Method for efficiently and selectively extracting vanadium from vanadium shale
By adjusting the pH value of the vanadium shale acid leachate and optimizing the extraction process, the problems of low vanadium leaching rate and low purity of vanadium pentoxide in the vanadium shale extraction process were solved, and efficient and selective preparation of vanadium pentoxide and high-purity vanadium pentoxide were achieved.
Patent Information
- Application Number
- CN202510877362.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-06-27
- Publication Date
- 2025-08-29
AI Technical Summary
In the existing vanadium shale extraction process, the vanadium leaching rate is low, the concentration of impurity iron ion, the vanadium loss is not used in neutralization slag, the extraction efficiency is low and the purity of vanadium pentoxide product is low.
By adjusting the pH value of the vanadium shale acid leach solution to 2.5~3.5, using vanadium re-extraction in neutralization slag, combining extraction agent and countercurrent extraction technology, optimizing the extraction series and hydrothermal vanadium sink process, controlling the precipitation of impurity iron ions, and preparing high-purity vanadium pentoxide.
The vanadium leaching rate is as high as 92%, the concentration of impurity iron ions is reduced, and the purity of vanadium pentoxide product exceeds 99.20%, which strengthens the extraction efficiency of vanadium ions and shortens the extraction series.
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of extracting vanadium from vanadium shale, and specifically relates to a method for efficiently and selectively extracting vanadium from vanadium shale. Background Art
[0002] Vanadium shale is a significant vanadium resource in my country and a key raw material for the production of high-end vanadium-based materials and high-performance vanadium electrolytes. With the explosive growth of all-vanadium liquid flow energy storage and the accelerated development of downstream high-end manufacturing, the overall demand for high-purity vanadium has surged. The development of technologies to produce high-purity vanadium products is crucial to the sustainable development of the vanadium industry chain. The vanadium-containing acid leachate obtained by acid leaching of vanadium shale contains high concentrations of impure iron ions. This precipitation of iron ions leads to vanadium loss, hindering the selective enrichment of vanadium ions from the organic phase during the extraction process and reducing the purity of the vanadium pentoxide product. Therefore, achieving efficient and selective vanadium extraction from vanadium shale to produce high-purity vanadium pentoxide has attracted widespread attention from those skilled in the art.
[0003] The patented technology "A two-stage leaching process for vanadium extraction from stone coal using concentrated acid" (CN 115354173 A) involves mixing stone coal with concentrated sulfuric acid and reacting them at 150-300°C for 1-6 hours. The filtrate is then purified and enriched after pH adjustment and pretreatment, and vanadium is precipitated to produce a refined vanadium product. The vanadium leaching rate in this process is only 80-86%, and the vanadium recovery rate is 78-84%. Liu Daxue et al. (Liu Daxue, Li Yanjiang, Chang Yaochao, et al. Scale-up test of direct sulfuric acid leaching process for stone coal vanadium ore [J]. Mining and Metallurgy, 2013, 22(4):60-66.) adopted a staged leaching process for stone coal vanadium ore, achieving a vanadium leaching rate of 86%. The vanadium concentration in the leachate was 2.12 g / L and the impurity iron concentration was 11.32 g / L, which was 5.3 times the vanadium concentration. Huang Yunsheng et al. (Huang Yunsheng, Wu Haiying, Dai Zilin, et al. Study on the separation of vanadium and iron in the acid leaching solution of a stone coal vanadium mine in Shaanxi Province [J]. Mining and Metallurgical Engineering, 2013, 33(4): 104-107.) used a multi-stage sulfuric acid leaching method to separate vanadium and iron from the leaching solution. After pretreatment, the concentration of impurity iron in the raw extract was more than three times the concentration of vanadium. Fu Chaoyang et al. (Fu Chaoyang, Zhang Yimin, Liu Tao, et al. Effect of impurity ions in the stripping solution of stone coal vanadium extraction on vanadium precipitation with acidic ammonium salt [J]. Rare Metals, 2016, 40(10): 1060-1065.) found that when the impurity Fe ion in the vanadium-rich solution was too high, the purity of the prepared vanadium pentoxide was less than 98.00%. The above research shows that in the current vanadium shale extraction process, the vanadium leaching rate needs to be further improved and the selective separation effect of vanadium and iron needs to be strengthened. The concentration of impurity iron in the acid leaching solution obtained by current technology is several times the concentration of vanadium, which seriously affects the separation index of vanadium and iron in the extraction process and reduces the purity of the vanadium product prepared by the vanadium precipitation process.
[0004] Acidic phosphorus extractants are well-established for separating and purifying vanadium from impure iron in industrial production solutions. The initial pH of vanadium shale acid leachate is typically 0.1-0.8, and current acidic phosphorus extractants generally control the pH of vanadium extraction to around 1.8-2.5. The patented technology, "A Method for Separating Iron and Vanadium from Vanadium Acid Leachate" (CN 106086408 A), treats vanadium acid leachate with an initial pH less than 1. Lime milk is used to adjust the pH of the vanadium-containing solution to 1.0-2.5 before extraction. This separation of vanadium from impurities occurs in four to five stages of positive extraction. Research by Zheng Qiaoqiao et al. (Qiaoqiao Zheng, YiminZhang, Shenxu Bao, et al. Effects of different alkalis on the behavior of vanadium loss in the pretreatment of vanadium-bearing acid leaching solution[J]. Science Asia, 2019, 45:43-49.) shows that the initial pH of the vanadium-containing acid leaching solution is 0.33. Using lime milk to adjust the pH to 2.0 produces neutralized slag. During pH adjustment, iron ions hydrolyze to form colloidal precipitates and highly viscous calcium sulfate, which carry over some vanadium ions from the leaching solution, leading to vanadium loss in the neutralized slag. The patented technology, "A leaching process for stone-coal vanadium ore with residual acid recovery" (CN 104988337A), pre-treats the tailings from the wet vanadium extraction process directly into a tailings pond. This results in the loss of vanadium carried over into the neutralized slag without recycling.
[0005] In summary, the existing vanadium shale extraction process has prominent problems such as low vanadium leaching rate, high concentration of impurity iron ions in the leachate, ineffective utilization of vanadium lost in neutralization slag, low extraction efficiency and low purity of vanadium pentoxide product. Summary of the Invention
[0006] The present invention aims to overcome the defects of the prior art and aims to provide a method for highly efficient and selective extraction of vanadium from vanadium shale. The method can re-extract and utilize vanadium in the neutralized slag, obtain a high vanadium leaching rate, enhance the extraction efficiency of vanadium ions in the extraction process, shorten the extraction stage, and produce high-purity vanadium pentoxide.
[0007] To achieve the above object, the specific steps of the technical solution adopted by the present invention are: Step 1: Sulfuric acid solution I and vanadium shale powder are mixed at a liquid-solid ratio of 0.7-1.5:1 L / kg to obtain a mixed slurry; then, the leaching aid is added to the mixed slurry at a mass ratio of the leaching aid to the vanadium shale powder of 0.015-0.06:1, the slurry is adjusted, stirred for the first time, and solid-liquid separation is performed to obtain a vanadium-containing leachate and a leaching residue.
[0008] Step 2: adding sodium sulfite to the vanadium-containing leachate at a molar ratio of sodium sulfite to vanadium in the vanadium-containing leachate of 0.28-0.45:1, stirring for a second time to obtain a reduced solution; adjusting the pH value of the reduced solution to 2.5-3.5 with calcium hydroxide, and performing solid-liquid separation to obtain an extract solution and a neutralized residue.
[0009] The neutralized slag obtained in this operation is kept until step 1 of the next operation and is directly mixed with the mixed slurry after the leaching agent is added.
[0010] Step 3: Mix the extracted organic phase and the extracted stock solution at a volume ratio of 1:1-4, and perform countercurrent extraction at 25-30° C. to obtain a loaded organic phase.
[0011] The loaded organic phase and the sulfuric acid solution II are mixed at a volume ratio of 4-10:1, and countercurrent stripping is performed at 25-30° C. to obtain a vanadium-rich solution.
[0012] Step 4: adding the sodium chlorate to the vanadium-rich solution at a molar ratio of sodium chlorate to vanadium in the vanadium-rich solution of 0.25-0.55:1, stirring for a third time to obtain an oxidized solution; adjusting the pH value of the oxidized solution to 1.8-2.2 with aqueous ammonia, performing a hydrothermal reaction, and performing solid-liquid separation to obtain a vanadium precipitation mother liquor and a vanadium precipitation intermediate product.
[0013] The vanadium precipitation intermediate product is calcined at 500-550° C. in air for 1-2 hours to obtain vanadium pentoxide.
[0014] The preparation method of the vanadium shale ore powder is as follows: crushing the vanadium shale, grinding the ore until the particle size is less than 0.074 mm, accounting for 45-80%, to obtain the vanadium shale ore powder.
[0015] The sulfuric acid concentration of the sulfuric acid solution I is 2.0-6.2 mol / L.
[0016] The leaching aid is calcium fluoride or sodium fluoride.
[0017] The stirring is: The first stirring in step 1 is: stirring at 80-95° C. for 5-15 hours; The second stirring in step 2 is: stirring at 50-70° C. for 10-30 minutes; The third stirring in step 4 is: stirring at 50-80° C. for 20-40 minutes.
[0018] The extraction organic phase is a mixture of 10-20 vol% of an extractant and 80-90 vol% of sulfonated kerosene; the extractant is di(2-ethylhexyl) phosphate or 2-ethylhexylphosphonic acid mono-2-ethylhexyl ester.
[0019] The concentration of the sulfuric acid solution II is 1.2-2.5 mol / L.
[0020] The number of stages of the countercurrent forward extraction is 2 to 3, and the single-stage reaction time of the countercurrent forward extraction is 7 to 15 minutes.
[0021] The number of stages of the countercurrent stripping is 3 to 5, and the single-stage reaction time of the countercurrent stripping is 5 to 15 minutes.
[0022] The conditions of the hydrothermal reaction are: the hydrothermal reaction temperature is 85-95° C., and the hydrothermal reaction time is 1-2 hours.
[0023] Due to the adoption of the above technical solution, the present invention has the following positive effects compared with the prior art: (1) The prior art uses sulfuric acid wet leaching for vanadium shale. The initial pH value of the vanadium-containing leachate is 0.1-0.8. The suitable pH value for vanadium ion extraction by acidic phosphorus extractants is 1.8-2.5. The positive extraction reaction is that vanadium ions exchange ions with hydrogen atoms on phosphorus hydroxyl groups and adsorb on the extractant molecules. The hydrogen ions are released from the extractant and transferred to the aqueous phase, which reduces the pH value of the aqueous phase to 1.0-1.5. The extraction reaction of vanadium ions is inhibited, reducing the extraction efficiency. The present invention adjusts the pH value of the vanadium shale acid leachate to 2.5-3.5 by adding alkali, so that the pH value of the aqueous phase in the positive extraction process is stabilized in the range of 2.0-2.5, ensuring that the exchange reaction between vanadium ions and extractant groups is always in the appropriate pH range. The positive extraction stage is significantly shortened to 2-3 stages, achieving the goal of efficient extraction of vanadium ions in the extraction stock solution.
[0024] (2) After the vanadium-containing leachate of vanadium shale is reduced, a reduced liquid is obtained. During the process of adjusting the pH value of the reduced liquid with alkali, a neutralized slag (whose main components are calcium sulfate and colloidal precipitate) is produced. During the pH value change of the reduced liquid, the iron ions undergo hydrolysis reaction to produce ferrous hydroxide precipitate, which is converted into ferric hydroxide colloidal precipitate when it comes into contact with air during the stirring process. At the same time, the calcium ions combine with sulfate to produce an emulsion of calcium sulfate. As the lime concentration increases, the calcium sulfate agglomerates to form a gypsum precipitate with a certain viscosity. The vanadate ions in the reduced liquid are carried to the neutralized slag in an adsorbed state and lost. The present invention utilizes the property that the adsorbed vanadium ions in the neutralized slag are easily soluble in acid. The neutralized slag generated by adjusting the pH value of the reduced liquid is returned to the mixed slurry for leaching. The acidity and temperature environment of the leaching slurry are fully utilized to re-extract the vanadium in the neutralized slag. This overcomes the current disadvantage that the vanadium in the neutralized slag is not recycled, and achieves efficient extraction of vanadium with a vanadium leaching rate of more than 92%.
[0025] (3) The ratio of the concentration of impurity iron ions to the concentration of vanadium ions in the vanadium-containing leachate obtained by the prior art is greater than 3. After extraction, a vanadium-rich solution is obtained. When hydrothermal vanadium precipitation is performed at a pH of about 2.0, iron ions, as typical impurity ions, are easily precipitated into the vanadium product, reducing the purity of the vanadium pentoxide product. Therefore, controlling and reducing the concentration of impurity iron in the vanadium-containing solution from the source is an important way to obtain a high-purity vanadium pentoxide product. The present invention adjusts the pH value of the vanadium-containing leachate to 2.5-3.5, and the impurity iron ions in the solution are fully precipitated and solidified into the neutralized slag. The ratio of the mass concentration of impurity iron ions to the mass concentration of vanadium ions in the vanadium-containing solution (extracted stock solution) is reduced to below 0.4, effectively reducing the concentration of impurity iron ions in the vanadium-containing solution from the source, avoiding the co-precipitation of impurity ions with vanadium and reducing the purity of the vanadium product, and achieving deep separation of vanadium and impurity ions from the source. The purity of the prepared vanadium pentoxide product is greater than 99.20%.
[0026] According to the present invention, the vanadium leaching rate is 92.52-94.11%, the ratio of the mass concentration of iron ions to the mass concentration of vanadium ions in the extraction solution is 0.22-0.35, and the purity of the prepared vanadium pentoxide product is 99.25-99.85%.
[0027] Therefore, the present invention has the characteristics of being able to re-extract and utilize vanadium in the neutralized slag, obtaining a high vanadium leaching rate, enhancing the extraction efficiency of vanadium ions, shortening the extraction stages, obtaining a low concentration of impure iron in the extracted stock solution, and preparing high-purity vanadium pentoxide. DETAILED DESCRIPTION
[0028] The present invention is further described below in conjunction with specific embodiments, which does not limit its scope of protection: A method for efficiently and selectively extracting vanadium from vanadium shale. The steps of the method described in this embodiment are: Step 1: Sulfuric acid solution I and vanadium shale powder are mixed at a liquid-solid ratio of 0.7-1.5:1 L / kg to obtain a mixed slurry; then, the leaching aid is added to the mixed slurry at a mass ratio of the leaching aid to the vanadium shale powder of 0.015-0.06:1, the slurry is adjusted, stirred for the first time, and solid-liquid separation is performed to obtain a vanadium-containing leachate and a leaching residue.
[0029] Step 2: adding sodium sulfite to the vanadium-containing leachate at a molar ratio of sodium sulfite to vanadium in the vanadium-containing leachate of 0.28-0.45:1, stirring for a second time to obtain a reduced solution; adjusting the pH value of the reduced solution to 2.5-3.5 with calcium hydroxide, and performing solid-liquid separation to obtain an extract solution and a neutralized residue.
[0030] The neutralized slag obtained in this operation is kept until step 1 of the next operation and is directly mixed with the mixed slurry after the leaching agent is added.
[0031] Step 3: Mix the extracted organic phase and the extracted stock solution at a volume ratio of 1:1-4, and perform countercurrent extraction at 25-30° C. to obtain a loaded organic phase.
[0032] The loaded organic phase and the sulfuric acid solution II are mixed at a volume ratio of 4-10:1, and countercurrent stripping is performed at 25-30° C. to obtain a vanadium-rich solution.
[0033] Step 4: adding the sodium chlorate to the vanadium-rich solution at a molar ratio of sodium chlorate to vanadium in the vanadium-rich solution of 0.25-0.55:1, stirring for a third time to obtain an oxidized solution; adjusting the pH value of the oxidized solution to 1.8-2.2 with aqueous ammonia, performing a hydrothermal reaction, and performing solid-liquid separation to obtain a vanadium precipitation mother liquor and a vanadium precipitation intermediate product.
[0034] The vanadium precipitation intermediate product is calcined at 500-550° C. in air for 1-2 hours to obtain vanadium pentoxide.
[0035] The preparation method of the vanadium shale ore powder is as follows: crushing the vanadium shale, grinding the ore until the particle size is less than 0.074 mm, accounting for 45-80%, to obtain the vanadium shale ore powder.
[0036] The sulfuric acid concentration of the sulfuric acid solution I is 2.0-6.2 mol / L.
[0037] The leaching aid is calcium fluoride or sodium fluoride.
[0038] The stirring is: The first stirring in step 1 is: stirring at 80-95° C. for 5-15 hours; The second stirring in step 2 is: stirring at 50-70° C. for 10-30 minutes; The third stirring in step 4 is: stirring at 50-80° C. for 20-40 minutes.
[0039] The extraction organic phase is a mixture of 10-20 vol% of an extractant and 80-90 vol% of sulfonated kerosene; the extractant is di(2-ethylhexyl) phosphate or 2-ethylhexylphosphonic acid mono-2-ethylhexyl ester.
[0040] The concentration of the sulfuric acid solution II is 1.2-2.5 mol / L.
[0041] The number of stages of the countercurrent forward extraction is 2 to 3, and the single-stage reaction time of the countercurrent forward extraction is 7 to 15 minutes.
[0042] The number of stages of the countercurrent stripping is 3 to 5, and the single-stage reaction time of the countercurrent stripping is 5 to 15 minutes.
[0043] The conditions of the hydrothermal reaction are: the hydrothermal reaction temperature is 85-95° C., and the hydrothermal reaction time is 1-2 hours.
[0044] Example 1 A method for efficiently and selectively extracting vanadium from vanadium shale. The steps of the method described in this embodiment are: Step 1: Sulfuric acid solution I and vanadium shale powder are mixed at a liquid-solid ratio of 1.5:1 L / kg to obtain a mixed slurry; then, the leaching aid is added to the mixed slurry at a mass ratio of the leaching aid to the vanadium shale powder of 0.015:1, the slurry is adjusted, stirred for the first time, and the solid-liquid is separated to obtain a vanadium-containing leachate and a leaching residue.
[0045] Step 2: adding sodium sulfite to the vanadium-containing leachate at a molar ratio of sodium sulfite to vanadium in the vanadium-containing leachate of 0.45:1, stirring for a second time to obtain a reduced solution; adjusting the pH value of the reduced solution to 2.5 with calcium hydroxide, and performing solid-liquid separation to obtain an extract solution and a neutralized residue.
[0046] The neutralized slag obtained in this operation is kept until step 1 of the next operation and is directly mixed with the mixed slurry after the leaching agent is added.
[0047] Step 3: Mix the extracted organic phase and the extracted stock solution at a volume ratio of 1:1, and perform countercurrent extraction at 25° C. to obtain a loaded organic phase.
[0048] The loaded organic phase and the sulfuric acid solution II were mixed at a volume ratio of 10:1, and countercurrent stripping was performed at 25° C. to obtain a vanadium-rich solution.
[0049] Step 4: adding sodium chlorate to the vanadium-rich solution at a molar ratio of sodium chlorate to vanadium in the vanadium-rich solution of 0.45:1, stirring for a third time to obtain an oxidized solution; adjusting the pH value of the oxidized solution to 2.0 with aqueous ammonia, performing a hydrothermal reaction, and performing solid-liquid separation to obtain a vanadium precipitation mother liquor and a vanadium precipitation intermediate product.
[0050] The vanadium precipitation intermediate product is calcined at 550° C. in air for 2 hours to obtain vanadium pentoxide.
[0051] The preparation method of the vanadium shale ore powder is as follows: crushing the vanadium shale, grinding the ore until the particle size is less than 0.074 mm, accounting for 45%, to obtain the vanadium shale ore powder.
[0052] The sulfuric acid concentration of the sulfuric acid solution I is 3.5 mol / L.
[0053] The leaching aid is calcium fluoride.
[0054] The stirring is: The first stirring in step 1 is: stirring at 95° C. for 8 h; The second stirring in step 2 is: stirring at 60° C. for 30 min; The third stirring in step 4 is: stirring at 50° C. for 40 minutes.
[0055] The extraction organic phase is a mixture of 20 vol% of an extractant and 80 vol% of sulfonated kerosene; the extractant is di(2-ethylhexyl) phosphate.
[0056] The concentration of the sulfuric acid solution II is 1.2 mol / L.
[0057] The number of stages of the countercurrent forward extraction is 2, and the single-stage reaction time of the countercurrent forward extraction is 10 minutes.
[0058] The number of stages of the countercurrent stripping is 3, and the single-stage reaction time of the countercurrent stripping is 10 minutes.
[0059] The conditions of the hydrothermal reaction are: the hydrothermal reaction temperature is 95° C., and the hydrothermal reaction time is 1 hour.
[0060] According to the test results of this embodiment, the vanadium leaching rate was 92.52%, the ratio of the mass concentration of iron ions to the mass concentration of vanadium ions in the extraction solution was 0.35, and the purity of the prepared vanadium pentoxide product was 99.25%.
[0061] Example 2 A method for efficiently and selectively extracting vanadium from vanadium shale. The steps of the method described in this embodiment are: Step 1: Sulfuric acid solution I and vanadium shale powder are mixed at a liquid-solid ratio of 1.2:1 L / kg to obtain a mixed slurry; then, the leaching aid is added to the mixed slurry at a mass ratio of the leaching aid to the vanadium shale powder of 0.045:1, the slurry is adjusted, stirred for the first time, and the solid-liquid is separated to obtain a vanadium-containing leachate and a leaching residue.
[0062] Step 2: adding sodium sulfite to the vanadium-containing leachate at a molar ratio of sodium sulfite to vanadium in the vanadium-containing leachate of 0.35:1, stirring for a second time to obtain a reduced solution; adjusting the pH value of the reduced solution to 3.5 with calcium hydroxide, and performing solid-liquid separation to obtain an extract solution and a neutralized residue.
[0063] The neutralized slag obtained in this operation is kept until step 1 of the next operation and is directly mixed with the mixed slurry after the leaching agent is added.
[0064] Step 3: Mix the extracted organic phase and the extracted stock solution at a volume ratio of 1:2, and perform countercurrent extraction at 27° C. to obtain a loaded organic phase.
[0065] The loaded organic phase and the sulfuric acid solution II were mixed at a volume ratio of 8:1, and countercurrent stripping was performed at 27° C. to obtain a vanadium-rich solution.
[0066] Step 4: adding sodium chlorate to the vanadium-rich solution at a molar ratio of sodium chlorate to vanadium in the vanadium-rich solution of 0.55:1, stirring for a third time to obtain an oxidized solution; adjusting the pH value of the oxidized solution to 2.2 with aqueous ammonia, performing a hydrothermal reaction, and performing solid-liquid separation to obtain a vanadium precipitation mother liquor and a vanadium precipitation intermediate product.
[0067] The vanadium precipitation intermediate product is calcined at 520° C. in air for 1.8 hours to obtain vanadium pentoxide.
[0068] The preparation method of the vanadium shale ore powder is as follows: crushing the vanadium shale, grinding the ore until the particle size is less than 0.074 mm, accounting for 55%, to obtain the vanadium shale ore powder.
[0069] The sulfuric acid concentration of the sulfuric acid solution I is 5.0 mol / L.
[0070] The leaching aid is sodium fluoride.
[0071] The stirring is: The first stirring in step 1 is: stirring at 90° C. for 12 h; The second stirring in step 2 is: stirring at 70° C. for 20 min; The third stirring in step 4 is: stirring at 60° C. for 35 minutes.
[0072] The extraction organic phase is a mixture of 18 vol% of an extractant and 82 vol% of sulfonated kerosene; the extractant is 2-ethylhexylphosphonic acid mono-2-ethylhexyl ester.
[0073] The concentration of the sulfuric acid solution II is 1.8 mol / L.
[0074] The number of stages of the countercurrent forward extraction is 3, and the single-stage reaction time of the countercurrent forward extraction is 15 minutes.
[0075] The number of stages of the countercurrent stripping is 4, and the single-stage reaction time of the countercurrent stripping is 15 minutes.
[0076] The conditions of the hydrothermal reaction are: the hydrothermal reaction temperature is 90° C., and the hydrothermal reaction time is 1.5 h.
[0077] According to the test results of this embodiment, the vanadium leaching rate was 94.11%, the ratio of the mass concentration of iron ions to the mass concentration of vanadium ions in the extraction solution was 0.25, and the purity of the prepared vanadium pentoxide product was 99.85%.
[0078] Example 3 A method for efficiently and selectively extracting vanadium from vanadium shale. The steps of the method described in this embodiment are: Step 1: Sulfuric acid solution I and vanadium shale powder are mixed at a liquid-solid ratio of 1.0:1 L / kg to obtain a mixed slurry; then, the leaching aid is added to the mixed slurry at a mass ratio of the leaching aid to the vanadium shale powder of 0.03:1, the slurry is adjusted, stirred for the first time, and the solid-liquid is separated to obtain a vanadium-containing leachate and a leaching residue.
[0079] Step 2: adding sodium sulfite to the vanadium-containing leachate at a molar ratio of sodium sulfite to vanadium in the vanadium-containing leachate of 0.28:1, stirring for a second time to obtain a reduced solution; adjusting the pH value of the reduced solution to 3.0 with calcium hydroxide, and performing solid-liquid separation to obtain an extract solution and a neutralized residue.
[0080] The neutralized slag obtained in this operation is kept until step 1 of the next operation and is directly mixed with the mixed slurry after the leaching agent is added.
[0081] Step 3: Mix the extracted organic phase and the extracted stock solution at a volume ratio of 1:4, and perform countercurrent extraction at 30° C. to obtain a loaded organic phase.
[0082] The loaded organic phase and the sulfuric acid solution II were mixed at a volume ratio of 4:1, and countercurrent stripping was performed at 30° C. to obtain a vanadium-rich solution.
[0083] Step 4: adding sodium chlorate to the vanadium-rich solution at a molar ratio of sodium chlorate to vanadium in the vanadium-rich solution of 0.35:1, stirring for a third time to obtain an oxidized solution; adjusting the pH value of the oxidized solution to 1.9 with aqueous ammonia, performing a hydrothermal reaction, and performing solid-liquid separation to obtain a vanadium precipitation mother solution and a vanadium precipitation intermediate product.
[0084] The vanadium precipitation intermediate product is calcined at 510° C. in air for 1.5 hours to obtain vanadium pentoxide.
[0085] The preparation method of the vanadium shale ore powder is as follows: crushing the vanadium shale, grinding the ore until the particle size is less than 0.074 mm, accounting for 65%, to obtain the vanadium shale ore powder.
[0086] The sulfuric acid concentration of the sulfuric acid solution I is 2.0 mol / L.
[0087] The leaching aid is calcium fluoride.
[0088] The stirring is: The first stirring in step 1 is: stirring at 85° C. for 5 h; The second stirring in step 2 is: stirring at 50° C. for 10 min; The third stirring in step 4 is: stirring at 70° C. for 25 minutes.
[0089] The extraction organic phase is a mixture of 10 vol% of an extractant and 90 vol% of sulfonated kerosene; the extractant is di(2-ethylhexyl) phosphate.
[0090] The concentration of the sulfuric acid solution II is 2.1 mol / L.
[0091] The number of stages of the countercurrent forward extraction is 3, and the single-stage reaction time of the countercurrent forward extraction is 8 minutes.
[0092] The number of stages of the countercurrent stripping is 4, and the single-stage reaction time of the countercurrent stripping is 12 minutes.
[0093] The conditions of the hydrothermal reaction are: the hydrothermal reaction temperature is 85° C., and the hydrothermal reaction time is 2 h.
[0094] According to the test results of this embodiment, the vanadium leaching rate was 93.85%, the ratio of the mass concentration of iron ions to the mass concentration of vanadium ions in the extraction solution was 0.30, and the purity of the prepared vanadium pentoxide product was 99.72%.
[0095] Example 4 A method for efficiently and selectively extracting vanadium from vanadium shale. The steps of the method described in this embodiment are: Step 1: Sulfuric acid solution I is mixed with vanadium shale powder at a liquid-solid ratio of 0.7:1 L / kg to obtain a mixed slurry; then, the leaching aid is added to the mixed slurry at a mass ratio of the leaching aid to the vanadium shale powder of 0.06:1, the slurry is adjusted, stirred for the first time, and the solid-liquid is separated to obtain a vanadium-containing leachate and a leaching residue.
[0096] Step 2: adding sodium sulfite to the vanadium-containing leachate at a molar ratio of sodium sulfite to vanadium in the vanadium-containing leachate of 0.40:1, stirring for a second time to obtain a reduced solution; adjusting the pH value of the reduced solution to 3.2 with calcium hydroxide, and performing solid-liquid separation to obtain an extract solution and a neutralized residue.
[0097] The neutralized slag obtained in this operation is kept until step 1 of the next operation and is directly mixed with the mixed slurry after the leaching agent is added.
[0098] Step 3: Mix the extracted organic phase and the extracted stock solution at a volume ratio of 1:3, and perform countercurrent extraction at 28° C. to obtain a loaded organic phase.
[0099] The loaded organic phase and the sulfuric acid solution II were mixed at a volume ratio of 6:1, and countercurrent stripping was performed at 29° C. to obtain a vanadium-rich solution.
[0100] Step 4: adding sodium chlorate to the vanadium-rich solution at a molar ratio of sodium chlorate to vanadium in the vanadium-rich solution of 0.25:1, stirring for a third time to obtain an oxidized solution; adjusting the pH value of the oxidized solution to 1.8 with aqueous ammonia, performing a hydrothermal reaction, and performing solid-liquid separation to obtain a vanadium precipitation mother liquor and a vanadium precipitation intermediate product.
[0101] The vanadium precipitation intermediate product is calcined at 500° C. in air for 1 hour to obtain vanadium pentoxide.
[0102] The preparation method of the vanadium shale ore powder is as follows: crushing the vanadium shale, grinding the ore until the particle size is less than 0.074 mm, accounting for 80%, to obtain the vanadium shale ore powder.
[0103] The sulfuric acid concentration of the sulfuric acid solution I is 6.2 mol / L.
[0104] The leaching aid is sodium fluoride.
[0105] The stirring is: The first stirring in step 1 is: stirring at 80° C. for 15 h; The second stirring in step 2 is: stirring at 55° C. for 15 minutes; The third stirring in step 4 is: stirring at 80° C. for 20 minutes.
[0106] The extraction organic phase is a mixture of 15 vol% of an extractant and 85 vol% of sulfonated kerosene; the extractant is 2-ethylhexylphosphonic acid mono-2-ethylhexyl ester.
[0107] The concentration of the sulfuric acid solution II is 2.5 mol / L.
[0108] The number of stages of the countercurrent forward extraction is 2, and the single-stage reaction time of the countercurrent forward extraction is 7 minutes.
[0109] The number of stages of the countercurrent stripping is 5, and the single-stage reaction time of the countercurrent stripping is 5 minutes.
[0110] The conditions of the hydrothermal reaction are: the hydrothermal reaction temperature is 93° C., and the hydrothermal reaction time is 1.8 h.
[0111] According to the test results of this embodiment, the vanadium leaching rate was 93.66%, the ratio of the mass concentration of iron ions to the mass concentration of vanadium ions in the extraction solution was 0.22, and the purity of the prepared vanadium pentoxide product was 99.68%.
[0112] Compared with the prior art, this embodiment has the following positive effects: (1) The prior art uses sulfuric acid wet leaching for vanadium shale. The initial pH value of the vanadium-containing leachate is 0.1-0.8. The suitable pH value for vanadium ion extraction by acidic phosphorus extractants is 1.8-2.5. The positive extraction reaction is that vanadium ions exchange ions with hydrogen atoms on phosphorus hydroxyl groups and adsorb on the extractant molecules. The hydrogen ions are released from the extractant and transferred to the aqueous phase, which reduces the pH value of the aqueous phase to 1.0-1.5. The extraction reaction of vanadium ions is inhibited, which reduces the extraction efficiency. This specific embodiment adjusts the pH value of the vanadium shale acid leachate to 2.5-3.5 by adding alkali, so that the pH value of the aqueous phase in the positive extraction process is stabilized in the range of 2.0-2.5, ensuring that the exchange reaction between vanadium ions and extractant groups is always in the appropriate pH range. The positive extraction stage is significantly shortened to 2-3 stages, achieving the goal of efficient extraction of vanadium ions in the extraction stock solution.
[0113] (2) After the vanadium-containing leachate of vanadium shale is reduced, a reduced liquid is obtained. During the process of adjusting the pH value of the reduced liquid with alkali, a neutralized slag (whose main components are calcium sulfate and colloidal precipitate) is produced. During the pH value change of the reduced liquid, the iron ions undergo hydrolysis reaction, resulting in ferrous hydroxide precipitate. During the stirring process, it is converted into a colloidal precipitate of ferric hydroxide when in contact with air. At the same time, the calcium ions combine with sulfate to produce an emulsion of calcium sulfate. As the lime concentration increases, the calcium sulfate agglomerates to form a gypsum precipitate with a certain viscosity. The vanadate ions in the reduced liquid are carried to the neutralized slag in an adsorbed state and lost. This specific embodiment utilizes the property that the adsorbed vanadium ions in the neutralized slag are easily soluble in acid. The neutralized slag generated by adjusting the pH value of the reduced liquid is returned to the mixed slurry for leaching. The acidity and temperature environment of the leaching slurry are fully utilized to re-extract the vanadium in the neutralized slag. This overcomes the current disadvantage that the vanadium in the neutralized slag is not recycled, and achieves efficient extraction of vanadium. The vanadium leaching rate is greater than 92%.
[0114] (3) The ratio of the concentration of impurity iron ions to the concentration of vanadium ions in the vanadium-containing leachate obtained by the prior art is greater than 3. After extraction, a vanadium-rich solution is obtained. When hydrothermal vanadium precipitation is performed at a pH of about 2.0, iron ions, as typical impurity ions, are easily precipitated into the vanadium product, reducing the purity of the vanadium pentoxide product. Therefore, controlling and reducing the concentration of impurity iron in the vanadium-containing solution from the source is an important way to obtain a high-purity vanadium pentoxide product. This specific embodiment adjusts the pH value of the vanadium-containing leachate to 2.5-3.5, and the impurity iron ions in the solution are fully precipitated and solidified into the neutralized slag. The ratio of the mass concentration of impurity iron ions to the mass concentration of vanadium ions in the vanadium-containing solution (extracted stock solution) is reduced to below 0.4, effectively reducing the concentration of impurity iron ions in the vanadium-containing solution from the source, avoiding the co-precipitation of impurity ions with vanadium and reducing the purity of the vanadium product, and achieving deep separation of vanadium and impurity ions from the source. The purity of the prepared vanadium pentoxide product is greater than 99.20%.
[0115] According to the present embodiment, the vanadium leaching rate is tested to be 92.52-94.11%, the ratio of the mass concentration of iron ions to the mass concentration of vanadium ions in the extraction solution is 0.22-0.35, and the purity of the prepared vanadium pentoxide product is 99.25-99.85%.
[0116] The testing standards for the indicators involved in this specific implementation method are: the vanadium leaching rate is calculated according to the leaching rate formula in "Hydrometallurgy-Leaching Technology" (Liu Hongping, Metallurgical Industry Press, 2010); the mass concentration of iron ions and the mass concentration of vanadium ions in the extraction solution are determined and the ratio is calculated according to the GB / T 8704.10-2020 standard; the purity of the vanadium pentoxide product is tested according to the YB / T5304-2017 standard.
[0117] Therefore, this specific embodiment has the characteristics of being able to re-extract and utilize vanadium in the neutralized slag, obtaining a high vanadium leaching rate, enhancing the extraction efficiency of vanadium ions, shortening the extraction stages, obtaining a low concentration of impure iron in the extracted stock solution, and preparing high-purity vanadium pentoxide.
Claims
1. A method for highly efficient and selective extraction of vanadium from vanadium shale, characterized in that: The specific steps of the method are: Step 1: mixing sulfuric acid solution I with vanadium shale powder at a liquid-solid ratio of 0.7-1.5:1 L / kg to obtain a mixed slurry; then adding a leaching aid to the mixed slurry at a mass ratio of leaching aid to vanadium shale powder of 0.015-0.06:1, slurrying, stirring for the first time, and solid-liquid separation to obtain a vanadium-containing leachate and leach residue; Step 2: adding sodium sulfite to the vanadium-containing leachate at a molar ratio of sodium sulfite to vanadium in the vanadium-containing leachate of 0.28 to 0.45:1, stirring for a second time to obtain a reduced solution; adjusting the pH value of the reduced solution to 2.5 to 3.5 with calcium hydroxide, and performing solid-liquid separation to obtain an extract solution and a neutralized residue; The neutralized slag from this operation is kept in step 1 of the next operation and directly mixed with the mixed slurry after adding the leaching agent; Step 3: Mix the extracted organic phase and the extracted stock solution at a volume ratio of 1:1-4, and extract in a countercurrent manner at 25-30°C to obtain a loaded organic phase; The loaded organic phase and sulfuric acid solution II are mixed at a volume ratio of 4-10:1, and countercurrent stripping is performed at 25-30°C to obtain a vanadium-rich solution; Step 4: adding sodium chlorate to the vanadium-rich solution at a molar ratio of sodium chlorate to vanadium in the vanadium-rich solution of 0.25 to 0.55:1, stirring for a third time to obtain an oxidized solution; adjusting the pH of the oxidized solution to 1.8 to 2.2 with aqueous ammonia, performing a hydrothermal reaction, and performing solid-liquid separation to obtain a vanadium precipitation mother solution and a vanadium precipitation intermediate product; The vanadium precipitation intermediate product is calcined at 500-550° C. in air for 1-2 hours to obtain vanadium pentoxide.
2. The method for highly efficient and selective extraction of vanadium from vanadium shale according to claim 1, characterized in that: The preparation method of the vanadium shale ore powder is as follows: crushing the vanadium shale, grinding the ore until the particle size is less than 0.074 mm, accounting for 45-80%, to obtain the vanadium shale ore powder.
3. The method for highly efficient and selective extraction of vanadium from vanadium shale according to claim 1, characterized in that: The sulfuric acid concentration of the sulfuric acid solution I is 2.0-6.2 mol / L.
4. The method for highly efficient and selective extraction of vanadium from vanadium shale according to claim 1, characterized in that: The leaching aid is calcium fluoride or sodium fluoride.
5. The method for highly efficient and selective extraction of vanadium from vanadium shale according to claim 1, characterized in that: The stirring is: The first stirring in step 1 is: stirring at 80-95° C. for 5-15 hours; The second stirring in step 2 is: stirring at 50-70° C. for 10-30 minutes; The third stirring in step 4 is: stirring at 50-80° C. for 20-40 minutes.
6. The method for highly efficient and selective extraction of vanadium from vanadium shale according to claim 1, characterized in that: The extraction organic phase is a mixture of 10-20 vol% of an extractant and 80-90 vol% of sulfonated kerosene; the extractant is di(2-ethylhexyl) phosphate or 2-ethylhexylphosphonic acid mono-2-ethylhexyl ester.
7. The method for highly efficient and selective extraction of vanadium from vanadium shale according to claim 1, characterized in that: The concentration of the sulfuric acid solution II is 1.2-2.5 mol / L.
8. The method for highly efficient and selective extraction of vanadium from vanadium shale according to claim 1, characterized in that: The number of stages of the countercurrent forward extraction is 2 to 3, and the single-stage reaction time of the countercurrent forward extraction is 7 to 15 minutes.
9. The method for highly efficient and selective extraction of vanadium from vanadium shale according to claim 1, characterized in that: The number of stages of the countercurrent stripping is 3 to 5, and the single-stage reaction time of the countercurrent stripping is 5 to 15 minutes.
10. The method for highly efficient and selective extraction of vanadium from vanadium shale according to claim 1, characterized in that: The conditions of the hydrothermal reaction are: the hydrothermal reaction temperature is 85-95° C., and the hydrothermal reaction time is 1-2 hours.
Citation Information
Patent Citations
Stone coal vanadium ore leaching process for recycling residual acid
CN104988337A
Method for separating ferrum and vanadium in vanadium pickle liquor
CN106086408A
Stone coal concentrated acid two-stage curing vanadium extraction process
CN115354173A
Cited By
Method for recovering silver and vanadium from silver associated vanadium shale mineral
CN121109765A