An ultra-low loss optical fiber for computing networks and its fabrication method

By introducing a linear refractive index profile and alkali metal oxide doping into the optical fiber structure, and combining it with PCVD to prepare optical fiber preforms, the problems of nonlinear effects and Rayleigh scattering loss in ultra-low loss optical fibers in computing networks have been solved, enabling low-loss transmission over longer distances and reducing production costs.

CN120595424BActive Publication Date: 2026-11-10FIBERHOME TELECOMMUNICATION TECHNOLOGIES CO LTD +2
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202510785050.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-06-12
Publication Date
2026-11-10
Estimated Expiration
2045-06-12

AI Technical Summary

Technical Problem

Existing ultra-low loss optical fibers suffer from nonlinear effects in computing networks, resulting in low incident light power and limited transmission distance without repeaters. Furthermore, they exhibit high Rayleigh scattering loss, making it difficult to meet the requirements for low-loss transmission across the O+E+S+C+L wideband.

Method used

By employing a core layer, auxiliary core layer, recessed cladding, and outer cladding structure arranged radially from the inside to the outside of the optical fiber, and by doping alkali metal oxides in the core layer and introducing a linear refractive index profile design in the transition layer, combined with PCVD method for simultaneous doping of alkali metal oxides, an optical fiber preform with uniform alkali metal doping was fabricated.

Benefits of technology

It significantly increases the effective mode area of ​​optical fiber, suppresses nonlinear effects, reduces Rayleigh scattering loss, enables longer-distance repeaterless transmission, meets the low-loss and wide-band transmission requirements of computing networks, and reduces production costs and maintenance complexity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120595424B_ABST
    Figure CN120595424B_ABST
Patent Text Reader

Abstract

This application relates to an ultra-low loss optical fiber for computing networks and its fabrication method. The fiber comprises a core layer, an auxiliary core layer, a recessed cladding layer, and an outer cladding layer arranged radially from the inside out. A first transition layer is provided between the core layer and the auxiliary core layer, a second transition layer between the auxiliary core layer and the recessed cladding layer, and a third transition layer between the recessed cladding layer and the outer cladding layer. The core layer is made of pure quartz glass doped with alkali metal oxides or fluorine-doped quartz glass doped with alkali metal oxides. The auxiliary core layer, recessed cladding layer, and outer cladding layer are made of fluorine-doped quartz glass. The refractive index of the auxiliary core layer increases linearly from the inside out along the radial direction of the fiber. This application can solve the problem in related technologies where the nonlinear effect of ultra-low loss optical fibers leads to low incident light power and limited transmission distance without repeaters.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of single-mode optical fiber in optical communication, and in particular to an ultra-low loss optical fiber for computing networks and its fabrication method. Background Technology

[0002] With the rapid development of next-generation information technologies such as big data, artificial intelligence, and machine learning, global data traffic is experiencing exponential growth. In computing network infrastructure, the transmission rate of optical communication systems is evolving towards 400Gbps and even 1Tbps. However, existing optical network architectures based on standard single-mode fiber (G.652.D) face a significant increase in the required optical signal-to-noise ratio when using higher-order modulation formats, leading to a sharp decrease in repeaterless transmission distance as the data rate increases. This technological bottleneck severely restricts the development of ultra-high-speed, ultra-long-distance optical transmission.

[0003] Ultra-low loss optical fiber, with its breakthrough attenuation coefficient and large effective area, offers a new technological approach to solving this critical problem. Compared to traditional G.652.D fiber, ultra-low loss optical fiber can significantly increase the transmission distance of high-speed optical communication systems, effectively reduce the deployment density of relay stations, and decrease investment and maintenance costs for relay equipment. Furthermore, the large effective area design can significantly suppress nonlinear effects, further enhancing system capacity.

[0004] In the specific application scenario of computing networks, ultra-low loss optical fiber has unique technical advantages. Its excellent transmission performance can effectively support distributed computing and meet the stringent requirements of low latency and high bandwidth for applications such as artificial intelligence training and scientific computing. At the same time, by reducing the density of relay nodes, the energy consumption and operation and maintenance complexity of data center interconnection can be significantly reduced.

[0005] However, there are still many problems to be solved before ultra-low loss optical fibers can be widely used in computing networks.

[0006] For example, Rayleigh scattering loss is high, making it difficult to meet the requirements of low-loss transmission in the O+E+S+C+L wideband of computing networks.

[0007] For example, nonlinear effects result in lower incident light power, limiting the transmission distance without relays. Summary of the Invention

[0008] This application provides an ultra-low loss optical fiber for computing networks and its fabrication method to solve the problem in related technologies where the nonlinear effect of ultra-low loss optical fibers leads to low incident light power and limited transmission distance without relays.

[0009] In a first aspect, an ultra-low loss optical fiber for computing networks is provided, comprising: a core layer, an auxiliary core layer, a recessed cladding layer and an outer cladding layer arranged sequentially from the inside to the outside along its radial direction, wherein a first transition layer is provided between the core layer and the auxiliary core layer, a second transition layer is provided between the auxiliary core layer and the recessed cladding layer, and a third transition layer is provided between the recessed cladding layer and the outer cladding layer. The core layer is made of pure quartz glass doped with alkali metal oxides or fluorine-doped quartz glass doped with alkali metal oxides, and the auxiliary core layer, the recessed cladding layer and the outer cladding layer are made of fluorine-doped quartz glass. The refractive index of the auxiliary core layer increases linearly from the inside to the outside along the radial direction of the optical fiber.

[0010] In some embodiments, the thickness ΔR1 of the core layer is 6–8 μm; And / or, the relative refractive index difference Δn1 of the core layer is 0 to -0.1%; And / or, the concentration of alkali metal doped in the core layer is 200 to 500 ppm.

[0011] In some embodiments, the relative refractive index difference of the first transition layer is Δn2; Δn2=a2+b2(x2 3 +x2 5 ), where x2 is the radial distance from any point in the first transition layer to the outer edge of the core layer, a2 and b2 are transition coefficients, with a2 ranging from -0.04% to -0.06% and b2 ranging from -0.11% to -0.17%.

[0012] In some embodiments, the thickness ΔR2 of the auxiliary core layer is 5–7 μm; And / or, the relative refractive index difference of the auxiliary core layer is Δn3, Δn3=a3+b3x3, where x3 is the radial distance from any point in the auxiliary core layer to the outer edge of the first transition layer, a3 and b3 are linear coefficients, the value of a3 is in the range of -0.3% to -0.4%, and the value of b3 is in the range of 0.015% to 0.023%.

[0013] In some embodiments, the relative refractive index difference of the second transition layer is Δn4; Δn4=a4+b4x4 3 , where x4 is the radial distance from any point in the second transition layer to the outer edge of the auxiliary core layer, a4 and b4 are transition coefficients, with a4 ranging from -0.1% to -0.3% and b4 ranging from -0.18% to -0.28%.

[0014] In some embodiments, the thickness ΔR3 of the sunken cladding is 3–5 μm; And / or, the relative refractive index difference Δn5 of the sunken cladding is -0.4% to -0.5%.

[0015] In some embodiments, the relative refractive index difference of the third transition layer is Δn6; Δn6=a6+b6x6 3 , where x6 is the radial distance from any point in the third transition layer to the inner edge of the outer cladding layer, a6 and b6 are transition coefficients, with a6 ranging from -0.19% to -0.29% and b6 ranging from -0.1% to -0.2%.

[0016] In some embodiments, the outer cladding layer has a diameter of 125 μm; And / or, the relative refractive index difference Δn7 of the outer cladding is -0.2% to -0.3%.

[0017] Secondly, a method for fabricating ultra-low loss optical fiber for computing networks as described in any of the above-mentioned methods is provided, comprising: While depositing the core layer in the reaction zone using the PCVD method, heated alkali metal halide vapor is blown into the reaction zone by a carrier gas so that the alkali metal oxide generated by the reaction is solidified together with the reactants on the inner wall of the fluorine-doped reaction tube to obtain an alkali metal oxide doped preform. The alkali metal oxide-doped preform is sleeved to obtain an optical fiber preform. Melting and drawing are used to obtain ultra-low loss optical fiber for computing networks.

[0018] In some embodiments, an alkali metal oxide doping apparatus is provided, the alkali metal oxide doping apparatus including a feeding device, a conveying pipe, a crucible and a heating electrode, the crucible being located inside the reaction tube of a PCVD deposition apparatus and between an inlet rotary seal chuck and a holding furnace, the heating electrode being located on the inner wall of the crucible, one end of the conveying pipe passing through the reaction tube and communicating with the crucible, and the other end being used to input carrier gas, the feeding device being communicated with the conveying pipe; While the reactants are introduced into the reaction tube, the carrier gas blown into the crucible is heated into alkali metal halide vapor using the heating electrode and then blown into the reaction zone.

[0019] The beneficial effects of the technical solution provided in this application include: This application introduces a linear refractive index profile into the transitional auxiliary core layer, which can significantly increase the effective mode area of ​​ultra-low loss optical fiber, suppress nonlinear effects, increase incident light power, and achieve repeaterless transmission over longer distances.

[0020] This application dops alkali metal oxides in the core layer to reduce Rayleigh scattering loss in the optical fiber. By designing the refractive index profile, the normalized frequency V value is made smaller, which lowers the cutoff wavelength and meets the requirements of O+E+S+C+L wideband low-loss transmission of computing networks. Attached Figure Description

[0021] To more clearly illustrate the technical solutions in the embodiments of this application, the accompanying drawings used in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0022] Figure 1 A refractive index profile of the ultra-low loss optical fiber provided in the embodiments of this application; Figure 2 The PCVD deposition and doping apparatus provided in the embodiments of this application.

[0023] In the diagram: 1. Core layer; 2. First transition layer; 3. Auxiliary core layer; 4. Second transition layer; 5. Sunken cladding layer; 6. Third transition layer; 7. Outer cladding layer; 11. Feeding device; 12. Conveying pipe; 13. Crucible; 14. Heating electrode; 15. Reaction tube; 16. Inlet rotary sealing chuck; 17. Insulation furnace; 18. Microwave resonant cavity; 19. Exhaust rotary sealing chuck. Detailed Implementation

[0024] To make the objectives, technical solutions, and advantages of the embodiments of this application clearer, the technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, not all embodiments. Based on the embodiments of this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application.

[0025] To facilitate understanding of this application, the technical terms used in this application are defined as follows: Core layer: Located at the center of the optical fiber core, it is made of pure quartz glass doped with alkali metal oxides or fluorine-doped quartz glass doped with alkali metal oxides, and is the main area for optical signal transmission. Auxiliary core layer: The annular region located outside the core layer is made of fluorine-doped quartz glass and is used to control the effective area of ​​the mode field; Depressed cladding: A ring-shaped region located outside the auxiliary core layer, which is made of deeply fluorine-doped quartz glass and is used to cut off the distribution of the mode field and improve the bending resistance of the optical fiber. Outer cladding: The annular region located outside the depressed cladding is made of fluorine-doped silica glass and is used to achieve total internal reflection, confining the mode within the optical fiber; Relative refractive index difference:

[0026] n iThe refractive index of the corresponding region compared to pure quartz glass n0 at a wavelength of 1550 nm.

[0027] n1 and Δn1 represent the refractive index of the core layer and its relative refractive index difference with pure quartz glass, respectively; n2 and Δn2 represent the refractive index of the first transition layer and its relative refractive index difference with pure quartz glass, respectively; n3 and Δn3 represent the refractive index of the auxiliary core layer and its relative refractive index difference with pure quartz glass, respectively; n4 and Δn4 represent the refractive index of the second transition layer and its relative refractive index difference with pure quartz glass, respectively; n5 and Δn5 represent the refractive index of the recessed cladding layer and its relative refractive index difference with pure quartz glass, respectively; n6 and Δn6 represent the refractive index of the third transition layer and its relative refractive index difference with pure quartz glass, respectively; and n7 and Δn7 represent the refractive index of the outer cladding layer and its relative refractive index difference with pure quartz glass, respectively.

[0028] See Figure 1 As shown, an ultra-low loss optical fiber for computing networks includes a core layer 1, an auxiliary core layer 3, a recessed cladding layer 5, and an outer cladding layer 7 arranged sequentially from the inside to the outside along its radial direction. A first transition layer 2 is provided between the core layer 1 and the auxiliary core layer 3, a second transition layer 4 is provided between the auxiliary core layer 3 and the recessed cladding layer 5, and a third transition layer 6 is provided between the recessed cladding layer 5 and the outer cladding layer 7. The core layer 1 is made of pure quartz glass doped with alkali metal oxides or fluorine-doped quartz glass doped with alkali metal oxides, and the auxiliary core layer, the recessed cladding layer, and the outer cladding layer are made of fluorine-doped quartz glass. The refractive index of the auxiliary core layer 3 increases linearly from the inside to the outside along the radial direction of the optical fiber.

[0029] This application introduces a linear refractive index profile into the transitional auxiliary core layer, which reduces the equivalent refractive index difference of the fiber and weakens the light-binding ability of the fiber waveguide structure, significantly increasing the effective mode area of ​​the fundamental mode in ultra-low loss fibers. Since the nonlinear coefficient in an optical fiber is inversely proportional to the effective mode area, a larger effective mode area results in a smaller nonlinear coefficient, weakening the nonlinear effects of the fiber and allowing for greater input power. Therefore, this application can suppress nonlinear effects and increase incident light power, enabling longer-distance repeaterless transmission.

[0030] Since linearly increasing the refractive index is more advantageous than linearly constant or linearly decreasing in reducing the equivalent refractive index difference of the optical fiber, it can further improve the effective mode area. Therefore, the refractive index of the auxiliary core layer 3 in this application adopts a linearly increasing change method.

[0031] This application dops alkali metal oxides in the core layer to reduce Rayleigh scattering loss in the optical fiber. By designing the refractive index profile, the normalized frequency V value is made smaller, which lowers the cutoff wavelength and meets the requirements of O+E+S+C+L wideband low-loss transmission of computing networks.

[0032] The aforementioned alkali metal oxides include one or a mixture of K2O, Na2O, Li2O, Rb2O, and Cs2O.

[0033] In some embodiments, the thickness ΔR1 of the core layer 1 is 6 to 8 μm.

[0034] The relative refractive index difference Δn1 of the core layer 1 is 0 to -0.1%.

[0035] The concentration of alkali metal doped in the core layer 1 is 200–500 ppm.

[0036] In some embodiments, the relative refractive index difference of the first transition layer 2 is Δn2; Δn2=a2+b2(x2 3 +x2 5 ), where x2 is the radial distance from any point in the first transition layer 2 to the outer edge of the core layer 1, a2 and b2 are transition coefficients used to determine the specific refractive index distribution of the first transition layer 2, a2 ​​represents the relative refractive index difference at the top of the first transition layer 2, and b2 represents the height scaling of the first transition layer 2. The value range of a2 is -0.04% to -0.06%, and the value range of b2 is -0.11% to -0.17%.

[0037] In some embodiments, the thickness ΔR2 of the auxiliary core layer 3 is 5–7 μm; The relative refractive index difference of the auxiliary core layer 3 is Δn3, where Δn3 = a3 + b3x3, x3 is the radial distance from any point in the auxiliary core layer 3 to the outer edge of the first transition layer 2, a3 and b3 are linear coefficients used to determine the specific refractive index distribution of the auxiliary core layer 3, a3 represents the relative refractive index difference at the inner edge of the auxiliary core layer 3, and b3 represents the slope of the relative refractive index difference of the auxiliary core layer 3 as a function of fiber diameter. The value range of a3 is -0.3% to -0.4%, and the value range of b3 is 0.015% to 0.023%.

[0038] In some embodiments, the relative refractive index difference of the second transition layer 4 is Δn4; Δn4=a4+b4x4 3 Where x4 is the radial distance from any point in the second transition layer 4 to the outer edge of the auxiliary core layer 3, and a4 and b4 are transition coefficients used to determine the specific refractive index distribution of the second transition layer 4. a4 represents the relative refractive index difference at the top of the second transition layer 4, and b4 represents the height scaling of the second transition layer 4. The value range of a4 is -0.1% to -0.3%, and the value range of b4 is -0.18% to -0.28%.

[0039] In some embodiments, the thickness ΔR3 of the sunken cladding 5 is 3 to 5 μm; The relative refractive index difference Δn5 of the sunken cladding 5 is -0.4% to -0.5%.

[0040] In some embodiments, the relative refractive index difference of the third transition layer 6 is Δn6; Δn6=a6+b6x6 3 Where x6 is the radial distance from any point in the third transition layer 6 to the inner edge of the outer cladding layer 7, and a6 and b6 are transition coefficients used to determine the specific refractive index distribution of the third transition layer 6. a6 represents the relative refractive index difference at the top of the third transition layer 6, and b6 represents the height scaling of the third transition layer 6. The value range of a6 is -0.19% to -0.29%, and the value range of b6 is -0.1% to -0.2%.

[0041] In some embodiments, the outer cladding layer 7 has a diameter of 125 μm; The relative refractive index difference Δn7 of the outer cladding layer 7 is -0.2% to -0.3%.

[0042] To reduce Rayleigh scattering loss in optical fibers, this application dops the core layer with alkali metal oxides. However, during the actual fabrication process, it was found that diffusion doping of alkali metal oxides still presents some challenges. Diffusion of alkali metal oxides into the solidified glass at high temperatures is difficult to achieve uniform doping in the preform core region because diffusion tends to proceed from high-concentration areas to low-concentration areas. Furthermore, the diffusion depth of alkali metal oxides in the solidified glass is limited due to the difficulty in diffusion, making it challenging to achieve uniform doping of alkali metal oxides in large-diameter preforms.

[0043] To prepare large-diameter core preforms, the process was improved by dividing the core into two parts for doping, with each part containing a different amount of dopant. This resulted in lower decay and the production of large-diameter alkali metal oxide doped preforms. However, the manufacturing process was complex and the production cycle was long.

[0044] To address the challenges of achieving uniform doping in the preform core region using diffusion methods for alkali metal oxides, and the limited diffusion depth of alkali metal oxides, this application provides a method for fabricating ultra-low loss optical fibers for computing networks, comprising: 101: While depositing the core layer in the reaction zone using the PCVD method, heated alkali metal halide vapor is blown into the reaction zone through a carrier gas, so that the alkali metal oxide generated by the reaction is solidified together with the reactants on the inner wall of the fluorine-doped reaction tube to obtain an alkali metal oxide doped preform.

[0045] 102: The alkali metal oxide doped preform is sleeved to obtain an optical fiber preform.

[0046] 103: Melting and drawing to obtain ultra-low loss optical fiber for computing networks.

[0047] By simultaneously introducing alkali metal halide vapor into the deposition core layer and controlling the feed rate of alkali metal halide and the carrier gas flow rate, the content of alkali metal oxides in the reactants can be precisely controlled, achieving uniform and quantitative doping of alkali metal oxides. At the same time, the problem of limited diffusion depth of alkali metal oxides can be overcome, resulting in large-size alkali metal oxide doped preforms.

[0048] Specifically, see Figure 2 As shown, a PCVD deposition and doping apparatus is provided, which adds an alkali metal oxide doping device to the PCVD deposition apparatus. During the deposition process, alkali metal oxides are doped into the core layer to reduce the viscosity of the core layer and achieve viscosity matching between the core layer and the cladding, thereby manufacturing an alkali metal oxide-doped optical fiber preform, which is then sleeving and drawn into an ultra-low loss optical fiber.

[0049] The alkali metal oxide doping device includes a feeding device 11, a conveying pipe 12, a crucible 13, and a heating electrode 14. The crucible 13 is located inside the reaction tube 15 of the PCVD deposition apparatus and between the inlet rotary sealing chuck 16 and the holding furnace 17. The heating electrode 14 is located on the inner wall of the crucible 13. One end of the conveying pipe 12 passes through the reaction tube 15 and connects to the crucible 13, while the other end is used to input carrier gas. The feeding device 11 is connected to the conveying pipe 12. The carrier gas blows the alkali metal halide fed by the feeding device 11 into the conveying pipe 12 and into the space between the heating electrodes 14. The reaction gas enters from the side at the inlet end, which is connected to the inlet rotary sealing chuck 16. The exhaust rotary sealing chuck 19 is connected to the vacuum pump system through an exhaust pipe. The inlet rotary sealing chuck 16 and the exhaust rotary sealing chuck 19 are respectively connected to a synchronous rotary drive device. A microwave resonant cavity 18 is provided between the two rotary sealing chucks.

[0050] While the reactants are introduced into the reaction tube 15, the carrier gas blown into the crucible 13 by the heating electrode 14 is heated into alkali metal halide vapor and then blown into the reaction zone.

[0051] The feeding device 11 feeds the alkali metal halide into the conveying pipe 12 at a feed rate of 1 to 100 mg / min.

[0052] The carrier gas is O2 gas, which is fed into the conveying pipeline by the feeding device 11 at a flow rate of 1500-3000 mL / min to blow the alkali metal halide into the crucible 13.

[0053] The heating electrode 14 has a feedback adjustment system that can maintain the temperature fluctuation within ±1℃ of the set value. The heating electrode 14 heats the crucible 13 to 850-1000℃. The alkali metal halide blown into the crucible 13 is rapidly heated into alkali metal halide vapor. The alkali metal halide vapor is blown into the reaction zone to participate in the reaction, generating alkali metal oxide, which is solidified together with the reactants on the inner wall of the fluorine-doped reaction tube to obtain an alkali metal oxide-doped preform.

[0054] The crucible 13 has a U-shaped structure, which confines the alkali metal halide to a very small area, making the alkali metal halide heat more uniformly and facilitating the uniform doping of alkali metal oxides.

[0055] In summary, the ultra-low loss optical fiber provided in this application has an attenuation value of ≤0.157dB / km at a wavelength of 1550nm and an attenuation value of ≤0.29dB / km at a wavelength of 1383nm, achieving low-attenuation transmission in the O+E+S+C+L bands and meeting the requirements for long-distance data transmission in computing networks.

[0056] In the PCVD deposition process, this application uniformly dops alkali metal oxides into the preform, overcoming the problem of uneven alkali metal concentration distribution during diffusion doping and further reducing optical fiber loss. The alkali metal oxide doping region of the optical fiber preform is controllable. When the core layer is deposited, the feeding device is turned on to obtain an optical fiber preform with only the core layer doped with alkali metal oxide. By controlling the feeding speed of the feeding device, the flow rate of the carrier gas, and the temperature of the heating electrode, the doping concentration of the alkali metal oxide in the core layer can be precisely controlled. Unaffected by the diffusion depth of alkali metal oxides, uniform doping of large core diameter preforms can be achieved, reducing the production cost of optical fibers; The deposition and alkali metal oxide doping processes of optical fiber preforms are carried out simultaneously, eliminating the need for an additional alkali metal oxide doping process and shortening the production cycle of optical fiber preforms.

[0057] Example 1: like Figure 1 As shown, the relative refractive index difference of the first transition layer is Δn2, which is expressed as Δn2 = a2 + b2(x2) 3 +x2 5 The transition coefficient is calculated as follows: x2 is the radial distance from any point in the first transition layer to the outer edge of the core layer, a2 and b2 are transition coefficients, a2 is -0.05% and b2 is -0.14%.

[0058] The relative refractive index difference of the second transition layer is Δn4, which is expressed as Δn4 = a4 + b4x4. 3The result is achieved by setting x4 to the radial distance from any point in the second transition layer to the outer edge of the auxiliary core layer, and a4 and b4 to the transition coefficients, where a4 is -0.2% and b4 is -0.23%.

[0059] The relative refractive index difference of the third transition layer is Δn6, which is expressed as Δn6 = a6 + b6x6. 3 The implementation is achieved, where x6 is the radial distance from any point in the third transition layer to the inner edge of the outer cladding layer, and a6 and b6 are transition coefficients, with a6 taking the value of -0.24% and b6 taking the value of -0.15%.

[0060] The core layer has a thickness ΔR1 of 7 μm and a relative refractive index difference Δn1 of -0.05%.

[0061] The thickness ΔR2 of the auxiliary core layer is 6 μm, and the relative refractive index difference is Δn3, which is achieved by Δn3=a3+b3x3, where x3 is the radial distance from any point in the auxiliary core layer to the outer edge of the first transition layer, and a3 and b3 are linear coefficients, with a3 taking the value of -0.35% and b3 taking the value of 0.019%.

[0062] The thickness of the sunken cladding ΔR3 is 4 μm, and the relative refractive index difference Δn5 is -0.45%.

[0063] The outer cladding layer has a diameter of 125 μm and a relative refractive index difference Δn7 of -0.24%.

[0064] The core layer is pure quartz glass doped with alkali metal oxides or micro-fluorine-doped quartz glass, and the auxiliary core layer, the recessed cladding, and the outer cladding are fluorine-doped quartz glass. The concentration of alkali metal doped in the core layer of the optical fiber preform is 500 ppm.

[0065] The feeding device feeds the alkali metal halide into the conveying pipeline at a feed rate of 18 mg / min, the carrier gas flow rate is 2000 mL / min, and the heating electrode heats the crucible to 900°C.

[0066] The ultra-low loss optical fiber has an attenuation of 0.153 dB / km at a wavelength of 1550 nm and an attenuation of ≤0.27 dB / km at a wavelength of 1383 nm.

[0067] Example 2: This example is basically the same as Example 1, except that the relative refractive index difference of the first transition layer is Δn2, which is expressed as Δn2 = a2 + b2(x2) 3 +x2 5 The transition coefficient is calculated as follows: x2 is the radial distance from any point in the first transition layer to the outer edge of the core layer, a2 and b2 are transition coefficients, a2 is -0.06% and b2 is -0.15%.

[0068] The relative refractive index difference of the second transition layer is Δn4, which is expressed as Δn4 = a4 + b4x4. 3 The result is achieved by setting x4 to the radial distance from any point in the second transition layer to the outer edge of the auxiliary core layer, and a4 and b4 to the transition coefficients, with a4 taking the value of -0.22% and b4 taking the value of -0.18%.

[0069] The relative refractive index difference of the third transition layer is Δn6, which is expressed as Δn6 = a6 + b6x6. 3 The implementation is achieved, where x6 is the radial distance from any point in the third transition layer to the inner edge of the outer cladding layer, and a6 and b6 are transition coefficients, with a6 taking the value of -0.22% and b6 taking the value of -0.18%.

[0070] The core layer has a thickness ΔR1 of 6 μm and a relative refractive index difference Δn1 of -0.06%.

[0071] The thickness ΔR2 of the auxiliary core layer is 6 μm, and the relative refractive index difference is Δn3, which is achieved by Δn3=a3+b3x3, where x3 is the radial distance from any point in the auxiliary core layer to the outer edge of the first transition layer, and a3 and b3 are linear coefficients, with a3 taking the value of -0.36% and b3 taking the value of 0.023%.

[0072] The thickness of the sunken cladding ΔR3 is 5 μm, and the relative refractive index difference Δn5 is -0.4%.

[0073] The outer cladding layer has a diameter of 125 μm and a relative refractive index difference Δn7 of -0.22%.

[0074] The core layer is pure quartz glass doped with alkali metal oxides or micro-fluorine-doped quartz glass, and the auxiliary core layer, the recessed cladding, and the outer cladding are fluorine-doped quartz glass. The concentration of alkali metal doped in the core layer of the optical fiber preform is 300 ppm.

[0075] The feeding device feeds the alkali metal halide into the conveying pipeline at a feed rate of 15 mg / min, the carrier gas flow rate is 2200 mL / min, and the heating electrode heats the crucible to 950°C.

[0076] The ultra-low loss optical fiber has an attenuation of 0.156 dB / km at a wavelength of 1550 nm and an attenuation of ≤0.29 dB / km at a wavelength of 1383 nm.

[0077] In the description of this application, it should be noted that the terms "upper," "lower," etc., indicating the orientation or positional relationship are based on the orientation or positional relationship shown in the accompanying drawings, and are only for the convenience of describing this application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation, and therefore should not be construed as a limitation of this application. Unless otherwise expressly specified and limited, the terms "installed," "connected," and "linked" should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral connection; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium; they can refer to the internal communication between two elements. For those skilled in the art, the specific meaning of the above terms in this application can be understood according to the specific circumstances.

[0078] It should be noted that in this application, relational terms such as "first" and "second" are used merely to distinguish one entity or operation from another, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Furthermore, the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such a process, method, article, or apparatus. Without further limitations, an element defined by the phrase "comprising one..." does not exclude the presence of other identical elements in the process, method, article, or apparatus that includes said element.

[0079] The above description is merely a specific embodiment of this application, enabling those skilled in the art to understand or implement this application. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of this application. Therefore, this application is not to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features claimed herein.

Claims

1. An ultra-low loss optical fiber for computing power networks, characterized in that, It includes: a core layer (1), an auxiliary core layer (3), a sunken cladding layer (5) and an outer cladding layer (7) arranged in sequence from the inside to the outside along its radial direction; a first transition layer (2) is provided between the core layer (1) and the auxiliary core layer (3); a second transition layer (4) is provided between the auxiliary core layer (3) and the sunken cladding layer (5); and a third transition layer (6) is provided between the sunken cladding layer (5) and the outer cladding layer (7). The core layer (1) is made of pure quartz glass doped with alkali metal oxides or fluorine-doped quartz glass doped with alkali metal oxides, and the auxiliary core layer (3), the recessed cladding layer (5) and the outer cladding layer (7) are made of fluorine-doped quartz glass. The refractive index of the auxiliary core layer (3) increases linearly from the inside to the outside along the radial direction of the optical fiber; The thickness ΔR1 of the core layer (1) is 6-8 μm; The relative refractive index difference Δn1 of the core layer (1) is 0 to -0.1%; The concentration of alkali metal doped in the core layer (1) is 200–500 ppm; The relative refractive index difference of the first transition layer (2) is Δn2; Δn2=a2+b2(x2 3 +x2 5 ), where x2 is the radial distance from any point in the first transition layer (2) to the outer edge of the core layer (1), a2 and b2 are transition coefficients, with a2 ranging from -0.04% to -0.06% and b2 ranging from -0.11% to -0.17%; The thickness ΔR2 of the auxiliary core layer (3) is 5-7 μm; The relative refractive index difference of the auxiliary core layer (3) is Δn3, where Δn3 = a3 + b3x3, x3 is the radial distance from any point in the auxiliary core layer (3) to the outer edge of the first transition layer (2), a3 and b3 are linear coefficients, a3 ranges from -0.3% to -0.4%, and b3 ranges from 0.015% to 0.023%. The relative refractive index difference of the second transition layer (4) is Δn4; Δn4=a4+b4x4 3 Where x4 is the radial distance from any point in the second transition layer (4) to the outer edge of the auxiliary core layer (3), and a4 and b4 are transition coefficients, with a4 ranging from -0.1% to -0.3% and b4 ranging from -0.18% to -0.28%. The thickness ΔR3 of the sunken cladding (5) is 3 to 5 μm; The relative refractive index difference Δn5 of the sunken cladding (5) is -0.4% to -0.5%. The relative refractive index difference of the third transition layer (6) is Δn6; Δn6=a6+b6x6 3 , where x6 is the radial distance from any point in the third transition layer (6) to the inner edge of the outer cladding layer (7), a6 and b6 are transition coefficients, the value range of a6 is -0.19% to -0.29%, the value range of b6 is -0.1% to -0.2%, and the relative refractive index difference Δn7 of the outer cladding layer (7) is -0.2% to -0.3%.

2. The ultra-low loss optical fiber for computing networks as described in claim 1, characterized in that: The outer cladding layer (7) has a diameter of 125 μm.

3. A method for fabricating ultra-low loss optical fiber for computing networks as described in any one of claims 1 to 2, characterized in that, It includes: While depositing the core layer (1) in the reaction zone using the PCVD method, heated alkali metal halide vapor is blown into the reaction zone by a carrier gas so that the alkali metal oxide generated by the reaction is solidified together with the reactants on the inner wall of the fluorine-doped reaction tube (15) to obtain an alkali metal oxide doped preform. The alkali metal oxide-doped preform is sleeved to obtain an optical fiber preform. Melting and drawing are used to obtain ultra-low loss optical fiber for computing networks.

4. The method for fabricating ultra-low loss optical fiber for computing networks as described in claim 3, characterized in that: An alkali metal oxide doping apparatus is provided, comprising a feeding device (11), a conveying pipe (12), a crucible (13), and a heating electrode (14). The crucible (13) is located inside the reaction tube (15) of the PCVD deposition apparatus and between the gas inlet rotary sealing chuck (16) and the holding furnace (17). The heating electrode (14) is located on the inner wall of the crucible (13). One end of the conveying pipe (12) passes through the reaction tube (15) and is connected to the crucible (13), and the other end is used to input carrier gas. The feeding device (11) is connected to the conveying pipe (12). While the reactants are introduced into the reaction tube (15), the carrier gas is blown into the crucible (13) by the heating electrode (14) to heat the alkali metal halide into alkali metal halide vapor and blown into the reaction zone.

Citation Information

Patent Citations

  • Method for preparing ultra-low attenuation optical fiber

    CN107162401A

  • Method for producing a glass optical fiber preform

    EP2481716A1