A sunshade composite fabric for vehicle sunroofs and its preparation method
By using a three-layer structure of sunshade composite fabric for vehicle sunroofs, especially the combination of modified polycaprolactam and modified titanium dioxide, the problems of sunshade materials being brittle under direct sunlight and lacking impact resistance have been solved, achieving excellent UV resistance and impact resistance.
Patent Information
- Application Number
- CN202510758888.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-06-09
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2045-06-09
AI Technical Summary
Existing sunroof shading materials for vehicles are prone to brittleness under direct sunlight, and since ventilation and protection functions must be balanced, their impact resistance is insufficient.
The sunshade composite fabric for vehicle sunroofs adopts a three-layer structure, including a surface layer, an anti-UV intermediate layer, and a base layer. The anti-UV intermediate layer is composed of modified polycaprolactam and modified titanium dioxide. The toughness is improved by modifiers and siloxane structure, and the nano-titanium dioxide is combined to improve the anti-UV and impact resistance.
It improves the UV resistance and impact resistance of shading materials, and enhances the durability and protective performance of the materials.
Abstract
Description
Technical Field
[0001] This invention relates to the field of composite fabric technology, specifically to a sunshade composite fabric for vehicle sunroofs and its preparation method. Background Technology
[0002] With the rapid development of the automotive industry, consumers have placed higher demands on the comfort, functionality, and aesthetics of car interiors. Sunroofs, in particular, are widely used in vehicle design because they improve interior lighting and ventilation, greatly enhancing the driving and riding experience. However, during sunroof use, vehicles sometimes face direct sunlight, causing increased interior temperature and ultraviolet radiation, which actually reduces the driving and riding experience. Therefore, sunshade materials are often used to block direct sunlight from the sunroof.
[0003] In existing technologies, because sunroofs are located horizontally, sunshade materials need to be exposed to sunlight for a longer period of time. Furthermore, due to their own weight, commonly used vertical sunshade materials are more prone to brittleness. In addition, during daily use, in order to improve ventilation, it may be necessary to open the sunroof and use sunshade materials at the same time. Therefore, sunshade materials for sunroofs also need to take into account certain protective functions for the roof, such as certain impact resistance, to block stones, branches, etc. on the road.
[0004] In summary, the development of a sunshade composite fabric for vehicle sunroofs is of great significance in addressing the aforementioned issues. Summary of the Invention
[0005] The purpose of this invention is to provide a sunshade composite fabric for vehicle sunroofs and its preparation method, so as to solve the problems mentioned in the background art.
[0006] To solve the above-mentioned technical problems, the present invention provides the following technical solution: A sunshade composite fabric for vehicle sunroofs: the composite fabric has a three-layer structure, consisting of a surface layer, an anti-UV intermediate layer, and a base fabric layer bonded together in sequence; The UV-resistant interlayer is made of nylon fiber, and the raw materials of the nylon fiber include the following components: by mass parts, 40-50 parts of polyhexamethylene adipamide, 40-50 parts of modified polycaprolactam, 5-8 parts of modified titanium dioxide, 1-2 parts of antioxidant, and 1-1.5 parts of heat stabilizer.
[0007] Preferred method for preparing the UV-resistant interlayer includes the following steps: mixing polyhexamethylene adipamide, modified polycaprolactam, antioxidant, modified titanium dioxide, and heat stabilizer in a spiral extrusion rod, melt spinning, winding and forming nylon fiber; and weaving to obtain the UV-resistant interlayer.
[0008] Preferred method for preparing the modified polycaprolactam includes the following steps: (1) Under a nitrogen atmosphere, 4,4'-dihydroxybiphenyl, di(4-hydroxyphenyl)acetic acid and triethylamine are added to anhydrous tetrahydrofuran and stirred until homogeneous. Phenylphosphoryl dichloride is slowly added dropwise in an ice-water bath and stirred for 2-2.5 h. The mixture is heated to 70-75°C and stirred for 5-6 h. Hydroxyl-terminated dimethylsiloxane is added and stirred for 10-12 h. The mixture is filtered, the solvent is removed by rotary evaporation, washed, purified, and dried to obtain an anti-ultraviolet agent. (2) Add the UV stabilizer to anhydrous tetrahydrofuran and stir until uniform. Add 1,6-hexamethylene diisocyanate and stir at 60-70°C for 1-1.5 h. Evaporate the solvent to obtain the modifier. (3) Heat caprolactam to 120-130°C. After removing water, divide it into two parts. Add the modifier to one part and sodium hydroxide to the other part. Stir each part for 10-15 min. Mix the two parts evenly and stir at 155-165°C for 30-40 min. Transfer to a screw extruder for extrusion granulation to obtain modified polycaprolactam.
[0009] Preferably, the UV stabilizer comprises the following raw materials, in parts by weight: 4.3-4.5 parts 4,4'-dihydroxybiphenyl, 1.3-1.5 parts di(4-hydroxyphenyl)acetic acid, 3.1-3.3 parts triethylamine, 5.6-5.7 parts phenylphosphodichloro, and 4.8-5.2 parts hydroxyl-terminated dimethylsiloxane; The mass ratio of the UV stabilizer to 1,6-hexamethylene diisocyanate is 10:0.45~0.55; The modified polycaprolactam comprises the following raw materials, by weight: 100 parts caprolactam, 4-6 parts modifier, and 1.5-2 parts sodium hydroxide.
[0010] Preferably, the molecular weight of the hydroxyl-terminated dimethylsiloxane is 3000-4000.
[0011] Preferred method for preparing modified titanium dioxide includes the following steps: (1) adding nano-titanium dioxide to deionized water and dispersing it evenly by ultrasonication, adding anhydrous ethanol and 3-aminopropyltriethoxysilane, filtering, washing, and drying to obtain aminated titanium dioxide; (2) adding aminated titanium dioxide to toluene and dispersing it evenly by ultrasonication, adding 1,6-hexamethylene diisocyanate under a nitrogen atmosphere, stirring at 70-80°C for 1-1.5 h, adding hydroxyl-terminated dimethylsiloxane, stirring at 75-85°C for 30-50 min, adding 1,4-butanediol, 4,4'-dihydroxybenzophenone and dibutyltin dilaurate, stirring at 80-90°C for 1-2 h, filtering, washing, and drying to obtain modified titanium dioxide.
[0012] Preferably, the aminated titanium dioxide comprises the following raw materials, in parts by weight: 1-2 parts nano titanium dioxide, 30-40 parts deionized water, 50-60 parts anhydrous ethanol, and 0.4-0.6 parts 3-aminopropyltriethoxysilane. The modified titanium dioxide comprises the following raw materials, by weight: 1-2 parts aminated titanium dioxide, 40-50 parts toluene, 10-12 parts 1,6-hexamethylene diisocyanate, 25-28 parts hydroxyl-terminated dimethylsiloxane, 2-3 parts 1,4-butanediol, 3-4 parts 4,4'-dihydroxybenzophenone, and 0.01-0.02 parts dibutyltin dilaurate.
[0013] Preferably, during the weaving process, the fiber specifications are 35~50D / 72~96F.
[0014] A preferred method for preparing a sunshade composite fabric for vehicle sunroofs includes the following steps: coating both sides of an anti-UV intermediate layer with hot melt adhesive, layering a surface layer on top of it, layering a base fabric layer on the bottom of it, hot-pressing and curing, and drying to obtain the sunshade composite fabric for vehicle sunroofs.
[0015] Preferably, the surface layer is a PET aluminized film with a thickness of 10~20μm, wherein the aluminum layer thickness is 300~700Å; the base fabric layer is a non-woven fabric with a thickness of 0.05~0.2mm. During the hot-press curing process, the temperature is 160~180℃, the pressure is 3~5MPa, and the time is 1~3min.
[0016] Compared with the prior art, the beneficial effects achieved by the present invention are as follows: The sunshade composite fabric for vehicle sunroofs provided by the present invention is made by bonding a surface layer, an anti-ultraviolet intermediate layer and a base fabric layer. The anti-ultraviolet intermediate layer is made by melt spinning modified polycaprolactam and polyhexamethylene adipamide, and a certain amount of modified titanium dioxide is added, which has excellent impact resistance and anti-ultraviolet properties.
[0017] Among them, the modified polycaprolactam is obtained by copolymerizing caprolactam with a modifier. The preparation process of the modifier is as follows: 4,4'-dihydroxybiphenyl and di(4-hydroxyphenyl)acetic acid react with phenylphosphodichloro under the catalysis of triethylamine to form a phosphorus-containing activator, which then reacts with one end of a hydroxyl-terminated dimethylsiloxane to form an anti-UV agent with a hydroxyl-terminated siloxane chain. The activator is further reacted with 1,6-hexamethylene diisocyanate to obtain the modifier. By introducing a modifier into the copolymer, a polysiloxane structure was introduced, improving the toughness and impact resistance of polycaprolactam. The low surface energy of polysiloxane and the chemical inertness of its siloxane groups to ultraviolet radiation further enhance the UV resistance of polycaprolactam. However, the molecular weight of the polysiloxane needs to be limited to 3000-4000. Excessive molecular weight restricts chain movement, reducing impact resistance, while insufficient molecular weight may lead to microphase separation at the interface, resulting in decreased strength. The introduction of a phosphorus-containing activator significantly improves the material's UV resistance and thermal stability. Furthermore, the introduction of rigid benzene-containing polymer segments synergistically enhances the impact resistance of polycaprolactam with the toughness of the polysiloxane structure. The π electrons in the benzene ring also have a conjugated effect, absorbing UV radiation to some extent and improving UV resistance. Simultaneously, the introduced di(4-hydroxyphenyl)acetic acid, with its carboxyl structure, promotes ring-opening of caprolactam to some extent, increasing polymerization efficiency and thus improving fiber performance.
[0018] The modified titanium dioxide was obtained by introducing an amino group with a silane coupling agent, followed by the addition of 1,6-hexamethylene diisocyanate and hydroxyl-terminated dimethylsiloxane, and then chain extension using 1,4-butanediol and 4,4'-dihydroxybenzophenone. The addition of nano-titanium dioxide significantly improves the material's UV resistance and acts as a stress concentration point when the material is subjected to impact, absorbing and dispersing stress under external force, thus improving impact resistance. The introduction of similar chain segments improves the dispersibility of nano-titanium dioxide in the system, and the benzophenone structure in 4,4'-dihydroxybenzophenone can further enhance the material's UV resistance, thereby improving both UV resistance and impact resistance. Detailed Implementation
[0019] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0020] It should be noted that the following quantities are by weight. There are no special restrictions on the manufacturers from which the raw materials involved in this invention can be purchased. Exemplary examples include: CAS number 92-88-6 for 4,4'-dihydroxybiphenyl; CAS number 40232-93-7 for di(4-hydroxyphenyl)acetic acid; CAS number 121-44-8 for triethylamine; CAS number 824-72-6 for phenylphosphodichloro; CAS number 3000-4000 for hydroxyl-terminated dimethylsiloxane; and CAS number 1,6-hexamethylenediisocyanate. : 822-06-0; CAS number of caprolactam: 105-60-2; Polyhexamethylene adipamide, model ST801, provided by Suzhou Yunmili Plastic Co., Ltd.; Nano titanium dioxide, particle size 20~80nm; CAS number of 3-aminopropyltriethoxysilane: 919-30-2; CAS number of 4,4'-dihydroxybenzophenone: 611-99-4; CAS number of dibutyltin dilaurate: 77-58-7; In the following examples, the above and other raw materials used but not mentioned are all commercially available.
[0021] In each embodiment and comparative example, the antioxidant is GA-80; the heat stabilizer is H3337; the PET aluminized film has a thickness of 10~20μm, wherein the aluminum layer thickness is 300~700Å; and the base fabric is a non-woven fabric with a thickness of 0.05~0.2mm.
[0022] Example 1: The preparation method of sunshade composite fabric for vehicle sunroofs includes the following steps: Step 1: Preparation of modified polycaprolactam: (1) Under a nitrogen atmosphere, 4.4 parts of 4,4'-dihydroxybiphenyl, 1.4 parts of di(4-hydroxyphenyl)acetic acid and 3.2 parts of triethylamine were added to 30 parts of anhydrous tetrahydrofuran and stirred evenly. 5.65 parts of phenylphosphodichlorochloride were slowly added dropwise in an ice-water bath and stirred for 2 hours. The mixture was heated to 70°C and stirred for 5 hours. 5 parts of hydroxyl-terminated dimethylsiloxane were added and stirred for 12 hours. The mixture was filtered, the solvent was removed by rotary evaporation, washed, purified, and dried to obtain the UV inhibitor. (2) Add the UV stabilizer to 30 parts of anhydrous tetrahydrofuran and stir until uniform. Add 1,6-hexanediisocyanate with a mass ratio of 10:0.5 to the UV stabilizer. Stir at 65°C for 1 hour and evaporate the solvent to obtain the modifier. (3) Heat 100 parts of caprolactam to 125°C, remove water, divide into two parts, add 5 parts of modifier to one part and 1.5 parts of sodium hydroxide to the other part, stir each part for 15 minutes, mix the two parts evenly, stir at 160°C for 35 minutes, transfer to a screw extruder for extrusion granulation to obtain modified polycaprolactam.
[0023] Step 2: Preparation of modified titanium dioxide: (1) Add 1.5 parts of nano titanium dioxide to 35 parts of deionized water and ultrasonically disperse evenly. Add 55 parts of anhydrous ethanol and 0.5 parts of 3-aminopropyltriethoxysilane, filter, wash, and dry to obtain aminated titanium dioxide. (2) 1.5 parts of aminated titanium dioxide were added to 45 parts of toluene and ultrasonically dispersed evenly. Under a nitrogen atmosphere, 11 parts of 1,6-hexamethylene diisocyanate were added and stirred at 75°C for 1 h. 26 parts of hydroxyl-terminated dimethylsiloxane were added and stirred at 80°C for 40 min. 2.5 parts of 1,4-butanediol, 3.5 parts of 4,4'-dihydroxybenzophenone and 0.01 parts of dibutyltin dilaurate were added and stirred at 85°C for 1.5 h. The mixture was filtered, washed and dried to obtain modified titanium dioxide. Step 3: Preparation of UV-blocking fabric: 45 parts of polyhexamethylene adipamide, 45 parts of modified polycaprolactam, 6 parts of modified titanium dioxide, 1.5 parts of antioxidant, and 1 part of heat stabilizer are added to a spiral extrusion rod and mixed. The mixture is then melt-spun, wound, and shaped to form nylon fibers. The fibers are then woven to obtain an anti-UV interlayer. The fiber specifications are 40D / 84F. Step 4: Preparation of sunshade composite fabric for vehicle sunroof: hot melt adhesive is coated on both sides of nylon sunshade fabric, a PET aluminized film is stacked on top, and a non-woven fabric is stacked on the bottom. The fabric is then hot-pressed at a pressure of 4MPa and a temperature of 170℃ for 2 minutes and dried to obtain sunshade composite fabric for vehicle sunroof.
[0024] Example 2: The preparation method of sunshade composite fabric for vehicle sunroofs includes the following steps: Step 1: Preparation of modified polycaprolactam: (1) Under a nitrogen atmosphere, 4.4 parts of 4,4'-dihydroxybiphenyl, 1.4 parts of di(4-hydroxyphenyl)acetic acid and 3.2 parts of triethylamine were added to 30 parts of anhydrous tetrahydrofuran and stirred evenly. 5.65 parts of phenylphosphodichlorochloride were slowly added dropwise in an ice-water bath and stirred for 2 hours. The mixture was heated to 70°C and stirred for 5 hours. 5 parts of hydroxyl-terminated dimethylsiloxane were added and stirred for 12 hours. The mixture was filtered, the solvent was removed by rotary evaporation, washed, purified, and dried to obtain the UV inhibitor. (2) Add the UV stabilizer to 30 parts of anhydrous tetrahydrofuran and stir until uniform. Add 1,6-hexanediisocyanate with a mass ratio of 10:0.5 to the UV stabilizer. Stir at 65°C for 1 hour and evaporate the solvent to obtain the modifier. (3) Heat 100 parts of caprolactam to 125°C, remove water, divide into two parts, add 5 parts of modifier to one part and 1.5 parts of sodium hydroxide to the other part, stir each part for 15 minutes, mix the two parts evenly, stir at 160°C for 35 minutes, transfer to a screw extruder for extrusion granulation to obtain modified polycaprolactam.
[0025] Step 2: Preparation of modified titanium dioxide: (1) Add 1.5 parts of nano titanium dioxide to 35 parts of deionized water and ultrasonically disperse evenly. Add 55 parts of anhydrous ethanol and 0.5 parts of 3-aminopropyltriethoxysilane, filter, wash, and dry to obtain aminated titanium dioxide. (2) 1.5 parts of aminated titanium dioxide were added to 45 parts of toluene and ultrasonically dispersed evenly. Under a nitrogen atmosphere, 11 parts of 1,6-hexamethylene diisocyanate were added and stirred at 75°C for 1 h. 26 parts of hydroxyl-terminated dimethylsiloxane were added and stirred at 80°C for 40 min. 2.5 parts of 1,4-butanediol, 3.5 parts of 4,4'-dihydroxybenzophenone and 0.01 parts of dibutyltin dilaurate were added and stirred at 85°C for 1.5 h. The mixture was filtered, washed and dried to obtain modified titanium dioxide. Step 3: Preparation of UV-blocking fabric: 50 parts of polyhexamethylene adipamide, 50 parts of modified polycaprolactam, 8 parts of modified titanium dioxide, 2 parts of antioxidant, and 1.5 parts of heat stabilizer are added to a spiral extruder and mixed. The mixture is then melt-spun, wound, and shaped to form nylon fibers. The fibers are then woven to obtain an anti-UV interlayer. The fiber specifications are 35D / 96F. Step 4: Preparation of sunshade composite fabric for vehicle sunroof: hot melt adhesive is coated on both sides of nylon sunshade fabric, a PET aluminized film is stacked on top, and a non-woven fabric is stacked on the bottom. The fabric is then hot-pressed at a pressure of 4MPa and a temperature of 170℃ for 2 minutes and dried to obtain sunshade composite fabric for vehicle sunroof.
[0026] Example 3: The preparation method of sunshade composite fabric for vehicle sunroofs includes the following steps: Step 1: Preparation of modified polycaprolactam: (1) Under a nitrogen atmosphere, 4.4 parts of 4,4'-dihydroxybiphenyl, 1.4 parts of di(4-hydroxyphenyl)acetic acid and 3.2 parts of triethylamine were added to 30 parts of anhydrous tetrahydrofuran and stirred evenly. 5.65 parts of phenylphosphodichlorochloride were slowly added dropwise in an ice-water bath and stirred for 2 hours. The mixture was heated to 70°C and stirred for 5 hours. 5 parts of hydroxyl-terminated dimethylsiloxane were added and stirred for 12 hours. The mixture was filtered, the solvent was removed by rotary evaporation, washed, purified, and dried to obtain the UV inhibitor. (2) Add the UV stabilizer to 30 parts of anhydrous tetrahydrofuran and stir until uniform. Add 1,6-hexanediisocyanate with a mass ratio of 10:0.5 to the UV stabilizer. Stir at 65°C for 1 hour and evaporate the solvent to obtain the modifier. (3) Heat 100 parts of caprolactam to 125°C, remove water, divide into two parts, add 5 parts of modifier to one part and 1.5 parts of sodium hydroxide to the other part, stir each part for 15 minutes, mix the two parts evenly, stir at 160°C for 35 minutes, transfer to a screw extruder for extrusion granulation to obtain modified polycaprolactam.
[0027] Step 2: Preparation of modified titanium dioxide: (1) Add 1.5 parts of nano titanium dioxide to 35 parts of deionized water and ultrasonically disperse evenly. Add 55 parts of anhydrous ethanol and 0.5 parts of 3-aminopropyltriethoxysilane, filter, wash, and dry to obtain aminated titanium dioxide. (2) 1.5 parts of aminated titanium dioxide were added to 45 parts of toluene and ultrasonically dispersed evenly. Under a nitrogen atmosphere, 11 parts of 1,6-hexamethylene diisocyanate were added and stirred at 75°C for 1 h. 26 parts of hydroxyl-terminated dimethylsiloxane were added and stirred at 80°C for 40 min. 2.5 parts of 1,4-butanediol, 3.5 parts of 4,4'-dihydroxybenzophenone and 0.01 parts of dibutyltin dilaurate were added and stirred at 85°C for 1.5 h. The mixture was filtered, washed and dried to obtain modified titanium dioxide. Step 3: Preparation of UV-blocking fabric: 40 parts of polyhexamethylene adipamide, 40 parts of modified polycaprolactam, 5 parts of modified titanium dioxide, 1 part of antioxidant, and 1 part of heat stabilizer are added to a spiral extrusion rod and mixed. The mixture is then melt-spun, wound, and shaped to form nylon fibers. The fibers are then woven to obtain an anti-UV interlayer. The fiber specifications are 50D / 72F. Step 4: Preparation of sunshade composite fabric for vehicle sunroof: hot melt adhesive is coated on both sides of nylon sunshade fabric, a PET aluminized film is stacked on top, and a non-woven fabric is stacked on the bottom. The fabric is then hot-pressed at a pressure of 4MPa and a temperature of 170℃ for 2 minutes and dried to obtain sunshade composite fabric for vehicle sunroof.
[0028] Comparative Example 1: Based on Example 1, the modified polycaprolactam was replaced with commercially available polycaprolactam, while the rest of the process remained unchanged, as follows: Step 1: Preparation of modified titanium dioxide: (1) Add 1.5 parts of nano titanium dioxide to 35 parts of deionized water and ultrasonically disperse evenly. Add 55 parts of anhydrous ethanol and 0.5 parts of 3-aminopropyltriethoxysilane, filter, wash, and dry to obtain aminated titanium dioxide. (2) 1.5 parts of aminated titanium dioxide were added to 45 parts of toluene and ultrasonically dispersed evenly. Under a nitrogen atmosphere, 11 parts of 1,6-hexamethylene diisocyanate were added and stirred at 75°C for 1 h. 26 parts of hydroxyl-terminated dimethylsiloxane were added and stirred at 80°C for 40 min. 2.5 parts of 1,4-butanediol, 3.5 parts of 4,4'-dihydroxybenzophenone and 0.01 parts of dibutyltin dilaurate were added and stirred at 85°C for 1.5 h. The mixture was filtered, washed and dried to obtain modified titanium dioxide. Step 2: Preparation of UV-blocking fabric: 45 parts of polyhexamethylene adipamide, 45 parts of polycaprolactam, 6 parts of modified titanium dioxide, 1.5 parts of antioxidant, and 1 part of heat stabilizer are added to a spiral extrusion rod and mixed. The mixture is then melt-spun, wound, and shaped to form nylon fibers. The fibers are then woven to obtain an anti-UV interlayer. The fiber specifications are 40D / 84F. Step 3: Preparation of sunshade composite fabric for vehicle sunroof: hot melt adhesive is coated on both sides of nylon sunshade fabric, a PET aluminized film is stacked on top, and a non-woven fabric is stacked on the bottom. The fabric is then hot-pressed at a pressure of 4MPa and a temperature of 170℃ for 2 minutes and dried to obtain sunshade composite fabric for vehicle sunroof.
[0029] Comparative Example 2: Based on Example 1, di(4-hydroxyphenyl)acetic acid was not added during the preparation of the modified polycaprolactam, and the rest of the process remained unchanged, as follows: Step 1: Preparation of modified polycaprolactam: (1) Under a nitrogen atmosphere, 5.8 parts of 4,4'-dihydroxybiphenyl and 3.2 parts of triethylamine were added to 30 parts of anhydrous tetrahydrofuran and stirred evenly. 5.65 parts of phenylphosphodichlorochloride were slowly added dropwise in an ice-water bath and stirred for 2 hours. The mixture was heated to 70°C and stirred for 5 hours. 5 parts of hydroxyl-terminated dimethylsiloxane were added and stirred for 12 hours. The mixture was filtered, the solvent was removed by rotary evaporation, washed, purified, and dried to obtain the UV inhibitor. (2) Add the UV stabilizer to 30 parts of anhydrous tetrahydrofuran and stir until uniform. Add 1,6-hexanediisocyanate with a mass ratio of 10:0.5 to the UV stabilizer. Stir at 65°C for 1 hour and evaporate the solvent to obtain the modifier. (3) Heat 100 parts of caprolactam to 125°C, remove water, divide into two parts, add 5 parts of modifier to one part and 1.5 parts of sodium hydroxide to the other part, stir each part for 15 minutes, mix the two parts evenly, stir at 160°C for 35 minutes, transfer to a screw extruder for extrusion granulation to obtain modified polycaprolactam.
[0030] Step 2: Preparation of modified titanium dioxide: (1) Add 1.5 parts of nano titanium dioxide to 35 parts of deionized water and ultrasonically disperse evenly. Add 55 parts of anhydrous ethanol and 0.5 parts of 3-aminopropyltriethoxysilane, filter, wash, and dry to obtain aminated titanium dioxide. (2) 1.5 parts of aminated titanium dioxide were added to 45 parts of toluene and ultrasonically dispersed evenly. Under a nitrogen atmosphere, 11 parts of 1,6-hexamethylene diisocyanate were added and stirred at 75°C for 1 h. 26 parts of hydroxyl-terminated dimethylsiloxane were added and stirred at 80°C for 40 min. 2.5 parts of 1,4-butanediol, 3.5 parts of 4,4'-dihydroxybenzophenone and 0.01 parts of dibutyltin dilaurate were added and stirred at 85°C for 1.5 h. The mixture was filtered, washed and dried to obtain modified titanium dioxide. Step 3: Preparation of UV-blocking fabric: 45 parts of polyhexamethylene adipamide, 45 parts of modified polycaprolactam, 6 parts of modified titanium dioxide, 1.5 parts of antioxidant, and 1 part of heat stabilizer are added to a spiral extrusion rod and mixed. The mixture is then melt-spun, wound, and shaped to form nylon fibers. The fibers are then woven to obtain an anti-UV interlayer. The fiber specifications are 40D / 84F. Step 4: Preparation of sunshade composite fabric for vehicle sunroof: hot melt adhesive is coated on both sides of nylon sunshade fabric, a PET aluminized film is stacked on top, and a non-woven fabric is stacked on the bottom. The fabric is then hot-pressed at a pressure of 4MPa and a temperature of 170℃ for 2 minutes and dried to obtain sunshade composite fabric for vehicle sunroof.
[0031] Comparative Example 3: Based on Example 1, the molecular weight of hydroxyl-terminated dimethylsiloxane was increased to 5000, while the rest of the process remained unchanged, as follows: Step 1: Preparation of modified polycaprolactam: (1) Under a nitrogen atmosphere, 4.4 parts of 4,4'-dihydroxybiphenyl, 1.4 parts of di(4-hydroxyphenyl)acetic acid, and 3.2 parts of triethylamine were added to 30 parts of anhydrous tetrahydrofuran and stirred evenly. 5.65 parts of phenylphosphodichlorochloride were slowly added dropwise in an ice-water bath and stirred for 2 hours. The mixture was heated to 70°C and stirred for 5 hours. 5 parts of hydroxyl-terminated dimethylsiloxane (molecular weight 5000) were added and stirred for 12 hours. The mixture was filtered, the solvent was removed by rotary evaporation, washed, purified, and dried to obtain the UV inhibitor. (2) Add the UV stabilizer to 30 parts of anhydrous tetrahydrofuran and stir until uniform. Add 1,6-hexanediisocyanate with a mass ratio of 10:0.5 to the UV stabilizer. Stir at 65°C for 1 hour and evaporate the solvent to obtain the modifier. (3) Heat 100 parts of caprolactam to 125°C, remove water, divide into two parts, add 5 parts of modifier to one part and 1.5 parts of sodium hydroxide to the other part, stir each part for 15 minutes, mix the two parts evenly, stir at 160°C for 35 minutes, transfer to a screw extruder for extrusion granulation to obtain modified polycaprolactam.
[0032] Step 2: Preparation of modified titanium dioxide: (1) Add 1.5 parts of nano titanium dioxide to 35 parts of deionized water and ultrasonically disperse evenly. Add 55 parts of anhydrous ethanol and 0.5 parts of 3-aminopropyltriethoxysilane, filter, wash, and dry to obtain aminated titanium dioxide. (2) 1.5 parts of aminated titanium dioxide were added to 45 parts of toluene and ultrasonically dispersed evenly. Under a nitrogen atmosphere, 11 parts of 1,6-hexamethylene diisocyanate were added and stirred at 75°C for 1 h. 26 parts of hydroxyl-terminated dimethylsiloxane were added and stirred at 80°C for 40 min. 2.5 parts of 1,4-butanediol, 3.5 parts of 4,4'-dihydroxybenzophenone and 0.01 parts of dibutyltin dilaurate were added and stirred at 85°C for 1.5 h. The mixture was filtered, washed and dried to obtain modified titanium dioxide. Step 3: Preparation of UV-blocking fabric: 45 parts of polyhexamethylene adipamide, 45 parts of modified polycaprolactam, 6 parts of modified titanium dioxide, 1.5 parts of antioxidant, and 1 part of heat stabilizer are added to a spiral extrusion rod and mixed. The mixture is then melt-spun, wound, and shaped to form nylon fibers. The fibers are then woven to obtain an anti-UV interlayer. The fiber specifications are 40D / 84F. Step 4: Preparation of sunshade composite fabric for vehicle sunroof: hot melt adhesive is coated on both sides of nylon sunshade fabric, a PET aluminized film is stacked on top, and a non-woven fabric is stacked on the bottom. The fabric is then hot-pressed at a pressure of 4MPa and a temperature of 170℃ for 2 minutes and dried to obtain sunshade composite fabric for vehicle sunroof.
[0033] Comparative Example 4: Based on Example 1, nano-titanium dioxide was only amination performed, while the remaining processes remained unchanged, as follows: Step 1: Preparation of modified polycaprolactam: (1) Under a nitrogen atmosphere, 4.4 parts of 4,4'-dihydroxybiphenyl, 1.4 parts of di(4-hydroxyphenyl)acetic acid and 3.2 parts of triethylamine were added to 30 parts of anhydrous tetrahydrofuran and stirred evenly. 5.65 parts of phenylphosphodichlorochloride were slowly added dropwise in an ice-water bath and stirred for 2 hours. The mixture was heated to 70°C and stirred for 5 hours. 5 parts of hydroxyl-terminated dimethylsiloxane were added and stirred for 12 hours. The mixture was filtered, the solvent was removed by rotary evaporation, washed, purified, and dried to obtain the UV inhibitor. (2) Add the UV stabilizer to 30 parts of anhydrous tetrahydrofuran and stir until uniform. Add 1,6-hexanediisocyanate with a mass ratio of 10:0.5 to the UV stabilizer. Stir at 65°C for 1 hour and evaporate the solvent to obtain the modifier. (3) Heat 100 parts of caprolactam to 125°C, remove water, divide into two parts, add 5 parts of modifier to one part and 1.5 parts of sodium hydroxide to the other part, stir each part for 15 minutes, mix the two parts evenly, stir at 160°C for 35 minutes, transfer to a screw extruder for extrusion granulation to obtain modified polycaprolactam.
[0034] Step 2: Preparation of modified titanium dioxide: (1) Add 1.5 parts of nano titanium dioxide to 35 parts of deionized water and ultrasonically disperse evenly. Add 55 parts of anhydrous ethanol and 0.5 parts of 3-aminopropyltriethoxysilane, filter, wash, and dry to obtain modified titanium dioxide. Step 3: Preparation of UV-blocking fabric: 45 parts of polyhexamethylene adipamide, 45 parts of modified polycaprolactam, 6 parts of modified titanium dioxide, 1.5 parts of antioxidant, and 1 part of heat stabilizer are added to a spiral extrusion rod and mixed. The mixture is then melt-spun, wound, and shaped to form nylon fibers. The fibers are then woven to obtain an anti-UV interlayer. The fiber specifications are 40D / 84F. Step 4: Preparation of sunshade composite fabric for vehicle sunroof: hot melt adhesive is coated on both sides of nylon sunshade fabric, a PET aluminized film is stacked on top, and a non-woven fabric is stacked on the bottom. The fabric is then hot-pressed at a pressure of 4MPa and a temperature of 170℃ for 2 minutes and dried to obtain sunshade composite fabric for vehicle sunroof.
[0035] Performance Test 1: The UV-resistant intermediate layer was prepared according to the scheme of Example 1, and the sample was tested as follows: (1) The fracture strength of the sample was tested according to GB / T 3923.1-2013. After the test, the sample was subjected to UV irradiation test according to ASTM G154. Under UVA-340 lamp, the irradiation intensity was 0.69W / m 2 Irradiation was carried out for 30 days, the fracture strength was measured, and the fracture strength reduction rate was calculated; (2) The notched impact strength of the sample was tested according to T1043-2008; (3) The limiting oxygen index (LOI) of the sample was tested according to ISO 4589-2 standard; (4) The thermogravimetric analyzer was used to test the sample, and the temperature at which 10% mass was lost was recorded. The heating rate was 20℃ / min, and the maximum temperature was 600℃; (5) The transmittance of the sample in ultraviolet wavelengths of 280~320nm was measured according to GB / T18830-2009; The experimental data are shown in Table 1: Table 1 project Example 1 Fracture strength 3632 Fracture strength reduction rate / % 0.27 <![CDATA[Impact strength / kJ·m -2 > 27.7 Loss of 10wt% temperature / ℃ 339 LOI 27.8 UV transmittance / % 0.82 As shown in Table 1, the UV-resistant interlayer prepared by this invention has excellent UV resistance and impact resistance, and also has certain flame retardancy and thermal stability.
[0036] Performance Test 2: Prepare UV-resistant intermediate layers according to the schemes of each embodiment and comparative example, and take samples for the following tests; (1) Test the fracture strength of the sample according to GB / T 3923.1-2013. After the test, conduct a UV irradiation test on the sample according to ASTM G154. Under a UVA-340 lamp, with an irradiation intensity of 0.69W / m 2 Irradiation was carried out for 30 days, the fracture strength was measured, and the fracture strength reduction rate was calculated; (2) The notched impact strength of the sample was tested according to T1043-2008; the experimental data are shown in Table 2: Table 2 project Fracture strength reduction rate / % Impact strength / kJ·m-2 Example 1 0.27 27.7 Example 2 0.42 26.7 Example 3 0.51 26.2 Comparative Example 1 1.94 21.2 Comparative Example 2 0.76 25.4 Comparative Example 3 1.32 23.4 Comparative Example 4 0.92 24.6 Table 2 shows that: in Comparative Example 1, replacing polycaprolactam with commercially available polycaprolactam increased the rate of decrease in tensile strength and decreased the impact strength, indicating that the modified polycaprolactam prepared in this invention can significantly improve UV resistance and impact resistance; in Comparative Example 2, without the addition of di(4-hydroxyphenyl)acetic acid, its UV resistance and impact resistance decreased slightly, indicating that the addition of di(4-hydroxyphenyl)acetic acid promoted the ring-opening polymerization of polycaprolactam to a certain extent, thus enhancing its performance; in Comparative Example 3, increasing the molecular weight of hydroxyl-terminated dimethylsiloxane restricted the movement of molecular chains, thus reducing the impact resistance of the material; in Comparative Example 4, nano-titanium dioxide was only aminated, resulting in decreased dispersibility in the material, thus reducing UV resistance and impact resistance.
[0037] Finally, it should be noted that the above descriptions are merely preferred embodiments of the present invention and are not intended to limit the present invention. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art can still modify the technical solutions described in the foregoing embodiments or make equivalent substitutions for some of the technical features. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A sunshade composite fabric for vehicle sunroofs, characterized in that: The composite fabric has a three-layer structure, consisting of a surface layer, an anti-UV intermediate layer, and a base fabric layer bonded together in sequence. The UV-resistant interlayer is made of nylon fiber, and the raw materials of the nylon fiber include the following components: by mass parts, 40-50 parts of polyhexamethylene adipamide, 40-50 parts of modified polycaprolactam, 5-8 parts of modified titanium dioxide, 1-2 parts of antioxidant, and 1-1.5 parts of heat stabilizer. The preparation method of the modified polycaprolactam includes the following steps: (1) Under a nitrogen atmosphere, 4,4'-dihydroxybiphenyl, di(4-hydroxyphenyl)acetic acid, and triethylamine are added to anhydrous tetrahydrofuran and stirred evenly. Phenylphosphoryl dichloride is slowly added dropwise in an ice-water bath and stirred for 2-2.5 h. The mixture is heated to 70-75°C and stirred for 5-6 h. Hydroxyl-terminated dimethylsiloxane is added and stirred for 10-12 h. The mixture is filtered, the solvent is removed by rotary evaporation, washed, purified, and dried to obtain the UV stabilizer; (2) Add the UV stabilizer to anhydrous tetrahydrofuran and stir until uniform. Add 1,6-hexamethylene diisocyanate and stir at 60-70°C for 1-1.5 h. Evaporate the solvent to obtain the modifier. (3) Heat caprolactam to 120-130°C. After removing water, divide it into two parts. Add the modifier to one part and sodium hydroxide to the other part. Stir each part for 10-15 min. Mix the two parts evenly and stir at 155-165°C for 30-40 min. Transfer to a screw extruder for extrusion granulation to obtain modified polycaprolactam. In the preparation of modified polycaprolactam, the molecular weight of hydroxyl-terminated dimethylsiloxane is 3000~4000. The preparation method of the modified titanium dioxide includes the following steps: (1) Add nano titanium dioxide to deionized water and ultrasonically disperse it evenly, add anhydrous ethanol and 3-aminopropyltriethoxysilane, filter, wash, and dry to obtain aminated titanium dioxide; (2) Add aminated titanium dioxide to toluene and ultrasonically disperse it evenly, add 1,6-hexamethylene diisocyanate under a nitrogen atmosphere, stir at 70~80℃ for 1~1.5h, add hydroxyl-terminated dimethylsiloxane, stir at 75~85℃ for 30~50min, add 1,4-butanediol, 4,4'-dihydroxybenzophenone and dibutyltin dilaurate, stir at 80~90℃ for 1~2h, filter, wash, and dry to obtain modified titanium dioxide.
2. The sunshade composite fabric for vehicle sunroofs according to claim 1, characterized in that: The method for preparing the UV-resistant interlayer includes the following steps: adding polyhexamethylene adipamide, modified polycaprolactam, antioxidant, modified titanium dioxide, and heat stabilizer into a spiral extrusion rod and mixing them, then melt spinning and winding to form nylon fibers; and weaving to obtain the UV-resistant interlayer.
3. The sunshade composite fabric for vehicle sunroofs according to claim 1, characterized in that: The UV stabilizer comprises the following raw materials, in parts by weight: 4.3-4.5 parts 4,4'-dihydroxybiphenyl, 1.3-1.5 parts di(4-hydroxyphenyl)acetic acid, 3.1-3.3 parts triethylamine, 5.6-5.7 parts phenylphosphodichloro, and 4.8-5.2 parts hydroxyl-terminated dimethylsiloxane; The mass ratio of the UV stabilizer to 1,6-hexamethylene diisocyanate is 10:0.45~0.55; The modified polycaprolactam comprises the following raw materials, by weight: 100 parts caprolactam, 4-6 parts modifier, and 1.5-2 parts sodium hydroxide.
4. The sunshade composite fabric for vehicle sunroofs according to claim 1, characterized in that: in, The aminated titanium dioxide comprises the following raw materials, by mass: 1-2 parts nano titanium dioxide, 30-40 parts deionized water, 50-60 parts anhydrous ethanol, and 0.4-0.6 parts 3-aminopropyltriethoxysilane; The modified titanium dioxide comprises the following raw materials, by weight: 1-2 parts aminated titanium dioxide, 40-50 parts toluene, 10-12 parts 1,6-hexamethylene diisocyanate, 25-28 parts hydroxyl-terminated dimethylsiloxane, 2-3 parts 1,4-butanediol, 3-4 parts 4,4'-dihydroxybenzophenone, and 0.01-0.02 parts dibutyltin dilaurate.
5. The sunshade composite fabric for vehicle sunroofs according to claim 2, characterized in that: During the weaving process, the fiber specifications are 35~50D / 72~96F.
6. A method for preparing a sunshade composite fabric for a vehicle sunroof according to any one of claims 1 to 5, characterized in that, Includes the following steps: Hot melt adhesive is coated on both sides of the UV-resistant intermediate layer, a surface layer is stacked on top of it, and a base fabric layer is stacked on the bottom. The layers are then hot-pressed, cured, and dried to obtain a sunshade composite fabric for vehicle sunroofs.
7. The method for preparing a sunshade composite fabric for a vehicle sunroof according to claim 6, characterized in that: The surface layer is a PET aluminum-coated film with a thickness of 10~20μm, wherein the aluminum layer thickness is 300~700Å; the base fabric layer is a non-woven fabric with a thickness of 0.05~0.2mm. During the hot-press curing process, the temperature is 160~180℃, the pressure is 3~5MPa, and the time is 1~3min.
Citation Information
Patent Citations
Modification method of fatty polyamide ultraviolet-resistant nano titanium dioxide
CN111471326A
Anti-ultraviolet / salt-spray-resistant polyamide composite material and preparation method thereof
CN119823571A