is controlled to be 5°C / min, and the temperature is raised to 720°C. Then, acetylene and argon are introduced, with argon as the load gas and acetylene as the carbon source gas. The growth is carried out for 45 minutes. After the growth is completed, the acetylene inlet valve is closed, and argon is continued to be introduced to cool down. The cooling rate is controlled to be 5°C / min until it reaches room temperature to obtain modified carbon fiber; 5: Impregnate the modified carbon fiber into the polyurethane-based sizing agent at a temperature of 50°C for 2 minutes. After impregnation, remove it and transfer it to a curing chamber for curing at 120°C for 30 minutes. Then dissolve the silane coupling agent in ethanol and spray the dissolved silane coupling agent on the surface of the cured modified carbon fiber to a thickness of 2 mm. Then transfer it to an 80°C oven, set the oven wind speed to 1.5 m / s, and dry it for 1 hour. 6: Butyl rubber film is laid between the dried modified carbon fiber layers, with one layer of butyl rubber film sandwiched between every two layers, wherein there are 4 layers of modified carbon fiber and 3 layers of butyl rubber film, and the total weight of butyl rubber film is 5g. It is then mixed with the modified butyl rubber resin matrix in a bath at a bath temperature of 60°C. After the bath is completed, the resin content is controlled by roller pressing to 350g. After rolling, it is transferred to a curing box, the curing box temperature is set to 80°C, and pre-cured for 10 minutes to obtain a prepreg; 7: Heat the mold to 80°C, then load the prepreg, pressurize it to 0.5MPa to eliminate bubbles, and then transfer it to a curing box. Set the curing box temperature to 80°C for initial curing for 1 hour. After the initial curing is completed, heat it to 120°C for secondary curing for 2 hours. After the secondary curing is completed, heat it to 150°C for tertiary curing for 2 hours. After the tertiary curing is completed, heat it to 180°C for final curing for 1 hour. After the final curing is completed, control the cooling rate to 5°C / min and cool it to room temperature. After cooling, the carbon fiber composite material with both interface properties and damping properties prepared in Example 4 is obtained.

[0019] Table 4, parameter table of reagents used in Example 4 .

[0020] Comparative Example 1 Example 1 of the Chinese patent publication number CN107459682A was selected as comparative example 1.

[0021] Comparative Example 2 Example 1 of the Chinese patent publication number CN108586836A was selected as comparative example 2.

[0022] Microdrop debonding test The composite materials prepared in Example 3, Example 4, Comparative Example 1, and Comparative Example 2 were respectively cut into standard samples with a length of 5 cm, a width of 300 μm, and a thickness of 300 μm. Subsequently, E-51 epoxy resin droplets with a diameter of 150 μm were suspended on the standard samples and cured at 80°C for 1 hour. The standard sample was suspended on an Instron 5944 micro-force testing machine. The two ends of the fiber were fixed on the fixture so that the droplet was located between the two blades. The blades were then used to push the droplet at a speed of 0.5 mm / min until the fiber and the resin were debonded. The maximum load was recorded. Table 5, Particle debonding test results .

[0023] By analyzing Table 5, it can be seen that the maximum load of the carbon fiber composite materials prepared in Examples 3 and 4 in the droplet debonding test is significantly higher than that in Comparative Examples 1 and 2. This shows that the carbon fiber composite materials prepared in Examples 3 and 4 can significantly improve the interfacial shear strength and have better interface performance. The rackets prepared in Examples 3 and 4 can significantly reduce the risk of fiber resin debonding when hitting the ball.

[0024] Damping performance test The composite materials prepared in Example 3, Example 4, Comparative Example 1, and Comparative Example 2 were prepared into rectangular strips with a length of 30 mm, a width of 20 mm, and a thickness of 2 mm. The rectangular strips were then placed in a three-point bending fixture and subjected to a periodic vibration load with an amplitude of 10 μm and a frequency of 1 Hz. The stress phase difference generated in the material was measured to obtain tan δ. The temperature was then lowered to -50°C. After the temperature was lowered, a curve of tan δ versus temperature was recorded in real time at a heating rate of 2°C / min. The temperature corresponding to the peak value of tan δ and the temperature range corresponding to tan δ being greater than 0.1 were recorded. Table 6, Damping performance test results .

[0025] By analyzing Table 6, it can be seen that the composite materials prepared in Examples 3 and 4 have better damping performance, among which Example 3 has the best damping performance, and its tan δ peak value can reach 0.14. The racket prepared using it can have better damping and shock absorption effect.

[0026] Humidity and heat aging test Rectangular strips made from the composite materials prepared in Example 3, Example 4, Comparative Example 1, and Comparative Example 2 were placed at 80° C. and 85% humidity for 500 hours, and the tan δ peak retention rate and impact strength retention rate were then recorded. Table 7, wet heat aging test results .

[0027] From the analysis of Table 7, it can be seen that after wet heat aging, the composite materials prepared in Example 3 and Example 4 still have good impact strength and damping performance, and their wet heat loss does not exceed 15%, which has good anti-aging ability.

[0028] The basic principles, main features, and advantages of the present invention are shown and described above. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The above embodiments and descriptions are merely illustrative of the principles of the present invention. Various changes and modifications may be made to the present invention without departing from the spirit and scope of the present invention. Such changes and modifications are intended to fall within the scope of the present invention. The scope of protection claimed in the present invention is defined by the appended claims and their equivalents.

Claims

1. A carbon fiber composite material having both interface properties and damping properties, characterized in that: It is composed of the following percentage components: 65-75% carbon fiber, 25-35% modified butyl rubber resin matrix, 0.5-2% butyl rubber film, 0.5-1% polyurethane-based sizing agent and 0.1-0.5% silane coupling agent; The preparation method of the modified butyl rubber resin matrix comprises the following steps: A1: Add butyl rubber to a crusher with a crushing size of 300 mesh. After crushing for 30 minutes, filter the crushed rubber through a 300-mesh filter screen to collect the sieved butyl rubber particles. Then, transfer the butyl rubber particles to a 20% acetone-butanone mixed solution. Set the stirrer speed to 600 rpm and stir at 60°C for 3-4 hours to dissolve the rubber. A2: Add maleic anhydride and dicumyl peroxide to the dissolved rubber, raise the temperature to 70-80°C, set the stirrer speed to 600 rpm, and mix and stir for 1.5-2 hours to obtain the grafted dissolved rubber; A3: Heat the epoxy resin to 50-60°C, then add the grafted dissolved rubber and carboxyl-terminated liquid butyl rubber, maintain the temperature, set the stirrer speed to 1200-1500 rpm and stir for 50-60 minutes, then transfer to an ultrasonic processor, set the ultrasonic frequency to 30-40 kHz, and ultrasonically disperse for 30 minutes to obtain the epoxy resin rubber pre-blend; A4: Transfer the epoxy resin rubber pre-blend to a vacuum distillation chamber, set the pressure of the vacuum distillation chamber to 10 kPa and the temperature to 80° C., and perform vacuum distillation until no bubbles escape from the epoxy resin rubber pre-blend to obtain an epoxy resin rubber blend; A5: Mix dicyandiamide powder and diurea-based accelerator and add them to a ball mill. Set the ball mill particle size to 4.5 μm. Ball mill mixing for 30-45 minutes. Then add them to the epoxy resin rubber blend. Set the stirrer speed to 300 rpm. Heat to 60°C and mix at low speed for 1-2 hours. After mixing, transfer to a vacuum deaerator and set the vacuum deaerator pressure to -0.095 MPa. Degas under vacuum for 30 minutes to obtain a dispersed epoxy resin rubber blend. A6: Heat the dispersed epoxy resin rubber blend to 80°C, pre-cure for 1 hour, then heat to 120°C for curing for 2 hours. After the curing is completed, heat to 150°C for repeated curing for 2 hours. After the repeated curing is completed, heat to 180°C for final curing for 1 hour. After the final curing is completed, naturally cool to room temperature to obtain a modified butyl rubber resin matrix.

2. The carbon fiber composite material having both interface properties and damping properties according to claim 1, characterized in that: The acetone-butanone mixed solution described in step A1 is a mixed solution of 20% acetone solution and 20% butanone solution, wherein the mass ratio of the acetone solution to the butanone solution is 1:

1.

3. The carbon fiber composite material having both interface properties and damping properties according to claim 1, characterized in that: The mass ratio of the butyl rubber particles and the 20% acetone-butanone mixed solution described in step A1 is 1:

4.

4. The carbon fiber composite material having both interface properties and damping properties according to claim 1, characterized in that: In step A2, the mass ratio of the dissolved rubber, maleic anhydride and diisopropyl peroxide is 100:2:

1.

5. The carbon fiber composite material having both interface properties and damping properties according to claim 1, characterized in that: In step A3, the mass ratio of the epoxy resin, the grafted dissolved rubber, and the carboxyl-terminated liquid butyl rubber is 100:10:

1.

6. The carbon fiber composite material having both interface properties and damping properties according to claim 1, characterized in that: The mass ratio of the dicyandiamide powder, the diurea-based accelerator and the epoxy resin rubber blend described in step A5 is 1:0.01:

20.

7. The method for preparing a carbon fiber composite material having both interface properties and damping properties according to claim 1, characterized in that: The following steps are involved: B1: Immerse the carbon fiber completely in acetone for 8-12 hours. After immersion, remove it and transfer it to an ultrasonic cleaner with an ultrasonic frequency of 60kHz. After ultrasonic cleaning for 5-10 minutes, transfer it to an oven with a temperature of 80°C and a wind speed of 1.5m / s and dry it for 2 hours. B2: The dried carbon fiber was transferred to a 65% nitric acid solution and repeatedly soaked for 1-2 hours. After soaking, it was transferred to an oven, the oven temperature was set to 80°C, the wind speed was 1.5m / s, and the drying was carried out for 45 minutes. Subsequently, ferric nitrate was dissolved in ethanol to prepare an ethanolic ferric nitrate solution, and then the dried carbon fiber was immersed in the ethanolic ferric nitrate solution for 0.5-1 hour. After the immersion was completed, it was transferred to an oven, the oven temperature was set to 60°C, the wind speed was 1.5m / s, and the drying was carried out for 45 minutes to obtain the loaded carbon fiber; B3: Transfer the loaded carbon fibers to a tube furnace, seal it, evacuate it to 0.1 Pa, then introduce argon gas, control the heating rate at 10°C / min, raise the temperature to 250-300°C, then introduce hydrogen gas and maintain for 4 hours; B4: After the hydrogen is introduced, the temperature is raised to 720°C at a rate of 5°C / min, and then acetylene and argon are introduced, with argon as the load gas and acetylene as the carbon source gas, and the growth is carried out for 45-60 minutes. After the growth is completed, the acetylene inlet valve is closed, and argon is continued to be introduced to cool down, and the cooling rate is controlled at 5°C / min until it reaches room temperature to obtain modified carbon fibers; B5: The modified carbon fiber was impregnated with a polyurethane-based sizing agent at 50°C for 2 minutes. After impregnation, the carbon fiber was removed and transferred to a curing chamber for curing at 120°C for 30 minutes. The silane coupling agent was then dissolved in ethanol and sprayed onto the cured modified carbon fiber surface to a thickness of 2 mm. The carbon fiber was then transferred to an 80°C oven with a wind speed of 1.5 m / s and dried for 1 hour. B6: Butyl rubber film is placed between the dried modified carbon fiber layers, with one layer of butyl rubber film sandwiched between every two layers. It is then mixed with the modified butyl rubber resin matrix in a bath at 60°C. After the bath, the resin content is controlled to 25-35% by roller pressing. After roller pressing, the prepreg is transferred to a curing box at 80°C and pre-cured for 10 minutes to obtain a prepreg. B7: Heat the mold to 80℃, then load the prepreg, apply pressure of 0.5MPa to eliminate bubbles, and then transfer it to a curing box. Set the curing box temperature to 80℃ for initial curing for 1h. After the initial curing is completed, heat it to 120℃ for secondary curing for 2h. After the secondary curing is completed, heat it to 150℃ for tertiary curing for 2h. After the tertiary curing is completed, heat it to 180℃ for final curing for 1h. After the final curing is completed, control the cooling rate to 5℃ / min and cool it to room temperature. After cooling, a carbon fiber composite material with both interface properties and damping properties is obtained.

8. The method for preparing a carbon fiber composite material having both interface properties and damping properties according to claim 7, characterized in that: The concentration of the ferric nitrate ethanol solution described in step B2 is 0.05 mol / L.

9. The method for preparing a carbon fiber composite material having both interface properties and damping properties according to claim 7, characterized in that: The mass ratio of the silane coupling agent to ethanol in step B5 is 1:9.

Citation Information

Patent Citations

  • Preparation method for carbon fiber enhanced rubber composite material

    CN107459682A

  • Carbon fiber-based rubber composite material and preparation method thereof

    CN108586836A

Cited By

  • Fiber reinforced resin matrix composite material with damping impact resistance performance and its preparation method and application

    CN122518747A

  • Fiber reinforced resin matrix composite material with damping impact resistance performance and its preparation method and application

    CN122518747B