A highly bioadhesive, on-demand peelable hydrogel and its preparation method
Hydrogels were prepared by free radical polymerization of hydrophobic amino acid vinyl monomers, hydrophilic monomers, and thermosensitive monomers, which solved the problem of adhesion instability of biological tissue adhesives in acute tissue injury. They achieved strong adhesion triggered by body temperature and mild peeling triggered by room temperature, making them suitable for rapid hemostasis and closure of various internal organs.
Patent Information
- Application Number
- CN202510490425.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-04-18
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2045-04-18
AI Technical Summary
Existing biological tissue adhesives are difficult to achieve in-situ wet bonding triggered by body temperature and gentle on-demand peeling triggered by room temperature in acute tissue injury, and are easily affected by interfacial water molecules, leading to unstable bonding and possible secondary tissue damage.
A highly biocompatible, on-demand peelable hydrogel was prepared by free radical polymerization using hydrophobic amino acid vinyl monomers, hydrophilic monomers, and thermosensitive monomers. The bonding and peeling were achieved by temperature-driven phase transition, and the special structure of the hydrophobic amino acid vinyl monomers enhanced the formation of multiple hydrogen bonds.
It achieves strong wet adhesion and gentle separation with various internal organs and tissues under physiological conditions, rapid hemostasis and closure, and is simple to operate, has good biocompatibility, and is suitable for rapid hemostasis and closure of acute tissue trauma.
Smart Images

Figure CN120554566B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of polymer hydrogel technology, and in particular to an on-demand peelable hydrogel with high biowet tissue adhesion through temperature-driven reversible phase transition, its preparation method, and its application. Background Technology
[0002] Acute tissue injury is often accompanied by massive bleeding, easily leading to serious conditions such as hypotension and multiple organ dysfunction. According to the World Health Organization, approximately five million people worldwide die each year from acute tissue trauma caused by factors such as traffic accidents, natural disasters, and surgery. Currently, sutures and staples are the main methods for emergency hemostasis and wound closure in clinical practice; however, their operation is complex and requires applying significant local stress to the tissue, easily causing postoperative infection, leakage, and secondary tissue damage, posing challenges when applied to fragile internal organs and in emergency situations. Hydrogel-based tissue adhesives, as a convenient, well-compliant, and biocompatible biomedical material, can be quickly applied to irregular tissue wounds and have gradually developed into an effective auxiliary and alternative solution to traditional surgical suturing and staples in recent years. However, achieving interfacial wet bonding remains challenging, primarily due to two reasons: First, solutions such as tissue exudate, blood, and tissue contents form a hydration layer on the surface of biological tissues, affecting and hindering direct contact and chemical bonding between the hydrogel and the biological tissue. Second, water molecules that penetrate the polymer network through osmosis disrupt the intermolecular interactions of the hydrogel matrix, thereby weakening the mechanical properties and structural stability of the hydrogel adhesive matrix. Therefore, effectively eliminating the interference of interfacial water molecules is crucial for developing hydrogel bio-tissue adhesives with strong and durable bonding properties.
[0003] Current design strategies for wet tissue adhesives are primarily inspired by marine organisms. Inspired by the underwater adhesion phenomena of mussels, molecules with catechol structures can effectively penetrate the interfacial hydration layer, achieving strong wet adhesion through various interactions with biological tissues. However, in emergency situations such as bleeding, once these adhesives form a strong and stable bond with the interface, subsequent misalignment correction and non-destructive, on-demand peeling can be challenging, potentially causing secondary damage to the injured tissue / organ and affecting subsequent clinical treatment. Summary of the Invention
[0004] The present invention aims to address how to achieve the characteristics of in-situ wet bonding triggered by body temperature and mild, on-demand peeling triggered by room temperature in biological tissue adhesives; and to provide a mechanism for in-situ wet bonding and mild, on-demand peeling of biological tissue adhesives driven by temperature-driven phase transition.
[0005] The purpose of this invention is to overcome the shortcomings of existing technologies and provide an on-demand peelable biological tissue adhesive and its preparation method. A peelable hydrogel with high adhesion to wet biological tissues is prepared by one-pot free radical polymerization of hydrophobic amino acid acrylamide monomers and hydrophilic monomers combined with temperature-sensitive vinyl monomers.
[0006] To achieve the above objectives, the technical solution adopted by the present invention is as follows:
[0007] On one hand, the present invention provides an on-demand peelable hydrogel with high biowet tissue adhesion, which is prepared by free radical polymerization of hydrophobic amino acid vinyl monomers, hydrophilic monomers and thermosensitive monomers.
[0008] Furthermore, the structure of the hydrophobic amino acid vinyl monomer is shown in formula (I):
[0009]
[0010] Furthermore, the ratio of the number of structural units between the hydrophobic amino acid vinyl monomer, the hydrophilic monomer, and the thermosensitive monomer is 1:(9-13):(0.5-2).
[0011] Furthermore, the hydrophobic amino acid vinyl monomer is selected from one or more of N-acryloylalanine (AL), N-acryloylvaline (AV), N-acryloylphenylalanine (APA), N-acryloylleucine (ALE), N-acryloylisoleucine (AIL), N-acryloyltryptophan (ATP), N-acryloylmethionine (AMT), N-acryloylalanine (ALN), N-acryloylvaline (AVN), and N-acryloylphenylalanine (APN); the hydrophilic monomer is selected from acrylic acid (AA), methacrylic acid (MAA), 2-hydroxyethyl acrylate (HEA), hydroxyethyl methacrylate (HEMA), acrylamide (AM), N-tris(hydroxymethyl)methacrylamide (THMA), and N,N-dimethylacrylamide. The thermosensitive monomer is selected from one or more of the following: DMA, HEAA, NVP, AASP, AGLU, AG, AT, AT, AS, AT, and AGT; the thermosensitive monomer is selected from N-isopropylacrylamide (NIPAM), OEGMA, NVCL, MEO2MA, N-vinylpyrrolidone (NVP), and HPA.
[0012] On the other hand, the present invention provides a method for preparing the on-demand peelable hydrogel with high bio-wet tissue adhesion as described above. The method includes the following steps: S1, dissolving the hydrophobic amino acid vinyl monomer, hydrophilic monomer, and thermosensitive monomer fully in an aqueous solution to obtain a colorless and transparent mixture; S2, adding an initiator and an initiator accelerator to the mixture at room temperature and mixing evenly to complete free radical polymerization and obtain a polymer; S3, storing the polymer in an environment below room temperature to obtain the on-demand peelable hydrogel with high bio-wet tissue adhesion.
[0013] Furthermore, the total concentration of the hydrophobic amino acid vinyl monomer and the hydrophilic monomer is 6.7–7.7 M, wherein the concentration ratio of the hydrophobic amino acid vinyl monomer to the hydrophilic monomer is 0.7–6:7; optionally, the concentration of the thermosensitive unit monomer is 0.2–1.0 mol / L.
[0014] Furthermore, the initiator is selected from one or more of potassium persulfate, ammonium persulfate, and azobisisobutyrazoline hydrochloride; the initiator promoter is N,N,N',N'-tetramethylethylenediamine.
[0015] Furthermore, the amount of the initiator added is 0.5% to 2% of the total mass of the hydrophobic amino acid vinyl monomer, the hydrophilic monomer, and the thermosensitive monomer; the amount of the initiator promoter added is greater than 0% and less than or equal to 30% of the mass of the initiator.
[0016] Furthermore, in step S1, the method of complete dissolution is selected from one or more of heating, ultrasonication, and vortex oscillation; in step S2, the temperature of free radical polymerization is 20-80℃, and the reaction time is 2-12h.
[0017] This invention provides the application of the on-demand peelable hydrogel with high bio-wet tissue adhesion as described above in the fields of wound closure and rapid hemostasis.
[0018] Compared with existing technologies, the on-demand peelable hydrogel with high bio-wet tissue adhesion, its preparation method, and its application provided by this invention have at least the following advantages:
[0019] This hydrogel is obtained by polymerizing a hydrophobic amino acid acrylamide derivative and a hydrophilic monomer with a temperature-sensitive monomer. The hydrophobic amino acid vinyl monomer phenylalanine derivative provided by this invention has a unique structure where the carboxyl group and benzene ring are located in the same structural unit. This structure not only effectively disrupts the hydration layer at the tissue interface but also enhances the strength of the matrix by forming stable multiple hydrogen bonds, achieving strong adhesion (60 kPa) within 5 seconds of contact with moist biological tissue. Furthermore, by exploring the mechanism of temperature-driven phase transition and the structure-activity relationship between phase transition and macroscopic properties, a multifunctional biological tissue adhesive has been developed that can achieve rapid hemostasis and closure of wounds in tissues such as arteries, heart, and liver under physiological conditions, and can gently peel off as needed in response to temperature stimuli.
[0020] (1) The on-demand peelable hydrogel with high bio-wet tissue adhesion provided by the present invention is simple and convenient to use, has strong adhesion and is very stable. It can form a strong and stable adhesion with wet tissue with only body temperature triggering. Moreover, the adhesion interface is not affected by external water molecules. In addition, the hydrogel exhibits strong and stable wet adhesion with various internal organs and tissues (heart, liver, lung, stomach, artery), and has the potential to promote tissue wound closure and rapid hemostasis.
[0021] (2) The on-demand peeling hydrogel with high biowet tissue adhesion provided by the present invention can achieve firm wet adhesion and gentle on-demand peeling of different types of biological tissues under physiological conditions, meeting the requirements of rapid hemostasis and closure of clinical tissue trauma and subsequent non-damaging on-demand peeling applications.
[0022] (3) The method for preparing and operating the on-demand peelable hydrogel with high bio-wet tissue adhesion provided by the present invention is simple and quick. The present invention prepares a polymer hydrogel through a one-step free radical polymerization method, which is convenient for low-temperature storage and requires only body temperature to trigger the formation of a strong and firm wet adhesion to the tissue.
[0023] (4) The on-demand peelable hydrogel with high biocompatibility to wet tissue provided by the present invention has good biocompatibility. The hydrogel patch obtained by free radical polymerization of hydrophobic amino acid derivatives, hydrophilic monomers and temperature-sensitive vinyl monomers has excellent biocompatibility, which is conducive to clinical translation and provides a new option for replacing surgical sutures to achieve wound closure and rapid hemostasis in clinical practice. Attached Figure Description
[0024] Figure 1 The graph shows the wet bond strength test results of the hydrogel provided in Example 5 at different temperatures;
[0025] Figure 2 The graph shows the test results of wet adhesion strength and switching efficiency between the hydrogel provided in Example 5 and various porcine tissues;
[0026] Figure 3 The graph shows the rheological test results of the gel modulus as a function of temperature provided in Example 5;
[0027] Figure 4 The images show the low-field NMR test results of the gels provided in Examples 1, 2, 3, 4, 5, 6, and 7. Detailed Implementation
[0028] The following embodiments are merely some, not all, of the embodiments of the present invention. Therefore, the detailed descriptions of the embodiments provided below are not intended to limit the scope of the claimed invention, but merely to illustrate selected embodiments. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without inventive effort are within the scope of protection of the present invention.
[0029] In this invention, unless otherwise specified, all equipment and raw materials are commercially available or commonly used in the industry. The methods described in the following embodiments are conventional methods in the art, unless otherwise specified.
[0030] In one embodiment, the hydrophobic amino acid vinyl monomer corresponding to the hydrophobic amino acid vinyl structural unit is selected from one or more of N-acryloylalanine, N-acryloylvaline, N-acryloylphenylalanine, N-acryloylleucine, N-acryloylisoleucine, N-acryloyltryptophan, N-acryloylmethionine, N-acryloylalanamide, N-acryloylvaline, and N-acryloylphenylalanamide.
[0031] In one embodiment, the hydrophilic monomer corresponding to the hydrophilic structural unit is selected from one or more of acrylic acid, methacrylic acid, 2-hydroxyethyl acrylate, hydroxyethyl methacrylate, acrylamide, N-trimethylolmethacrylamide, N,N-dimethylacrylamide, N-hydroxyethylacrylamide, 1-vinyl-2-pyrrolidone, N-acryloylaspartic acid, N-acryloylglutamic acid, N-acryloylglycine, N-acryloyltyrosine, N-acryloylserine, N-acryloylthreonine, and N-acryloylglutamine.
[0032] In one embodiment, the thermosensitive monomer is selected from N-isopropylacrylamide, polyethylene glycol methyl ether methacrylate, N-vinylcaprolactam, 2-(2-methoxyethoxy)ethyl methacrylate, N-vinylpyrrolidone, and hydroxypropyl acrylate.
[0033] The method for preparing this on-demand peelable hydrogel with high bio-wet tissue adhesion includes the following steps:
[0034] S1. Dissolve the hydrophobic amino acid vinyl monomer, the hydrophilic monomer, and the thermosensitive vinyl monomer fully in an aqueous solution to obtain a colorless and transparent mixture.
[0035] S2. At room temperature, add the initiator and initiator accelerator and mix thoroughly to complete the free radical polymerization;
[0036] S3. Soak the polymer in deionized water to obtain the on-demand peelable hydrogel with high biowet tissue adhesion.
[0037] In one embodiment, the total concentration of the hydrophobic amino acid vinyl monomer and the hydrophilic monomer is 6.7–7.7 mol / L;
[0038] The concentration of the thermosensitive vinyl unit monomer is 0.2–1.0 mol / L.
[0039] In one embodiment, the concentration of the thermosensitive vinyl unit monomer is 0.2–1.0 mol / L;
[0040] In one embodiment, the initiator is selected from one or more of potassium persulfate, ammonium persulfate, and azobisisobutyrazoline hydrochloride;
[0041] The initiator / promoter is N,N,N',N'-tetramethylethylenediamine.
[0042] In one embodiment, the amount of the initiator added is 0.5% to 2% of the total mass of the hydrophobic amino acid vinyl monomer, the hydrophilic monomer, and the zwitterionic monomer;
[0043] The amount of the initiator accelerator added is 0-30% of the mass of the initiator.
[0044] In one embodiment, in step S1, the method of achieving complete dissolution is selected from one or more of heating, ultrasonication, and vortex oscillation;
[0045] In step S2, the polymerization temperature is 20–80℃, and the polymerization reaction time is 2–12 h;
[0046] In step S3, the storage temperature should be below room temperature.
[0047] Examples 1-19 are provided based on the preparation method of the on-demand peelable hydrogel with high bio-wet tissue adhesion provided above.
[0048] The hydrophobic amino acid vinyl monomer mentioned in this invention is obtained according to the methods described in Biomacromolecules 2021, 22, 1297-1304; Sci. Adv. 2023, 9, eadg4031.
[0049] Example 1: P(APA) 0.7 -AA 7.0 )
[0050] Free radical copolymerization of APA and AA monomers: 153 mg APA and 504 mg AA were dissolved together in 1 mL of deionized water by heating at 60 °C, sonication, and vortexing to achieve a concentration of 0.7 mol / L for APA and 7.0 mol / L for AA. After complete dissolution, the mixed solution was cooled to room temperature, and 3.28 mg ammonium persulfate was added as an initiator, and 0.98 mg N,N,N',N'-tetramethylethylenediamine was added as an initiator accelerator. After mixing evenly, the mixture was placed in a 60 °C oven and allowed to stand for 3 h to initially obtain a hydrogel. The hydrogel was then stored in an environment below room temperature to obtain a peelable hydrogel with high bio-wet tissue adhesion.
[0051] Example 2: P(APA) 0.7 -AA 6.8 -NIPAM 0.2 )
[0052] Free radical copolymerization was carried out using APA, AA, and NIPAM monomers: 153 mg APA, 490 mg AA, and 22.636 mg NIPAM were dissolved together in 1 mL of deionized water by heating at 60 °C, sonication, and vortexing to achieve a concentration of 0.7 mol / L for APA, 6.8 mol / L for AA, and 0.2 mol / L for NIPAM. After complete dissolution, the mixed solution was cooled to room temperature, and 3.4 mg ammonium persulfate was added as an initiator, and 1.02 mg N,N,N',N'-tetramethylethylenediamine was added as an initiator accelerator. After mixing evenly, the mixture was placed in a 60 °C oven and allowed to stand for 3 h to initially obtain a hydrogel. The hydrogel was then stored in an environment below room temperature to obtain a peelable hydrogel with high bio-wet tissue adhesion.
[0053] Example 3: P(APA) 0.7 -AA 6.6 -NIPAM 0.4 )
[0054] Free radical copolymerization was carried out using APA, AA, and NIPAM monomers: 153 mg APA, 476 mg AA, and 45.3 mg NIPAM were dissolved together in 1 mL of deionized water by heating at 60 °C, sonication, and vortexing to achieve a concentration of 0.7 mol / L for APA, 6.6 mol / L for AA, and 0.4 mol / L for NIPAM. After complete dissolution, the mixed solution was cooled to room temperature, and 3.37 mg ammonium persulfate was added as an initiator, and 1.01 mg N,N,N',N'-tetramethylethylenediamine was added as an initiator accelerator. After mixing evenly, the mixture was placed in a 60 °C oven and allowed to stand for 3 h to initially obtain a hydrogel. The hydrogel was then stored in an environment below room temperature to obtain a peelable hydrogel with high bio-wet tissue adhesion.
[0055] Example 4: P(APA) 0.7 -AA 6.4 -NIPAM 0.6 )
[0056] Free radical copolymerization was carried out using APA, AA, and NIPAM monomers: 153 mg APA, 461 mg AA, and 67.9 mg NIPAM were dissolved in 1 mL of deionized water by heating at 60 °C, sonication, and vortexing to achieve a concentration of 0.7 mol / L for APA, 6.4 mol / L for AA, and 0.6 mol / L for NIPAM. After complete dissolution, the mixed solution was cooled to room temperature, and 3.40 mg ammonium persulfate was added as an initiator, along with 1.02 mg N,N,N',N'-tetramethylethylenediamine as an initiator accelerator. After thorough mixing, the mixture was placed in a 60 °C oven and allowed to stand for 3 hours to initially obtain a hydrogel. This hydrogel was then stored in an environment below room temperature to obtain a highly biocompatible, on-demand peelable hydrogel.
[0057] Example 5: P(APA) 0.7 -AA 6.2 -NIPAM 0.8 )
[0058] Free radical copolymerization was carried out using APA, AA, and NIPAM monomers: 153 mg APA, 446 mg AA, and 90.53 mg NIPAM were dissolved in 1 mL of deionized water by heating at 60 °C, sonication, and vortexing to achieve a concentration of 0.7 mol / L for APA, 6.2 mol / L for AA, and 0.8 mol / L for NIPAM. After complete dissolution, the mixed solution was cooled to room temperature, and 3.45 mg ammonium persulfate was added as an initiator, along with 1.03 mg N,N,N',N'-tetramethylethylenediamine as an initiator accelerator. After thorough mixing, the mixture was placed in a 60 °C oven and allowed to stand for 3 hours to initially obtain a hydrogel. This hydrogel was then stored in an environment below room temperature to obtain a highly biocompatible, on-demand peelable hydrogel.
[0059] Example 6: P(APA) 0.6 -AA 6.1 -NIPAM 0.9 )
[0060] Free radical copolymerization was carried out using APA, AA, and NIPAM monomers: 153 mg APA, 439 mg AA, and 101.84 mg NIPAM were dissolved in 1 mL of deionized water by heating at 60 °C, sonication, and vortexing to achieve a concentration of 0.7 mol / L for APA, 6.1 mol / L for AA, and 0.9 mol / L for NIPAM. After complete dissolution, the mixed solution was cooled to room temperature, and 3.47 mg ammonium persulfate was added as an initiator, along with 1.04 mg N,N,N',N'-tetramethylethylenediamine as an initiator accelerator. After thorough mixing, the mixture was placed in a 60 °C oven and allowed to stand for 3 hours to initially obtain a hydrogel. This hydrogel was then stored in an environment below room temperature to obtain a highly biocompatible, on-demand peelable hydrogel.
[0061] Example 7: P(APA) 0.7 -AA6-NIPAM1)
[0062] Free radical copolymerization was carried out using APA, AA, and NIPAM monomers: 153 mg APA, 432.42 mg AA, and 113.18 mg NIPAM were dissolved in 1 mL of deionized water by heating at 60 °C, sonication, and vortexing to achieve a concentration of 0.7 mol / L for APA, 6.0 mol / L for AA, and 1.0 mol / L for NIPAM. After complete dissolution, the mixed solution was cooled to room temperature, and 3.49 mg ammonium persulfate was added as an initiator, along with 1.05 mg N,N,N',N'-tetramethylethylenediamine as an initiator accelerator. After thorough mixing, the mixture was placed in a 60 °C oven and allowed to stand for 3 hours to initially obtain a hydrogel. This hydrogel was then stored in an environment below room temperature to obtain a highly biocompatible, on-demand peelable hydrogel.
[0063] Example 8: P(APA) 0.5 -AA 6.2 -NIPAM 0.8 )
[0064] Free radical copolymerization was carried out using APA, AA, and NIPAM monomers: 110 mg APA, 446 mg AA, and 90.53 mg NIPAM were dissolved in 1 mL of deionized water by heating at 60 °C, sonication, and vortexing to achieve a concentration of 0.5 mol / L for APA, 6.2 mol / L for AA, and 0.8 mol / L for NIPAM. After complete dissolution, the mixed solution was cooled to room temperature, and 3.23 mg ammonium persulfate was added as an initiator, along with 0.96 mg N,N,N',N'-tetramethylethylenediamine as an initiator accelerator. After thorough mixing, the mixture was placed in a 60 °C oven and allowed to stand for 3 hours to initially obtain a hydrogel. This hydrogel was then stored in an environment below room temperature to obtain a highly biocompatible, on-demand peelable hydrogel.
[0065] Example 9: P(APA) 0.6 -AA 6.2 -NIPAM 0.8 )
[0066] Free radical copolymerization was carried out using APA, AA, and NIPAM monomers: 131.5 mg APA, 446 mg AA, and 90.53 mg NIPAM were dissolved together in 1 mL of deionized water by heating at 60 °C, sonication, and vortexing to achieve a concentration of 0.6 mol / L for APA, 6.2 mol / L for AA, and 0.8 mol / L for NIPAM. After complete dissolution, the mixed solution was cooled to room temperature, and 3.34 mg ammonium persulfate was added as an initiator, along with 1.0 mg N,N,N',N'-tetramethylethylenediamine as an initiator accelerator. After thorough mixing, the mixture was placed in a 60 °C oven and allowed to stand for 3 hours to initially obtain a hydrogel. This hydrogel was then stored in an environment below room temperature to obtain a highly bioadhesive, on-demand peelable hydrogel.
[0067] Example 10: P(APA) 0.8 -AA 6.2 -NIPAM 0.8 )
[0068] Free radical copolymerization was carried out using APA, AA, and NIPAM monomers: 175 mg APA, 446 mg AA, and 90.53 mg NIPAM were dissolved in 1 mL of deionized water by heating at 60 °C, sonication, and vortexing to achieve a concentration of 0.8 mol / L for APA, 6.2 mol / L for AA, and 0.8 mol / L for NIPAM. After complete dissolution, the mixed solution was cooled to room temperature, and 3.56 mg ammonium persulfate was added as an initiator, along with 1.06 mg N,N,N',N'-tetramethylethylenediamine as an initiator accelerator. After thorough mixing, the mixture was placed in a 60 °C oven and allowed to stand for 3 hours to initially obtain a hydrogel. This hydrogel was then stored in an environment below room temperature to obtain a highly biocompatible, on-demand peelable hydrogel.
[0069] Example 11: P(APA) 0.9 -AA 6.2 -NIPAM 0.8 )
[0070] Free radical copolymerization was carried out using APA, AA, and NIPAM monomers: 197 mg APA, 446 mg AA, and 90.53 mg NIPAM were dissolved in 1 mL of deionized water by heating at 60 °C, sonication, and vortexing to achieve a concentration of 0.9 mol / L for APA, 6.2 mol / L for AA, and 0.8 mol / L for NIPAM. After complete dissolution, the mixed solution was cooled to room temperature, and 3.66 mg ammonium persulfate was added as an initiator, along with 1.10 mg N,N,N',N'-tetramethylethylenediamine as an initiator accelerator. After thorough mixing, the mixture was placed in a 60 °C oven and allowed to stand for 3 hours to initially obtain a hydrogel. This hydrogel was then stored in an environment below room temperature to obtain a highly biocompatible, on-demand peelable hydrogel.
[0071] Example 12: P(AL) 0.7 -AA 6.2 -NIPAM 0.8 )
[0072] Free radical copolymerization was performed using AL, AA, and NIPAM monomers: 100 mg AL, 446 mg AA, and 90.53 mg NIPAM were dissolved in 1 mL of deionized water by heating at 60 °C, sonication, and vortexing to achieve a concentration of 0.7 mol / L for AL, 6.2 mol / L for AA, and 0.8 mol / L for NIPAM. After complete dissolution, the mixed solution was cooled to room temperature, and 3.18 mg ammonium persulfate was added as an initiator, along with 0.95 mg N,N,N',N'-tetramethylethylenediamine as an initiator accelerator. After thorough mixing, the mixture was placed in a 60 °C oven and allowed to stand for 3 hours to initially obtain a hydrogel. This hydrogel was then stored in an environment below room temperature to obtain a highly biocompatible, on-demand peelable hydrogel.
[0073] Example 13: P(AV) 0.7 -AA 6.2 -NIPAM 0.8 )
[0074] Free radical copolymerization was performed using AV, AA, and NIPAM monomers: 120 mg AV, 446 mg AA, and 90.53 mg NIPAM were dissolved in 1 mL of deionized water by heating at 60 °C, sonication, and vortexing, resulting in a concentration of AV of 0.7 mol / L, AA of 6.2 mol / L, and NIPAM of 0.8 mol / L. After complete dissolution, the mixed solution was cooled to room temperature, and 3.28 mg ammonium persulfate was added as an initiator, along with 0.98 mg N,N,N',N'-tetramethylethylenediamine as an initiator accelerator. After thorough mixing, the mixture was placed in a 60 °C oven and allowed to stand for 3 hours to initially obtain a hydrogel. This hydrogel was then stored in an environment below room temperature to obtain a highly biocompatible, on-demand peelable hydrogel.
[0075] Example 14: P(ALE) 0.7 -AA 6.2 -NIPAM 0.8 )
[0076] Free radical copolymerization was performed using ALE, AA, and NIPAM monomers: 130 mg ALE, 446 mg AA, and 90.53 mg NIPAM were dissolved together in 1 mL of deionized water by heating at 60 °C, sonication, and vortexing, so that the concentration of ALE was 0.7 mol / L, the concentration of AA was 6.2 mol / L, and the concentration of NIPAM was 0.8 mol / L. After complete dissolution, the mixed solution was cooled to room temperature, and 3.33 mg ammonium persulfate was added as an initiator, and 0.99 mg N,N,N',N'-tetramethylethylenediamine was added as an initiator accelerator. After mixing evenly, the mixture was placed in a 60 °C oven and allowed to stand for 3 h to initially obtain a hydrogel. The hydrogel was then stored in an environment below room temperature to obtain a peelable hydrogel with high bio-wet tissue adhesion.
[0077] Example 15: P(AIL) 0.7 -AA 6.2 -NIPAM 0.8 )
[0078] Free radical copolymerization was performed using AIL, AA, and NIPAM monomers: 130 mg AIL, 446 mg AA, and 90.53 mg NIPAM were dissolved together in 1 mL of deionized water by heating at 60 °C, sonication, and vortexing, so that the concentration of AIL was 0.7 mol / L, the concentration of AA was 6.2 mol / L, and the concentration of NIPAM was 0.8 mol / L. After complete dissolution, the mixed solution was cooled to room temperature, and 3.33 mg ammonium persulfate was added as an initiator, and 0.99 mg N,N,N',N'-tetramethylethylenediamine was added as an initiator accelerator. After mixing evenly, the mixture was placed in a 60 °C oven and allowed to stand for 3 h to initially obtain a hydrogel. The hydrogel was stored in an environment below room temperature to obtain a peelable hydrogel with high bio-wet tissue adhesion.
[0079] Example 16: P(ATP) 0.7 -AA 6.2 -NIPAM 0.8 )
[0080] Free radical copolymerization was performed using ATP, AA, and NIPAM monomers: 181 mg ATP, 446 mg AA, and 90.53 mg NIPAM were dissolved together in 1 mL of deionized water by heating at 60 °C, sonication, and vortexing to achieve a concentration of 0.7 mol / L for ATP, 6.2 mol / L for AA, and 0.8 mol / L for NIPAM. After complete dissolution, the mixed solution was cooled to room temperature, and 3.59 mg ammonium persulfate was added as an initiator, along with 1.08 mg N,N,N',N'-tetramethylethylenediamine as an initiator promoter. After thorough mixing, the mixture was placed in a 60 °C oven and allowed to stand for 3 hours to initially obtain a hydrogel. This hydrogel was then stored in an environment below room temperature to obtain a highly bioadhesive, on-demand exfoliating hydrogel.
[0081] Example 17: P(APA) 0.7 -MAA 6.2 -NIPAM 0.8 )
[0082] Free radical copolymerization was carried out using APA, MAA, and NIPAM monomers: 153 mg APA, 534 mg MAA, and 90.53 mg NIPAM were dissolved together in 1 mL of deionized water by heating at 60 °C, sonication, and vortexing to achieve a concentration of 0.7 mol / L for APA, 6.2 mol / L for MAA, and 0.8 mol / L for NIPAM. After complete dissolution, the mixed solution was cooled to room temperature, and 4.03 mg ammonium persulfate was added as an initiator, along with 1.20 mg N,N,N',N'-tetramethylethylenediamine as an initiator accelerator. After thorough mixing, the mixture was placed in a 60 °C oven and allowed to stand for 3 hours to initially obtain a hydrogel. This hydrogel was then stored in an environment below room temperature to obtain a highly bioadhesive, on-demand peelable hydrogel.
[0083] Example 18: P(APA) 0.7 -HEAA 6.2 -NIPAM 0.8 )
[0084] Free radical copolymerization was carried out using APA, HEAA, and NIPAM monomers: 153 mg APA, 735 mg HEAA, and 90.53 mg NIPAM were dissolved in 1 mL of deionized water by heating at 60 °C, sonication, and vortexing to achieve a concentration of 0.7 mol / L for APA, 6.2 mol / L for HEAA, and 0.8 mol / L for NIPAM. After complete dissolution, the mixed solution was cooled to room temperature, and 4.89 mg ammonium persulfate was added as an initiator, along with 1.46 mg N,N,N',N'-tetramethylethylenediamine as an initiator accelerator. After thorough mixing, the mixture was placed in a 60 °C oven and allowed to stand for 3 hours to initially obtain a hydrogel. This hydrogel was then stored in an environment below room temperature to obtain a highly biocompatible, on-demand peelable hydrogel.
[0085] Example 19: P(APA) 0.7 -AG 6.2 -NIPAM 0.8 )
[0086] Free radical copolymerization was carried out using APA, AG, and NIPAM monomers: 153 mg APA, 801 mg AG, and 90.53 mg NIPAM were dissolved in 1 mL of deionized water by heating at 60 °C, sonication, and vortexing to achieve a concentration of 0.7 mol / L for APA, 6.2 mol / L for AG, and 0.8 mol / L for NIPAM. After complete dissolution, the mixed solution was cooled to room temperature, and 5.22 mg ammonium persulfate was added as an initiator, along with 1.57 mg N,N,N',N'-tetramethylethylenediamine as an initiator accelerator. After thorough mixing, the mixture was placed in a 60 °C oven and allowed to stand for 3 hours to initially obtain a hydrogel. This hydrogel was then stored in an environment below room temperature to obtain a highly biocompatible, on-demand exfoliating hydrogel.
[0087] Example 19: P(APA) 0.7 -AASP 6.2 -NIPAM 0.8 )
[0088] Free radical copolymerization was carried out using APA, AASP, and NIPAM monomers: 153 mg APA, 1160 mg AASP, and 90.53 mg NIPAM were dissolved together in 1 mL of deionized water by heating at 60 °C, sonication, and vortexing, so that the concentration of APA was 0.7 mol / L, the concentration of AASP was 6.2 mol / L, and the concentration of NIPAM was 0.8 mol / L. After complete dissolution, the mixed solution was cooled to room temperature, and 7.02 mg ammonium persulfate was added as an initiator, and 2.11 mg N,N,N',N'-tetramethylethylenediamine was added as an initiator accelerator. After mixing evenly, the mixture was placed in a 60 °C oven and allowed to stand for 3 h to obtain a preliminary hydrogel. The hydrogel was stored in an environment below room temperature to obtain a peelable hydrogel with high bio-wet tissue adhesion.
[0089] Example 19: P(APA) 0.7 -AA 6.2 -NVCL 0.8 )
[0090] Free radical copolymerization was carried out using APA, AA, and OEGMA monomers: 153 mg APA, 446 mg AA, and 111.38 mg NVCL were dissolved together in 1 mL of deionized water by heating at 60 °C, sonication, and vortexing to achieve a concentration of 0.7 mol / L for APA, 6.2 mol / L for AA, and 0.8 mol / L for NVCL. After complete dissolution, the mixed solution was cooled to room temperature, and 3.55 mg ammonium persulfate was added as an initiator, and 1.07 mg N,N,N',N'-tetramethylethylenediamine was added as an initiator accelerator. After mixing evenly, the mixture was placed in a 60 °C oven and allowed to stand for 3 h to initially obtain a hydrogel. The hydrogel was then stored in an environment below room temperature to obtain a peelable hydrogel with high bio-wet tissue adhesion.
[0091] Example 20: P(APA) 0.7 -AA 6.2 -OEGMA 0.8 )
[0092] Free radical copolymerization was performed using APA, AA, and OEGMA monomers: 153 mg APA, 446 mg AA, and 116.8 mg OEGMA were dissolved together in 1 mL of deionized water by heating at 60 °C, sonication, and vortexing, so that the concentration of APA was 0.7 mol / L, the concentration of AA was 6.2 mol / L, and the concentration of OEGMA was 0.8 mol / L. After complete dissolution, the mixed solution was cooled to room temperature, and 3.58 mg ammonium persulfate was added as an initiator, and 1.07 mg N,N,N',N'-tetramethylethylenediamine was added as an initiator accelerator. After mixing evenly, the mixture was placed in a 60 °C oven and allowed to stand for 3 h to initially obtain a hydrogel. The hydrogel was stored in an environment below room temperature to obtain a peelable hydrogel with high bio-wet tissue adhesion.
[0093] Effect test:
[0094] Figure 1 The wet bonding strength of the hydrogel provided in Example 5 with pigskin at different temperatures was demonstrated. The wet bonding strength gradually increased with increasing temperature. Its wet bonding strength reached as high as 70 kPa, which is significantly superior to other hydrogel patches (Adv. Mater. 2023, 35, 2209606; Adv. Funct. Mater. 2024, 34, 2401030).
[0095] Figure 2 The hydrogel provided in Example 5 demonstrated strong wet adhesion strength and rapid and efficient switching efficiency with different porcine tissues (including liver, lungs, heart, stomach, arteries, and skin).
[0096] Figure 3 The rheological test graph of the hydrogel modulus provided in Example 5 as a function of temperature is shown. The results show that there is a sudden decrease in the hydrogel modulus near 37°C, indicating that phase separation is released at this time. The decrease in modulus further confirms that the hydrogel releases phase separation at temperatures close to skin temperature.
[0097] Figure 4 The low-field NMR test results of the hydrogels provided in Examples 1, 2, 3, 4, 5, 6, and 7 are shown. The figures indicate that as the content of hydrophilic monomers decreases and the content of thermosensitive monomers increases, the internal hydrogen bond strength increases, making phase separation more likely. These results demonstrate that the hydrogels provided by this invention possess stable and durable on-demand peeling properties.
[0098] The on-demand peelable hydrogel with high biocompatibility prepared by this invention has good biocompatibility, is made from inexpensive and readily available raw materials, has excellent mechanical properties, and has the characteristics of rapid and firm wet adhesion to tissues while being able to be gently peeled off as needed. It has important clinical significance and practical value for emergency injury treatment, and provides a new option for replacing surgical sutures to achieve wound closure and rapid hemostasis in clinical practice.
Claims
1. A highly biocompatible, on-demand peelable hydrogel, characterized in that, The hydrogel was prepared by free radical polymerization of hydrophobic amino acid vinyl monomers, hydrophilic monomers, and thermosensitive monomers. The hydrophobic amino acid vinyl monomer is selected from one or more of N-acryloylalanine, N-acryloylvaline, N-acryloylphenylalanine, N-acryloylleucine, N-acryloylisoleucine, N-acryloyltryptophan, N-acryloylmethionine, N-acryloylalanamide, N-acryloylvaline, and N-acryloylphenylalanamide; The hydrophilic monomer is selected from one or more of acrylic acid, methacrylic acid, 2-hydroxyethyl acrylate, hydroxyethyl methacrylate, acrylamide, N-trimethylolmethacrylamide, N,N-dimethylacrylamide, N-hydroxyethylacrylamide, 1-vinyl-2-pyrrolidone, N-acryloylaspartic acid, N-acryloylglutamic acid, N-acryloylglycine, N-acryloyltyrosine, N-acryloylserine, N-acryloylthreonine, and N-acryloylglutamine. The thermosensitive monomer is selected from N-isopropylacrylamide, polyethylene glycol methyl ether methacrylate, N-vinylcaprolactam, and 2-(2-methoxyethoxy)ethyl methacrylate. This hydrogel can be gently peeled off as needed in response to temperature stimuli.
2. The on-demand peelable hydrogel with high bio-wet tissue adhesion as described in claim 1, characterized in that, The ratio of structural units between the hydrophobic amino acid vinyl monomer, the hydrophilic monomer, and the thermosensitive monomer is 1: (9~13): (0.5~2).
3. The method for preparing the on-demand peelable hydrogel with high bio-wet tissue adhesion as described in claim 1 or 2, characterized in that, The method includes the following steps: S1. Dissolve the hydrophobic amino acid vinyl monomer, hydrophilic monomer and thermosensitive monomer fully in an aqueous solution to obtain a colorless and transparent mixture. S2. At room temperature, an initiator and an initiator accelerator are added to the mixture and mixed evenly to complete free radical polymerization and obtain a polymer. S3. The polymer is stored in an environment below room temperature to obtain the on-demand peelable hydrogel with high bio-wet tissue adhesion.
4. The method for preparing the on-demand peelable hydrogel with high bio-wet tissue adhesion as described in claim 3, characterized in that, The total concentration of the hydrophobic amino acid vinyl monomer and the hydrophilic monomer is 6.7~7.7 M, wherein the concentration ratio of the hydrophobic amino acid vinyl monomer to the hydrophilic monomer is 0.7~6:7; The concentration of the thermosensitive monomer is 0.2~1.0 mol / L.
5. The method for preparing the on-demand peelable hydrogel with high bio-wet tissue adhesion as described in claim 4, characterized in that, The initiator is selected from one or more of potassium persulfate, ammonium persulfate, and azobisisobutyrazoline hydrochloride; The initiator / promoter is N,N,N',N'-tetramethylethylenediamine.
6. The method for preparing the on-demand peelable hydrogel with high bio-wet tissue adhesion as described in claim 4, characterized in that, The amount of the initiator added is 0.5% to 2% of the total mass of the hydrophobic amino acid vinyl monomer, the hydrophilic monomer, and the thermosensitive monomer; The amount of the initiator accelerator added is between 0% and 30% of the initiator mass.
7. The method for preparing the on-demand peelable hydrogel with high bio-wet tissue adhesion as described in claim 4, characterized in that, In step S1, the method of complete dissolution is selected from one or more of heating, ultrasonication, and vortex oscillation; In step S2, the temperature for free radical polymerization is 20~80 ℃, and the reaction time is 2~12 h.
8. The application of the on-demand peelable hydrogel with high bio-wet tissue adhesion as described in claim 1 or 2 in the preparation of wound closure and rapid hemostasis materials.
Citation Information
Patent Citations
Temperature-sensitive debonding wet tissue adhesion hydrogel and preparation method thereof
CN114644766A
Biological tissue adhesive capable of being instantly adhered when encountering water and preparation method of biological tissue adhesive