Mycelium leather based on hydrophobic treatment and preparation method thereof
The problem of hardening and not resistant to bending after filling is solved by hydrophobic treatment, and soft and plump mycelial leather is prepared, avoiding the pollution of chemical crosslinking and improving biodegradability.
Patent Information
- Application Number
- CN202511072035.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-08-01
- Publication Date
- 2025-09-02
- Estimated Expiration
- 2045-08-01
AI Technical Summary
In the prior art, mycelium leather is prone to hardening and not resistant to bending after filling operation, and the chemical crosslinking process leads to the problem of residual harmful chemical substances and difficulty in biodegradation.
Using the hydrophobic treatment method, through mechanical extrusion, solvent and water-absorbing medium dehydration, plasticization and hydrophobic treatment process, a hydrophobic film is formed on the surface of mycelium fibers by using silane coupling agent and silicon-containing polymer materials to avoid chemical crosslinking, maintain the dispersed fiber state, and improve flexibility and water resistance.
Soft, plump and water-resistant mycelial leather is prepared, which reduces the emission of harmful chemicals and improves biodegradability, meets the requirements of green technology, and the product can be completely degraded in natural environments.
Smart Images

Figure CN120574997A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of mycelium leather and relates to mycelium leather based on hydrophobic treatment and a preparation method thereof. Background Art
[0002] Mycelial leather-like products are future biomaterials that can replace petroleum-based synthetic leather and animal leather. They have the advantages of environmental protection and sustainability. The advantages of mycelial leather are mainly reflected in the following aspects: (1) Mycelial leather is made from mycelium, which is obtained by fermentation and culture using agricultural and forestry by-products as a nutrient base. The mycelium production process emits less greenhouse gases and consumes less water and natural resources. At the same time, its biocarbon content is as high as about 95%, which is more environmentally friendly and sustainable than traditional animal leather and synthetic leather. (2) Traditional leather uses harmful chemicals such as chromium in the preparation process. These harmful chemicals are likely to remain in the product and pose potential harm to the health of consumers. At the same time, its preparation process will generate a large amount of industrial wastewater. However, the production process of mycelial leather products does not require the addition of harmful chemicals such as chromium. Therefore, mycelial leather products are safer and their production process can avoid the discharge of a large amount of industrial wastewater. (3) Mycelial leather is a leather substitute made from bio-based materials with a low polymer content. The product is easily biodegradable after its life cycle and is not likely to cause environmental problems.
[0003] MycoWorks Biotechnologies has developed Reishi™, a material made from mycelium using Fine Mycelium™ technology. This material, containing less than 1% polymer, boasts excellent tensile strength, tear resistance, and durability, comparable to animal leather, making it a potential alternative to natural leather. Since then, research into mycelium-based leather has ignited a global wave.
[0004] Fungal mycelium is composed of a network of tubular microfilaments called hyphae. The main components of the mycelial cell wall are polysaccharides, followed by proteins and lipids. The cell wall accounts for 30% of the cell's dry matter. The polysaccharides that make up the mycelial cell wall are primarily polymers such as chitin, glucan, and mannan. Chitin is a polysaccharide composed of N-acetylglucosamine molecules linked by β-(1,4) glucosidic bonds. It is a tough, elastic, inert, and water-insoluble polysaccharide. Due to the compositional properties of the mycelial cell wall, mycelial materials can be processed into leather-like products or processed into composites with other materials such as cotton textiles and macromolecular polymers. Such composites can be used as textiles, packaging materials, and construction materials.
[0005] Currently, there are documents that disclose methods for modifying mycelial materials to prepare composite materials by crosslinking. These methods are basically based on the processing ideas of animal leather. First, a crosslinking agent is used to form chemical crosslinks between mycelial fibers after deacetylation to stabilize the fiber structure. Then, a soft leather-like blank is obtained by plasticization or lubrication. Finally, a product similar to animal leather is obtained by finishing and surface modification. The properties of mycelial materials can be regulated by chemical crosslinking modification. For example, the tensile strength, tear strength and wear resistance of mycelial leather can be improved to a certain extent by chemical crosslinking. However, the premise of chemical crosslinking modification is to treat the mycelial fibers with alkali to achieve deacetylation of chitin in the mycelial fibers and obtain chitosan components containing amino groups. This alkali treatment process will dissolve and remove some polysaccharides in the mycelial fibers, causing the loss of mycelial fiber components, resulting in a decrease in the mechanical properties and plumpness of the mycelial leather. Therefore, in fact, chemical crosslinking does not significantly improve the mechanical properties of mycelial leather. At the same time, the chemical crosslinking agents added during the chemical crosslinking process can also cause some environmental problems, such as the emission of harmful chemicals during production, the residue of harmful chemical components in the product, and the difficulty of achieving complete biodegradation of the product after its life cycle. In addition, for animal leather, the mechanical properties can be improved after the filling operation, but for mycelium leather, due to the hollow tubular structure of mycelium fibers and the lack of interweaving between fibers, they often become hard and less resistant to bending after the filling operation. Especially in the finishing process, mycelium leather is prone to breakage or tearing due to the repeated "water absorption and loss" during processing. Therefore, it can be seen that the processing concept of animal leather is not entirely suitable for the processing of mycelium leather.
[0006] Therefore, finding a suitable processing method for mycelium-based leather to address the problem of mycelium-based leather becoming hard and unbending after filling is a major challenge in this field. Furthermore, developing a mycelium-based leather production method that does not require a chemical cross-linking process would have significant implications for reducing the loss of mycelium fiber components during the production process, preventing the residual and emission of harmful chemicals in the product, and increasing the product's biodegradability at the end of its lifecycle. Summary of the Invention
[0007] In view of the problems that the existing mycelium leather preparation method that draws on the processing ideas of animal skins easily leads to the mycelium leather having poor toughness and being not resistant to bending, as well as the problems of harmful chemical reagents remaining in the product due to the need for chemical cross-linking, the emission of harmful substances during the preparation process, and the difficulty of the product to be completely biodegraded after the end of its life cycle, the present invention provides mycelium leather based on hydrophobic treatment and a preparation method thereof, so as to avoid the problems of mycelium leather becoming hard and not resistant to bending caused by the use of chemical cross-linking agents and the processing process, so as to obtain mycelium leather products that are soft, plump and have good toughness, and make the process more in line with the requirements of green chemical industry.
[0008] In order to achieve the above-mentioned object of the invention, the technical solution adopted by the present invention is as follows:
[0009] The preparation method of mycelium leather based on hydrophobic treatment comprises the following steps:
[0010] (1) Mechanical water squeezing
[0011] Mechanically squeezing water from freshly harvested and inactivated mycelium sheets or pretreated mycelium sheets until the water content is 40 wt% to 70 wt% to obtain squeezed mycelium sheets;
[0012] (2) Dehydration of solvent and water-absorbing medium
[0013] 100 parts by weight of the squeezed mycelium sheet, 100-300 parts by weight of a hydrophilic solvent, and 100-200 parts by weight of a water-absorbing medium are placed in a dehydration container, and the mixture is allowed to stand at room temperature to 50°C for 30-150 minutes for dehydration, followed by centrifugation. The mycelium sheet obtained by centrifugation is heated to remove the hydrophilic solvent from the mycelium sheet, thereby obtaining a dehydrated mycelium sheet;
[0014] (3) Plasticization and hydrophobic treatment
[0015] 6-40 parts by mass of a silicon-containing polymer material, 1-10 parts by mass of a silicon-based wetting agent, 8-30 parts by mass of a silane coupling agent and / or silicone oil are dissolved or fully dispersed in 60-300 parts by mass of a solvent to obtain a plasticizing and hydrophobizing treatment agent; the obtained plasticizing and hydrophobizing treatment agent and 100 parts by mass of dehydrated mycelium sheets are placed in a rotary drum, and the drum is rotated at a constant temperature of 35-60° C. for 2-8 hours to remove the skin, thereby obtaining a plasticized and hydrophobized mycelium skin blank;
[0016] (4) Drying and finishing
[0017] The plasticized and hydrophobized mycelium leather is dried and finished to obtain mycelium leather.
[0018] In the above technical solution, the silicon-containing polymer material in step (3) includes at least one of OMBRELLON 072, PERFECTOL HQ, and PERFECTOL QX.
[0019] In the above technical solution, the silicon-based wetting agent in step (3) is Silok 8008 or Silok 8000.
[0020] In the above technical solution, the silane coupling agent in step (3) includes at least one of N-β-aminoethyl-γ-aminopropylmethyldimethoxysilane, γ-aminopropyltriethoxysilane, and N-β-aminoethyl-γ-aminopropyltrimethoxysilane, and the silicone oil includes at least one of hydrogenated silicone oil, hydroxyl silicone oil, and dimethyl silicone oil. In step (3), the silane coupling agent or silicone oil is primarily used to react with the hydroxyl groups of the mycelium fibers and coat the surface of the mycelium fibers, thereby forming a hydrophobic effect.
[0021] In the above technical solution, when preparing the plasticizing and hydrophobizing agent, the solvent used is an organic solvent, water, or a mixture of an organic solvent and water. When the solvent cannot dissolve the hydrophobic material, it is necessary to add the hydrophobic material to a solvent at a temperature of 50-90°C and stir and emulsify it to form the plasticizing and hydrophobizing agent. The hydrophobic material is a combination of a silicon-containing polymer material, a silicon-based wetting agent, a silane coupling agent, and / or silicone oil.
[0022] In the above technical solution, in step (3), when preparing the plasticizing and hydrophobic treatment agent, it is best to fully disperse the silicon-containing polymer material, silicon-based wetting agent, and silane coupling agent in the solvent, or dissolve or fully disperse the silicon-containing polymer material, silicon-based wetting agent, silane coupling agent and silicone oil in the solvent to obtain the plasticizing and hydrophobic treatment agent.
[0023] In the above technical solution, the water-absorbing medium in step (2) includes zeolite, porous silica gel, or color-changing silica gel. To prevent the water-absorbing medium from damaging the mycelium sheet during the treatment process in step (2), the water-absorbing medium is preferably in the form of spherical particles. Furthermore, to improve the water absorption efficiency of the water-absorbing medium, the particle size of the spherical particles of the water-absorbing medium is preferably between 2 and 10 mm.
[0024] In the above technical solution, the hydrophilic solvent in step (2) is an organic solvent that is miscible with water and has a boiling point not exceeding 90°C, so as to facilitate recovery and recycling. For example, feasible hydrophilic solvents include anhydrous ethanol, methanol, acetone or methyl ethyl ketone.
[0025] In the above technical solution, the liquid phase obtained by centrifugation in step (2) is collected, the hydrophilic solvent in the liquid phase is recovered, and the recovered hydrophilic solvent is recycled. For example, the hydrophilic solvent can be recovered by distilling the collected liquid phase, and the recovered hydrophilic solvent can be recycled. The water-absorbing medium obtained by centrifugation in step (2) after absorbing water is collected, heated, and then regenerated for recycling. In order to reduce process costs and increase process environmental friendliness, the hydrophilic solvent volatilized during the heating of the mycelium sheets obtained by centrifugation in step (2) can also be collected and recycled.
[0026] In the above technical solution, in step (2), when heating the mycelium sheet obtained by centrifugation to remove the hydrophilic solvent in the mycelium sheet, the heating temperature is controlled to be above the boiling point of the hydrophilic solvent. The heating temperature can usually be controlled to be between T and (T+5°C), where T is the boiling point of the hydrophilic solvent.
[0027] In the above technical solution, the dehydration container in step (2) is a sealed container to prevent the hydrophilic solvent from volatilizing during the dehydration operation in step (2) and causing environmental pollution, and also to facilitate the recycling of the hydrophilic solvent.
[0028] In the above technical solution, the preparation method of the pretreated mycelium sheet in step (1) is as follows: 100 parts by mass of freshly harvested and inactivated mycelium sheets, 100-500 parts by mass of water, and 0.1-0.4 parts by mass of an alkaline material are placed in a pretreatment container, soaked at 35-80°C for 10-200 minutes, and then washed with water. During the pretreatment process of adding water and alkaline material, impurities such as soluble polysaccharides and attached culture medium on the surface of the mycelium sheets and between the mycelium fibers are mainly removed. Since the amount of alkaline material added is very small, this process will not cause excessive loss of polysaccharide components in the mycelium and damage the chitin in the cell wall of the mycelium.
[0029] Furthermore, in the above technical solution, the alkaline material is at least one of sodium carbonate, sodium bicarbonate, sodium hydroxide, potassium hydroxide, sodium formate, and sodium acetate.
[0030] In the above technical solution, step (1) can be performed by mechanically squeezing the freshly harvested and inactivated mycelium sheets or pretreated mycelium sheets by rolling, pressing, etc. to remove a large amount of free water therein. In practical applications, mechanical squeezing can be performed by using a through-type squeezing machine, a flat plate press, etc.
[0031] In the above technical solution, the method of controlling the rotation of the drum in step (3) is intermittent rotation. For example, the drum can be rotated intermittently for 5 to 15 minutes per hour.
[0032] In the above technical solution, in step (4), conventional methods of the prior art are used to dry and finish the plasticized and hydrophobized mycelium skin, which mainly includes the processes of drying on a stretching board, rewetting, softening, peeling or shaving.
[0033] In the above technical solution, the mycelium sheet refers to sheet-like mycelium, preferably sheet-like fungal mycelium. The mycelium sheet can be prepared according to existing techniques, typically by transplanting mycelium obtained from liquid fermentation onto a solid culture medium for cultivation. For example, mycelium obtained from liquid fermentation of a Ganoderma lucidum strain can be transplanted onto a solid culture medium for cultivation.
[0034] The present invention also provides mycelium leather prepared by the method.
[0035] Compared with the prior art, the technical solution of the present invention produces the following beneficial technical effects:
[0036] 1. The present invention provides a preparation method of mycelium leather based on hydrophobic treatment. The method first combines physical and chemical medium dehydration to completely dehydrate the mycelium sheets, so that the mycelium fibers are in a well-separated state. On this basis, the mycelium fibers in a well-separated state are treated with high-performance hydrophobic materials to form a hydrophobic film on the surface of the mycelium fibers or between the fibers, so that the mycelium fibers can be better maintained in a dispersed state. This can effectively avoid the problem of mycelium fibers easily losing water excessively and sticking together during drying, and effectively reduce the mycelium fibers' ability to adsorb water, especially solving the problem of fiber compaction caused by repeated "water absorption-dehydration" processes during the post-finishing process, which leads to the hardening and even brittle cracking of the mycelium leather. The key point of the method described in the present invention is to use a silane coupling agent in combination with a silicon-containing polymer material and a silicon-based wetting agent in an appropriate proportion. The silane coupling agent reacts with the hydroxyl groups on the mycelium fibers to firmly coat the surface of the mycelium fibers. Combined with the filling and hydrophobic effects of the silicon-containing polymer material and the silicon-based wetting agent, not only the flexibility and water resistance of the product are increased, but also the mycelium-based leather is given good softness and fullness.
[0037] 2. The method of the present invention does not use chemical cross-linking agents in the preparation process of mycelium leather, which can eliminate the problem of pollutant emissions in the processing process and the ecological safety problem of the end product from the source, and improve the biodegradability of the end product. In the dehydration process of the solvent and the water-absorbing medium in the method of the present invention, the hydrophilic solvent and the water-absorbing medium used can be recycled. In the plasticization and hydrophobic treatment process, the method of the present invention applies the hydrophobic material in the form of a solution or emulsion, which can improve the absorption rate of the hydrophobic material and reduce or even avoid the discharge of waste liquid in the processing process. Through the coordination of the above process details, the method of the present invention can better meet the requirements of sustainability, environmental protection and greening.
[0038] 3. The present invention has confirmed through soil landfill natural degradation tests that the mycelium leather prepared by the method of the present invention can be basically completely naturally degraded within 40 days after soil landfill in a natural environment, and has excellent biodegradability.
[0039] 4. The mycelium leather prepared by the method of the present invention is light yellow to light brown in color, has no odor, and the leather is soft, foamy, plump, and has a natural texture, which is comparable to the sensory properties of animal leather. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 The present invention is a process flow chart of the method for preparing the hydrophobic-treated mycelium leather.
[0041] Figure 2 This is a photograph of the grain surface of the mycelium-based leather prepared in Example 1.
[0042] Figure 3 This is a micrograph of fibers of the mycelium sheet used in Example 1.
[0043] Figure 4 This is a microscopic photograph of the fibers of the mycelium-based leather prepared in Example 1.
[0044] Figure 5 This is a photograph of the mycelium leather prepared in Comparative Example 1 when bent.
[0045] Figure 6 This is a photograph of the grain surface of the mycelium-based leather prepared in Example 2.
[0046] Figure 7 This is a microscopic photograph of the fibers of the mycelium-based leather prepared in Example 2.
[0047] Figure 8 This is a photograph of the grain surface of the mycelium-based leather prepared in Example 3.
[0048] Figure 9 This is a microscopic photograph of the fibers of the mycelium-based leather prepared in Example 3. DETAILED DESCRIPTION
[0049] The following examples further illustrate the hydrophobic treated mycelium leather and its preparation method provided by the present invention. It is important to note that the following examples are intended only to further illustrate the present invention and are not to be construed as limiting the scope of protection of the present invention. Non-essential improvements and adjustments made by persons skilled in the art based on the above disclosure are still within the scope of protection of the present invention.
[0050] In the following examples and comparative examples, the silicon-containing polymer materials, silicon-based wetting agents, water-absorbing media, silane coupling agents, silicone oils, etc. used are all commercial products on the market and can be directly purchased. Among them, the silicon-containing polymer material OMBRELLON072 is a commercial product of Zschimmer & Schwarz (Schima, Germany), and the silicon-containing polymer materials PERFECTOLHQ and PERFECTOL QX are commercial products of Schill & Seiacher, Germany; the silicon-based wetting agents Silok 8008 and Silok 8000 are commercial products of Guangzhou Silok Polymer Co., Ltd.; and the fatliquor XG-60 is a commercial product of Brother Chemical Co., Ltd.
[0051] In the following examples and comparative examples, the mycelium sheet refers to sheet-like mycelium, which is sourced from Tianjin Meikexin Biotechnology Co., Ltd. and is obtained by transplanting mycelia obtained by liquid fermentation of a Ganoderma lucidum strain onto a solid culture medium for cultivation.
[0052] In the following examples and comparative examples, the static water absorption rate was measured according to the method in GB / T 22899-2008 “Leather physical and mechanical tests - Determination of static water absorption rate”.
[0053] Example 1
[0054] In this embodiment, a method for preparing mycelium leather based on hydrophobic treatment is provided, and the process flow of the method is as follows: Figure 1 As shown, the steps are as follows:
[0055] (1) Mechanical water squeezing
[0056] 100 parts by mass of freshly harvested and inactivated mycelium sheets, 200 parts by mass of water, and 0.3 parts by mass of sodium carbonate were placed in a container and soaked at 50°C for 120 min to remove soluble polysaccharides and attached culture medium on the surface of the mycelium sheets and between the mycelium fibers. The mycelium sheets were then washed with water to obtain pretreated mycelium sheets.
[0057] The pretreated mycelium sheets were squeezed with a roller pressure of 10 MPa using a through-type squeezer to squeeze water to a water content of 40 wt% to 50 wt%, thereby obtaining squeezed mycelium sheets.
[0058] (2) Dehydration of solvent and water-absorbing medium
[0059] 100 parts by mass of squeezed mycelium sheets, 300 parts by mass of acetone, and 100 parts by mass of spherical porous color-changing silica gel particles with a particle size of approximately 3 to 5 mm were placed in a sealed container and allowed to stand at room temperature for 50 minutes for dehydration. The mixture was then centrifuged to remove most of the acetone in the mycelium sheets and the porous color-changing silica gel particles attached to the mycelium sheets. The mycelium sheets obtained by centrifugation were heated to 57°C and maintained at this temperature until the acetone in the mycelium sheets was completely removed, thereby obtaining dehydrated mycelium sheets.
[0060] The liquid phase obtained by centrifugation in this step is collected, and the collected liquid phase is distilled to recover acetone and the recovered acetone is recycled. The acetone volatilized during the heating process of the mycelium sheet obtained by centrifugation at 57°C is collected and recycled. The porous color-changing silica gel particles obtained by centrifugation are recovered, heated to remove moisture therein, and then regenerated and recycled.
[0061] (3) Plasticization and hydrophobic treatment
[0062] 40 parts by mass of OMBRELLON 072, 5 parts by mass of Silok 8008, and 10 parts by mass of γ-aminopropyltriethoxysilane (KH550) were thoroughly mixed and added to 200 parts by mass of hot water at 60°C with stirring to emulsify the mixture, thereby obtaining a plasticizing and hydrophobizing agent. The plasticizing and hydrophobizing agent and 100 parts by mass of dehydrated mycelium sheets were placed in a rotating drum. The drum was rotated intermittently at 3 rpm for 4 hours (5 minutes per hour) at a constant temperature of 40°C, and then the skins were removed to obtain plasticized and hydrophobized mycelium skins.
[0063] (4) Drying and finishing
[0064] The plasticized and hydrophobized leather blank is dried, rehumidified, softened and shaved according to conventional operations to obtain mycelium leather.
[0065] The grain surface of the mycelium leather prepared in this example is shown in FIG. Figure 2 As shown, the grain surface of the mycelium leather prepared in this embodiment presents a natural texture and is soft to the touch. The inner fiber hairs are extremely fine and have a velvety touch. At the same time, the mycelium leather prepared in this embodiment has good fullness and flexibility. By observing the fibers of the mycelium sheet used in step (1) of this embodiment through a microscope, it can be found that although the mycelium fiber components are visible at the edge of the mycelium sheet, there is a clear bonding phenomenon between the mycelium fibers (see Figure 3 By microscopically observing the fibers on the grain surface of the mycelium leather prepared in this embodiment, it can be clearly seen that the mycelium fibers of the mycelium leather are well dispersed after plasticization and hydrophobic treatment, and the fibers in the skin-core part are in a separated state (see Figure 4Since no cross-linking agent is used for chemical cross-linking during the entire mycelium leather processing process of this embodiment, the mycelium leather prepared in this embodiment does not contain chemical cross-linking agents that are harmful to the human body and the environment, and no wastewater containing chemical cross-linking agents is discharged during the preparation process, which is safe and environmentally friendly.
[0066] The static water absorption rate of the mycelium leather prepared in this example was tested, and the results showed that the static water absorption rate was between 115% and 125%.
[0067] Three small samples of 5 cm × 5 cm were cut from the mycelium leather sample prepared in this example. The small samples were buried in garden soil approximately 30 cm below the surface under natural conditions. The soil was dug up and observed on the 20th, 30th, and 40th days, respectively. It was found that the small samples had been basically naturally degraded into fine particles on the 40th day.
[0068] Comparative Example 1
[0069] In this comparative example, a method for preparing mycelium leather without plasticization and hydrophobic treatment is provided. The operation of this comparative example is basically the same as that of Example 1, except that step (3) of Example 1 is omitted.
[0070] The mycelium leather prepared in this comparative example looks very fluffy and light in weight, but feels hard and has almost no toughness. It is very easy to break when bent. Figure 5 As shown in the figure, the mycelium leather prepared in this comparative example can be easily broken by one hand and observed under an optical microscope. Figure 5 Fibers at the fracture site were examined. While there were cavities between the mycelial fibers, the fibers were poorly dispersed and exhibited significant adhesion. The mycelium leather prepared in this comparative example readily absorbed water, causing blistering and even exhibiting delamination of the mycelial fibers. Static water absorption testing of the mycelium leather prepared in this comparative example revealed a static water absorption rate between 280% and 290%.
[0071] It can be seen from Comparative Example 1 that, in the preparation process of mycelium leather, if plasticization and hydrophobic treatment are not performed, the prepared mycelium leather has no flexibility, is not resistant to bending, is very easy to break, and has very poor water resistance.
[0072] Comparative Example 2
[0073] In this comparative example, a method for preparing mycelium leather after plasticization is provided. The operation of this comparative example is basically the same as that of Example 1, except that step (3) of Example 1 is replaced by the following plasticization operation:
[0074] 100 parts by mass of water, 20 parts by mass of glycerol, 6 parts by mass of fatliquor XG-60, and 100 parts by mass of dehydrated mycelium sheets were placed in a drum, and the drum was rotated intermittently at a speed of 3 rpm for 4 hours (the drum was rotated for 5 minutes per hour) at a constant temperature of 40°C to remove the skin to obtain a plasticized mycelium skin blank.
[0075] During the drying and finishing process of step (4), the leather blank stretched board plasticized in step (3) is dried, rehumidified, softened, and shaved according to conventional operations to obtain mycelium leather.
[0076] The mycelium-based leather prepared in this comparative example has a moist feel and improved softness compared to Comparative Example 1. However, its softness and fullness are still poor, and it is slightly hard and lacks toughness. This is primarily due to the plasticizer being easily washed away during the finishing process. Upon contact with water, the mycelium-based leather prepared in this comparative example readily absorbs moisture, resulting in blistering. Static water absorption testing of the mycelium-based leather prepared in this comparative example showed a static water absorption rate between 185% and 195%.
[0077] Combined with Comparative Examples 1 to 2, it can be seen that in the preparation process of mycelium leather, although the plasticizing operation can improve the softness, fullness and water resistance of mycelium leather to a certain extent, the softness and fullness are still poor, and the water resistance is still at a poor level. At the same time, it is also difficult to effectively solve the problem of poor toughness of mycelium leather.
[0078] Comparative Example 3
[0079] In this comparative example, a method for preparing mycelium leather after glutaraldehyde cross-linking and plasticization treatment is provided, and the steps are as follows:
[0080] (1) Deacetylation treatment
[0081] 100 parts by mass of freshly harvested and inactivated mycelium sheets, 200 parts by mass of water and 3 parts by mass of sodium carbonate were placed in a container and immersed at 50°C for 180 minutes for deacetylation. The deacetylated mycelium sheets were then washed with water and centrifuged for dehydration to obtain deacetylated mycelium sheets.
[0082] (2) Cross-linking
[0083] 100 parts by mass of deacetylated mycelium sheets, 100 parts by mass of water, and 5 parts by mass of glutaraldehyde were placed in a rotary drum. The temperature of the bath was controlled at 32°C, and the drum was rotated for 3 hours. Then, sodium bicarbonate solution was added to the drum once every 0.5 hour, and sodium bicarbonate solution was added three times in total to adjust the pH value of the bath to 7.0-7.2. The temperature of the bath was raised to 40°C, and the drum was rotated for 1 hour. The mycelium sheets were allowed to stand for 12 hours and peeled to obtain cross-linked mycelium sheets.
[0084] (3) Plasticization
[0085] 100 parts by mass of cross-linked mycelium sheets, 100 parts by mass of water, 20 parts by mass of glycerol, and 6 parts by mass of fatliquor XG-60 were placed in a drum, and the drum was rotated intermittently at 3 rpm for 4 hours (5 minutes per hour) at a constant temperature of 40°C to remove the skin.
[0086] (4) Drying and finishing
[0087] The plasticized leather blank is dried, rehumidified, softened and shaved according to conventional operations to obtain mycelium leather.
[0088] The mycelium leather prepared in this comparative example has significantly improved softness and fullness compared to comparative example 1, and also significantly improved toughness and water resistance compared to comparative example 2. However, its water resistance is still poor. Static water absorption test of the mycelium leather prepared in this comparative example showed that the static water absorption of the mycelium leather prepared in this comparative example was between 160% and 170%.
[0089] Four small samples of 5 cm × 5 cm were cut from the mycelium leather sample prepared in this comparative example. The small samples were buried in garden soil about 30 cm below the surface under natural conditions. The soil was dug up and observed on the 60th, 90th, 120th and 150th days respectively. It was found that it took 150 days for the small samples to be naturally degraded into fine particles.
[0090] It can be seen from the combination with comparative examples 1 to 3 that, in the preparation process of mycelium leather, a chemical cross-linking agent is introduced before the plasticizing operation to carry out cross-linking, which can improve the fullness of mycelium leather and improve its water resistance to a certain extent, but the water resistance of the prepared mycelium leather is still not good. Since the mycelium fibers of mycelium leather are looser than the collagen fibers of animal skins, this will cause the water absorption of mycelium leather to be stronger. As shown in Example 1, even after plasticizing and hydrophobic treatment during the preparation process, the water absorption of the prepared mycelium leather is still stronger than natural animal leather. Therefore, for the preparation of mycelium leather, how to improve the problem of strong water absorption and poor water resistance caused by the relatively loose mycelium fibers is also very important for improving the application performance of mycelium leather. Crosslinking with a chemical crosslinker can form covalent bonds between mycelial fibers, increasing the connection and tightness between the mycelial fibers to a certain extent. Theoretically, crosslinking with a chemical crosslinker can improve the water resistance of mycelial leather. However, according to Comparative Example 3, chemical crosslinking with glutaraldehyde did not significantly improve the water resistance of mycelial leather. This suggests that chemical crosslinking is not effective in improving the water resistance of mycelial leather. In contrast, Example 1, through plasticization and hydrophobic treatment, achieved a better improvement in the water resistance of mycelial leather than Comparative Examples 1-3.
[0091] In addition, based on the natural degradation performance test results of Example 1 and Comparative Example 3, it can be seen that the introduction of a chemical cross-linking agent for cross-linking will lead to a decrease in the natural degradation performance of the mycelium-based leather.
[0092] Example 2
[0093] In this embodiment, a method for preparing mycelium leather based on hydrophobic treatment is provided, and the process flow of the method is as follows: Figure 1 As shown, the steps are as follows:
[0094] (1) Mechanical water squeezing
[0095] 100 parts by mass of freshly harvested and inactivated mycelium sheets, 300 parts by mass of water, and 0.4 parts by mass of sodium carbonate were placed in a container and soaked at 40°C for 100 min to remove soluble polysaccharides and attached culture medium on the surface of the mycelium sheets and between the mycelium fibers. The mycelium sheets were then washed with deionized water to obtain pretreated mycelium sheets.
[0096] The pretreated mycelium sheets were squeezed with a roller pressure of 6 MPa using a through-type squeezer to squeeze water to a water content of 45 wt% to 55 wt%, thereby obtaining squeezed mycelium sheets.
[0097] (2) Dehydration of solvent and water-absorbing medium
[0098] 100 parts by mass of squeezed mycelium sheets, 250 parts by mass of anhydrous ethanol, and 200 parts by mass of spherical porous color-changing silica gel particles with a particle size of approximately 6-8 mm were placed in a sealed container and allowed to stand at 40°C for 40 minutes for dehydration. The mixture was then centrifuged to remove most of the anhydrous ethanol in the mycelium sheets and the porous color-changing silica gel particles attached to the mycelium sheets. The mycelium sheets obtained by centrifugation were heated to 79°C and maintained at this temperature until the anhydrous ethanol in the mycelium sheets was completely removed, thereby obtaining dehydrated mycelium sheets.
[0099] The liquid phase obtained by centrifugation in this step is collected, and the collected liquid phase is distilled to recover anhydrous ethanol and the recovered anhydrous ethanol is recycled. The anhydrous ethanol volatilized during the heating process of the mycelium pieces obtained by centrifugation at 79°C is collected and recycled. The porous color-changing silica gel particles obtained by centrifugation are recovered, heated to remove moisture therein, and then regenerated and recycled.
[0100] (3) Plasticization and hydrophobic treatment
[0101] 6 parts by mass of PERFECTOL QX, 1 part by mass of Silok 8000, and 16 parts by mass of N-β-aminoethyl-γ-aminopropyltrimethoxysilane (KH792) were thoroughly mixed and added to 40 parts by mass of anhydrous ethanol and 50 parts by mass of hot water at 50°C, stirring and emulsifying to obtain a plasticizing and hydrophobizing agent. The plasticizing and hydrophobizing agent and 100 parts by mass of dehydrated mycelium sheets were placed in a rotating drum. The drum was rotated intermittently at 5 rpm for 5 hours at a constant temperature of 50°C (10 minutes per hour), and the skins were removed to obtain plasticized and hydrophobized mycelium skins.
[0102] (4) Drying and finishing
[0103] The plasticized and hydrophobized leather blank is dried, rehumidified, softened and shaved according to conventional operations to obtain mycelium leather.
[0104] The grain surface of the mycelium leather prepared in this example is shown in FIG. Figure 6 As shown, the grain surface of the mycelium leather prepared in this embodiment presents a natural texture and the grain surface is smoother (relative to Example 1), and it feels soft. The inner fiber hairs are extremely fine and have a velvety touch. At the same time, the mycelium leather prepared in this embodiment has good fullness and flexibility. By observing the fibers of the mycelium sheet used in step (1) of this embodiment through a microscope, it was found that there was obvious bonding between the mycelium fibers of the mycelium sheet. By microscopically observing the fibers of the grain surface of the mycelium leather prepared in this embodiment, it can be clearly seen that the mycelium fibers of the mycelium leather are in a well-dispersed state (see Figure 7The static water absorption rate of the mycelium leather prepared in this embodiment was tested, and the results showed that the static water absorption rate was between 120% and 130%.
[0105] Example 3
[0106] In this embodiment, a method for preparing mycelium leather based on hydrophobic treatment is provided, and the process flow of the method is as follows: Figure 1 As shown, the steps are as follows:
[0107] (1) Mechanical water squeezing
[0108] Freshly harvested and inactivated mycelium sheets were squeezed with a roller pressure of 20 MPa using a through-type squeezer to squeeze water to a water content of 55 wt% to 65 wt% to obtain squeezed mycelium sheets.
[0109] (2) Dehydration of solvent and water-absorbing medium
[0110] 100 parts by mass of squeezed mycelium sheets, 250 parts by mass of acetone, and 150 parts by mass of spherical porous color-changing silica gel particles with a particle size of approximately 4 to 6 mm were placed in a sealed container and allowed to stand at 40°C for 40 minutes for dehydration. The mixture was then centrifuged to remove most of the acetone in the mycelium sheets and the porous color-changing silica gel particles attached to the mycelium sheets. The mycelium sheets obtained by centrifugation were heated to 60°C and maintained at this temperature until the acetone in the mycelium sheets was completely removed, thereby obtaining dehydrated mycelium sheets.
[0111] The liquid phase obtained by centrifugation in this step is collected, and the collected liquid phase is distilled to recover acetone, and the recovered acetone is recycled. The acetone volatilized during the heating process of the mycelium sheet obtained by centrifugation at 60°C is collected and recycled. The porous color-changing silica gel particles obtained by centrifugation are recovered, heated to remove moisture therein, and then regenerated and recycled.
[0112] (3) Plasticization and hydrophobic treatment
[0113] Thoroughly mix 10 parts by mass of PERFECTOL HQ, 2 parts by mass of Silok 8008, and 30 parts by mass of N-β-aminoethyl-γ-aminopropyltrimethoxysilane (KH792). The resulting mixture is added to 30 parts by mass of anhydrous ethanol and 30 parts by mass of n-hexane and stirred thoroughly until dissolved to obtain a plasticizing and hydrophobizing agent. The plasticizing and hydrophobizing agent and 100 parts by mass of dehydrated mycelium sheets are placed in a rotating drum. The drum is rotated intermittently at 6 rpm for 3 hours (15 minutes per hour) at a constant temperature of 40°C. The skins are then removed to obtain plasticized and hydrophobized mycelium shells.
[0114] (4) Drying and finishing
[0115] The plasticized and hydrophobized leather blank is dried, rehumidified, softened and shaved according to conventional operations to obtain mycelium leather.
[0116] The grain surface of the mycelium leather prepared in this example is shown in FIG. Figure 8 As shown, the grain texture of the mycelium leather prepared in this embodiment is natural, flat and fine, soft to the touch, and the inner layer has a velvety touch. At the same time, the mycelium leather prepared in this embodiment has good fullness and flexibility. By observing the fibers of the mycelium sheet used in step (1) of this embodiment through a microscope, it was found that there was obvious bonding between the mycelium fibers of the mycelium sheet. By microscopically observing the fibers of the grain surface of the mycelium leather prepared in this embodiment, the mycelium fibers of the mycelium leather have a good dispersion state (see Figure 9 The static water absorption rate of the mycelium leather prepared in this embodiment was tested, and the results showed that the static water absorption rate was between 120% and 130%.
[0117] Example 4
[0118] In this embodiment, a method for preparing mycelium leather based on hydrophobic treatment is provided, and the process flow of the method is as follows: Figure 1 As shown, the steps are as follows:
[0119] (1) Mechanical water squeezing
[0120] 100 parts by mass of freshly harvested and inactivated mycelium sheets, 100 parts by mass of water, and 0.1 parts by mass of sodium carbonate were placed in a container and soaked at 35°C for 200 min to remove soluble polysaccharides and attached culture medium on the surface of the mycelium sheets and between the mycelium fibers. The mycelium sheets were then washed with deionized water to obtain pretreated mycelium sheets.
[0121] The freshly collected and inactivated mycelium sheets were squeezed with a roller pressure of 15 MPa using a through-type squeezer to squeeze water to a water content of 60 wt% to 70 wt%, thereby obtaining squeezed mycelium sheets.
[0122] (2) Dehydration of solvent and water-absorbing medium
[0123] 100 parts by mass of squeezed mycelium sheets, 300 parts by mass of anhydrous ethanol, and 200 parts by mass of spherical zeolite particles with a particle size of approximately 8 to 10 mm were placed in a sealed container and allowed to stand at 50°C for 100 minutes for dehydration. The mixture was then centrifuged to remove most of the anhydrous ethanol in the mycelium sheets and the zeolite particles attached to the mycelium sheets. The mycelium sheets obtained by centrifugation were heated to 80°C and maintained at this temperature until the anhydrous ethanol in the mycelium sheets was completely removed, thereby obtaining dehydrated mycelium sheets.
[0124] The liquid phase obtained by centrifugation in this step is collected, and the collected liquid phase is distilled to recover anhydrous ethanol, and the recovered anhydrous ethanol is recycled. The anhydrous ethanol volatilized during the heating process of the mycelium pieces obtained by centrifugation at 80°C is collected and recycled. The zeolite particles obtained by centrifugation are recovered, heated to remove water therein, and then regenerated and recycled.
[0125] (3) Plasticization and hydrophobic treatment
[0126] Thoroughly mix 15 parts by mass of OMBRELLON 072, 4 parts by mass of Silok 8008, and 8 parts by mass of dimethyl silicone oil. Add the resulting mixture to 250 parts by mass of hot water at 70°C and stir to emulsify to obtain a plasticizing and hydrophobizing agent. Place the plasticizing and hydrophobizing agent and 100 parts by mass of dehydrated mycelium sheets in a rotating drum. Rotate the drum intermittently at 6 rpm for 8 hours (10 minutes per hour) at a constant temperature of 35°C until the skins are removed, yielding plasticized and hydrophobized mycelium shells.
[0127] (5) Drying and finishing
[0128] The plasticized and hydrophobized leather blank is dried, rehumidified, softened and shaved according to conventional operations to obtain mycelium leather.
[0129] The mycelium leather prepared in this example exhibited a natural grain texture and a soft feel, with a slightly astringent grain and a velvety inner layer. Compared to Example 1, the mycelium leather prepared in this example was slightly less full-bodied. Static water absorption testing of the mycelium leather prepared in this example showed a static water absorption rate between 125% and 135%.
[0130] Example 5
[0131] In this embodiment, a method for preparing mycelium leather based on hydrophobic treatment is provided, and the process flow of the method is as follows: Figure 1 As shown, the steps are as follows:
[0132] (1) Mechanical water squeezing
[0133] 100 parts by mass of freshly harvested and inactivated mycelium sheets, 500 parts by mass of water, and 0.4 parts by mass of sodium carbonate were placed in a container and soaked at 80°C for 10 min to remove soluble polysaccharides and attached culture medium on the surface of the mycelium sheets and between the mycelium fibers. The mycelium sheets were then washed with deionized water to obtain pretreated mycelium sheets.
[0134] The pretreated mycelium sheets were squeezed with a roller pressure of 12 MPa using a through-type squeezer to squeeze water to a water content of 40 wt% to 50 wt%, thereby obtaining squeezed mycelium sheets.
[0135] (2) Dehydration of solvent and water-absorbing medium
[0136] 100 parts by mass of squeezed mycelium sheets, 100 parts by mass of methanol, and 150 parts by mass of spherical porous silica gel particles with a particle size of approximately 2 to 4 mm were placed in a sealed container and allowed to stand at room temperature for 150 minutes for dehydration. The mixture was then centrifuged to remove most of the methanol in the mycelium sheets and the porous silica gel particles attached to the mycelium sheets. The mycelium sheets obtained by centrifugation were heated to 66°C and maintained at this temperature until the methanol in the mycelium sheets was completely removed, thereby obtaining dehydrated mycelium sheets.
[0137] The liquid phase obtained by centrifugation in this step is collected, and the collected liquid phase is distilled to recover methanol and recycled. The methanol volatilized during the heating process of the mycelium pieces obtained by centrifugation at 66°C is collected and recycled. The porous silica gel particles obtained by centrifugation are recovered, heated to remove moisture therein, and then regenerated and recycled.
[0138] (3) Plasticization and hydrophobic treatment
[0139] 12 parts by mass of PERFECTOL HQ, 10 parts by mass of Silok 8000, 9 parts by mass of N-β-aminoethyl-γ-aminopropylmethyldimethoxysilane (KH602), and 6 parts by mass of hydroxy silicone oil were thoroughly mixed and added to 300 parts by mass of hot water at 80°C, stirred and emulsified to obtain a plasticizing and hydrophobizing agent. The plasticizing and hydrophobizing agent and 100 parts by mass of dehydrated mycelium sheets were placed in a rotating drum. The drum was rotated intermittently at 4 rpm for 2 hours at a constant temperature of 60°C (10 minutes per hour) to remove the skins, resulting in plasticized and hydrophobized mycelium skins.
[0140] (5) Drying and finishing
[0141] The plasticized and hydrophobized leather blank is dried, rehumidified, softened and shaved according to conventional operations to obtain mycelium leather.
[0142] The mycelium leather prepared in this example has a natural grain texture and a soft feel, and the inner layer has a velvety touch. The mycelium leather prepared in this example was tested for static water absorption, and the results showed that its static water absorption rate was between 115% and 125%.
Claims
1. A method for preparing a hydrophobically treated mycelium leather, characterized in that: The following steps are involved: (1) Mechanical water squeezing Mechanically squeezing water from freshly harvested and inactivated mycelium sheets or pretreated mycelium sheets until the water content is 40 wt % to 70 wt %, thereby obtaining squeezed mycelium sheets; (2) Dehydration of solvent and water-absorbing medium 100 parts by weight of the squeezed mycelium sheet, 100-300 parts by weight of a hydrophilic solvent, and 100-200 parts by weight of a water-absorbing medium are placed in a dehydration container, and the mixture is allowed to stand at room temperature to 50°C for 30-150 minutes for dehydration, followed by centrifugation. The mycelium sheet obtained by centrifugation is heated to remove the hydrophilic solvent from the mycelium sheet, thereby obtaining a dehydrated mycelium sheet; (3) Plasticization and hydrophobic treatment 6-40 parts by mass of a silicon-containing polymer material, 1-10 parts by mass of a silicon-based wetting agent, 8-30 parts by mass of a silane coupling agent and / or silicone oil are dissolved or fully dispersed in 60-300 parts by mass of a solvent to obtain a plasticizing and hydrophobizing treatment agent; the obtained plasticizing and hydrophobizing treatment agent and 100 parts by mass of dehydrated mycelium sheets are placed in a rotary drum, and the drum is rotated at a constant temperature of 35-60° C. for 2-8 hours to remove the skin, thereby obtaining a plasticized and hydrophobized mycelium skin blank; (4) Drying and finishing The hydrophobically treated mycelium skin is dried and finished to obtain mycelium leather.
2. The method for preparing the hydrophobically treated mycelium leather according to claim 1, wherein: The silicon-containing polymer material in step (3) includes at least one of OMBRELLON 072, PERFECTOL HQ, and PERFECTOL QX.
3. The method for preparing the hydrophobically treated mycelium leather according to claim 1, wherein: The silicon-based wetting agent in step (3) is Silok 8008 or Silok 8000.
4. The method for preparing the hydrophobic treated mycelium leather according to claim 1, characterized in that: The silane coupling agent in step (3) includes at least one of N-β-aminoethyl-γ-aminopropylmethyldimethoxysilane, γ-aminopropyltriethoxysilane, and N-β-aminoethyl-γ-aminopropyltrimethoxysilane, and the silicone oil includes at least one of hydrogenated silicone oil, hydroxy silicone oil, and dimethyl silicone oil.
5. The method for preparing hydrophobically treated mycelium leather according to any one of claims 1 to 4, characterized in that: The water-absorbing medium in step (2) includes zeolite, porous silica gel or color-changing silica gel, and the water-absorbing medium is in the form of spherical particles.
6. The method for preparing the hydrophobically treated mycelium leather according to claim 5, characterized in that: The particle size of the water absorbing medium is 2-10 mm.
7. The method for preparing hydrophobically treated mycelium leather according to any one of claims 1 to 4, characterized in that: The hydrophilic solvent in step (2) is an organic solvent that is miscible with water and has a boiling point not exceeding 90°C.
8. The method for preparing hydrophobically treated mycelium leather according to any one of claims 1 to 4, characterized in that: The liquid phase obtained by centrifugation in step (2) is collected, the hydrophilic solvent in the liquid phase is recovered and the recovered hydrophilic solvent is recycled, and the water-absorbing medium obtained by centrifugation in step (2) after absorbing water is collected, heated and regenerated, and then recycled.
9. The method for preparing hydrophobically treated mycelium leather according to any one of claims 1 to 4, characterized in that: The preparation method of the pretreated mycelium sheet in step (1) is as follows: 100 parts by mass of freshly collected and inactivated mycelium sheets, 100-500 parts by mass of water and 0.1-0.4 parts by mass of alkaline material are put into a pretreatment container, soaked at 35-80°C for 10-200 minutes, and then washed with water to obtain the pretreated mycelium sheet.
10. Mycelium-based leather prepared according to the method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Engineered composite materials
CN112996922A
Methods of generating mycelium materials with improved properties
CN113195211A
Composition for improving environmental impact of textiles and leathers
CN118076777A
Solid TCMTB formulations
US6241994B1