A method for manufacturing a combustion chamber head fairing

By optimizing the machining process of the combustion chamber head fairing, and combining mold design with precise machining methods, the problems of surface contour accuracy and precision hole position accuracy were solved, achieving high-quality and efficient machining results.

CN120619773BActive Publication Date: 2026-11-10CHINA HANGFA GUIZHOU LIYANG AVIATION POWER CO LTD
View PDF 2 Cites -1 Cited by

Patent Information

Application Number
CN202510931078.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-07-07
Publication Date
2026-11-10
Estimated Expiration
2045-07-07

Smart Images

  • Figure CN120619773B_ABST
    Figure CN120619773B_ABST
Patent Text Reader

Abstract

This invention discloses a method for manufacturing a combustion chamber head fairing, comprising the following steps: preparing a blank, deep drawing, heat treatment, deep drawing and reshaping to meet the final contour requirements of the combustion chamber head fairing, punching all elliptical and circular holes on the deep-drawn part in one pass and removing the inner and outer flange edges, machining the inner and outer circles of the deep-drawn part to ensure that the height and diameter of the machined part are consistent with the final dimensions of the combustion chamber head fairing, and cutting anti-crack grooves on the large end faces of the inner and outer circles of the machined part on a laser cutting machine. This method improves the manufacturing quality and yield of the combustion chamber head fairing, while also increasing manufacturing efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of aero-engine processing technology, specifically relating to a processing method for the head cowl of an aero-engine combustion chamber. Background Technology

[0002] like Figure 1 The cowling with arrayed holes shown is a hot-end component of an aero-engine, installed at the head of the combustion chamber to rectify the flow of fluid entering the combustion chamber, ensuring stable combustion. The part is machined from a high-temperature alloy and is a ring-shaped, thin-walled sheet metal part with an open C-shaped cross-section. It requires the machining of 16 high-precision elliptical holes and 16 circular holes, with 16 anti-crack grooves machined on both the inner and outer large end faces. The overall surface profile requirement for the part is 0.5.

[0003] During the initial trial production, the parts were processed using a process route of deep drawing → heat treatment → shaping → turning inner and outer diameters → laser cutting holes and crack-resistant grooves. However, since the fairing is a thin-walled sheet metal part, it has springback in its free state, making it difficult to align during laser processing. Furthermore, the holes need to be processed sequentially, and the part's state changes continuously during hole processing, causing deformation of the part after hole cutting. The surface profile is difficult to guarantee, and the inner and outer diameters and the positional accuracy of precision holes simultaneously exceed the tolerance. Therefore, it is necessary to study a reasonable and feasible processing method to produce similar parts. Summary of the Invention

[0004] The present invention aims to provide a processing method for a combustion chamber head fairing, which improves the processing quality and pass rate of parts on the one hand, and improves processing efficiency on the other.

[0005] To achieve the above objectives, the present invention adopts the following technical solution:

[0006] A method for manufacturing a combustion chamber head fairing includes the following steps:

[0007] Step 1: Prepare the blank by machining a flat, circular blank from sheet metal;

[0008] Step 2: Deep drawing. Place the annular blank in the deep drawing die for deep drawing to obtain a deep-drawn part with inner and outer circular flanges. Leave a deep drawing allowance during deep drawing.

[0009] Step 3: Heat treatment. The deep-drawn parts from Step 2 are subjected to heat treatment to eliminate the stress from the deep-drawing process.

[0010] Step 4: Shaping. Place the heat-treated drawn part from Step 3 into the drawing die from Step 2. Use the drawing allowance reserved in Step 2 to achieve shaping by drawing again and meet the final contour requirements of the combustion chamber head fairing.

[0011] Step 5: Punching and trimming. Place the drawn part after the shape correction in step 4 into the die on the punch press. Position and clamp the part with the profile of the drawn part. Punch all the elliptical holes and round holes on the combustion chamber head fairing in one go. Simultaneously cut off the inner and outer round flange edges.

[0012] Step 6: Machining. Machining the inner and outer circles of the deep-drawn part in step 5 to ensure that the height and diameter of the part after machining are consistent with the final height and diameter of the combustion chamber head fairing.

[0013] Step 7: Cut the anti-crack groove. Align the part machined in Step 6 on the laser cutting machine and cut the anti-crack groove on the inner and outer large end faces of the part machined in Step 6.

[0014] Alternatively, in step 2, the drawing die includes a pressing structure for pressing the inner end face and the outer end face of the annular blank.

[0015] As an option:

[0016] In step 2, a drawing allowance is reserved by placing a shim in the drawing die (see specific implementation, the shim is placed between the lower drawing die and the drawing support plate);

[0017] In step 4, the pad placed in step 2 is removed and stretched for shaping.

[0018] Alternatively, in steps 2 and 4, the same hydraulic press of the same specification is used to drive the same set of drawing dies.

[0019] Alternatively, the die in step 5 includes an upper die plate, a lower die plate, a punch, a punch head, an ejector cylinder, a die cavity, and a punch-die cavity, wherein:

[0020] The punch, ejector cylinder, die, and punch-die are all annular components. The punch and die are simultaneously assembled on the upper template, with the punch located in the inner annular surface of the die. The ejector cylinder is slidably assembled between the outer annular surface of the punch and the inner annular surface of the die. The lower end face of the ejector cylinder is a concave surface that matches the convex surface of the drawn part. The punch and die are mounted on the lower template, with the upper end face of the punch and die matching the concave surface of the drawn part. The inner and outer contour edges of the convex surface are machined with cutting edges. The end face of the punch that contacts the drawn part is a conforming concave arc surface, which matches the convex surface of the drawn part after shaping in step 4. The ejector cylinder, punch and die, and lower template all have through holes located on the path of the punch's movement.

[0021] Furthermore, the die also includes a cutter and a rubber ring. The cutter is mounted on the lower die plate and is located between the punch and the lower die plate and between the die and the lower die plate. The rubber ring is placed between the ejector cylinder and the upper die plate, and the rubber ring has a through hole for the punch.

[0022] Furthermore, in step 5, the above-mentioned die is used to punch and trim the drawn part after shaping in step 4, and includes the following steps:

[0023] Step 51: The upper template moves the punch, die, and ejector cylinder downwards until the ejector cylinder and the punch and die close together. The deep-drawn part is limited by the concave surface of the lower end face of the ejector cylinder and the convex surface of the deep-drawn part, and the convex surface of the upper end face of the punch and die and the concave surface of the deep-drawn part.

[0024] Step 52: Simultaneously move all punches to punch all elliptical holes and all round holes on the combustion chamber head fairing in one go. While punching the elliptical holes and round holes, the inner and outer flange edges of the deep-drawn parts are removed by the cutting edge on the die.

[0025] Alternatively, in step 6, the end of the deep-drawn part corresponding to the open C-shaped section is placed upwards and then machined in a machining fixture. The machining fixture is used to support the convex surface of the end of the deep-drawn part corresponding to the closed C-shaped section, and a pressure block is placed into the end of the deep-drawn part corresponding to the open C-shaped section to limit the inner surface for radial positioning. The circumferential positioning is achieved by locking through the round hole on the deep-drawn part.

[0026] Alternatively, in step 7, a five-axis laser cutting machine is used to fix the machined part and align its center before cutting the anti-crack groove.

[0027] Compared with existing technologies, this invention proposes a processing method for a combustion chamber head fairing. Through a reasonable process route and processing method, the dimensional accuracy of the combustion chamber head fairing profile and the dimensions of precision holes are guaranteed, improving the processing quality of the combustion chamber head fairing and significantly increasing processing efficiency. Currently, the processing method of this invention is being used in the field and has achieved the objectives and technical requirements of this invention. Attached Figure Description

[0028] Figure 1 This is a schematic diagram of the combustion chamber head fairing structure;

[0029] Figure 2 This is a schematic diagram of a circular ring-shaped blank;

[0030] Figure 3 These are schematic diagrams of the deep drawing process of the combustion chamber head fairing and cross-sectional diagrams of the deep drawing die.

[0031] Figure 4 This is a schematic diagram of the stamping die structure;

[0032] Figure 5 This is a schematic diagram of a punch structure used for elliptical holes;

[0033] In the figure, 1-punch, 2-punch head, 3-ejector cylinder, 4-die, 5-punch and die, 6-cutter, 7-rubber ring. Detailed Implementation

[0034] The present invention will be further described below with reference to specific embodiments, but it should not be construed as limiting the scope of the subject matter of the present invention to the following embodiments. All modifications, substitutions and alterations made based on ordinary technical knowledge and common practices in the art without departing from the above-described technical concept of the present invention are included within the scope of the present invention.

[0035] For processing Figure 1 The combustion chamber head fairing shown in the invention provides a manufacturing method for the combustion chamber head fairing, comprising the following steps:

[0036] Step 1: Prepare the blank. The blank is a flat, ring-shaped material, and it is made from sheet metal to facilitate subsequent deep drawing. The ring-shaped blank is as follows: Figure 2 As shown;

[0037] Step 2: Deep drawing. Place the ring-shaped blank in the deep drawing die for deep drawing. During deep drawing, place a 3mm thick shim between the lower drawing die and the drawing punch. The structure after deep drawing is as follows. Figure 3 As shown, the inner flange edge on the inner circle side and the outer flange edge on the outer circle side of the deep-drawn part. Figure 3 In deep drawing, the main components of the drawing die are a drawing die, a drawing support plate, a drawing punch, a shim, and a lower drawing die (all of these components are annular structures). The lower end face of the drawing die includes both a concave surface and an annular plane for forming the blank holder structure. The upper end face of the drawing support plate, as part of the blank holder structure, cooperates with the lower end face of the drawing die to form a blank holder structure that clamps one end face of the inner circle of the annular blank (two end faces in the blank thickness direction) and one end face of the outer circle (two end faces in the blank thickness direction). The shim is placed between the lower drawing die and the drawing support plate. The thickness of the shim controls the amount of deformation during the first deep drawing, ensuring it is less than the final height of the combustion chamber head fairing. Then, the shim is removed for reshaping to achieve the final height of the combustion chamber head fairing. At the start of deep drawing, both the deep drawing die and the deep drawing support plate are located above the deep drawing punch. The annular blank (sheet metal) is placed between the deep drawing die and the deep drawing support plate. The deep drawing die is driven to press down and clamp the blank together with the deep drawing support plate. It continues to move downward until it contacts the deep drawing punch, completing the first deep drawing. The shim is located below the deep drawing support plate to control the downward stroke and prevent it from being drawn to the final size during the first deep drawing. After heat treatment, the shim is removed, and the part is put back into the same deep drawing die. This time, it is drawn to the bottom to obtain the final size.

[0038] Step 3: Heat treatment. The deep-drawn parts are heat-treated to eliminate the stress from the deep-drawing process.

[0039] Step 4: Shaping. Place the heat-treated part back into the drawing die from Step 2, remove the shims, and draw and shape it again to obtain the final dimensions. The advantage of drawing in two stages is that it removes most of the internal stress during forming, leaving only the stress from the final drawing deformation, thus maintaining the stability of the part's dimensions.

[0040] Step 5: Punching and trimming. Place the drawn and shaped part into the die (punching and trimming die) on the punch press, using the part's profile for positioning and clamping. 16 oval holes and 16 round holes are punched in one go. Simultaneously, the inner and outer flange edges of the drawn and shaped part are removed (the positions of the inner and outer flange edges are shown in the image). Figure 3 As shown, during deep drawing, flange edges are generated on the inner and outer circles of the part. Only the C-shaped section protruding in the middle area is an effective profile, while the rest are redundant parts.

[0041] Step 6: Machining. Machin the inner and outer diameters of the deep-drawn part after punching and trimming, ensuring the height H, h and outer diameter are met. and inner diameter

[0042] Step 7: Cut the anti-crack groove. Align the machined part on the laser cutting machine and machine the anti-crack grooves on the inner and outer large end faces to ensure the relevant dimensions of groove H1 and groove H2.

[0043] in:

[0044] In step 1, the annular blank is machined from sheet metal, and the dimensions of the annular ring must meet the subsequent forming requirements, that is, the inner and outer diameters of the annular ring must be appropriate. For example... Figure 2 The outer diameter of the annular blank is Inner diameter is After blanking, remove burrs from the inner and outer surfaces of the parts;

[0045] In step 1, if the outer diameter of the annular blank is too small and the inner diameter is too large, there will be insufficient material for subsequent deep drawing. If the outer diameter is too large and the inner diameter is too small, the part will become unstable and wrinkle during deep drawing.

[0046] In step 2, the deep drawing process uses a 4000KN hydraulic press. The deep drawing die is required to have a blank holder structure, which consists of... Figure 3 The plane in the lower end face of the deep drawing die and the plane in the upper end face of the deep drawing support plate are combined to form the inner and outer circular edges of the blank together with the deep drawing die, forming the main body surface of the deep drawing part. The blank holder force is not less than 200T.

[0047] In step 2, a 3mm thick shim is placed during deep drawing to leave sufficient machining allowance for the subsequent shaping process after heat treatment;

[0048] In step 3, the heat treatment equipment used is a heat treatment furnace, which reduces the work hardening of the material caused during the deep drawing process and softens the material.

[0049] In step 4, the equipment used for calibration is a 4000KN hydraulic press, and the calibration mold used is the drawing mold used in step 2. During calibration, the shims are removed, and the calibration part is further drawn to ensure the stability of the part dimensions. At this time, the profile profile is no more than 0.5.

[0050] In step 5, the punching and trimming process uses a 5000KN punch press. To address the deformation issue caused by the initial laser cutting, a [specific feature / mechanism] was designed. Figure 4 The die set includes an upper die plate, a lower die plate, a punch 1, 32 punches 2, an ejector cylinder 3, a die 4, a punch and die 5, a cutter 6, and a rubber ring 7. The punch 1 is a ring-shaped component with a ring-shaped protrusion at the lower end of its outer ring surface. There are two types of punches 2: one for punching elliptical holes and the other for punching round holes. Round holes are punched in a relatively flat area, while elliptical holes are located on curved surfaces, making machining more difficult. The lower end of the punch 2 for elliptical holes is innovatively designed to conform to the curved surface of the drawn part, with the punch being made into a conformal concave arc surface. The structure of punch 2 is as follows: Figure 5 As shown, this ensures that punch 2 contacts the part surface simultaneously during punching, preventing tearing of the part body and causing defects. The die 4 is an annular part with an annular protrusion at the lower end of its inner ring surface. The annular protrusion of the die 4 and the annular protrusion of the punch 1 form a sliding assembly space for the ejector cylinder 3. The ejector cylinder 3 is also an annular part with a T-shaped cross-section, which limits its position between the two annular protrusions. A rubber ring 7 is also installed between the ejector cylinder 3 and the upper template. Below the ejector cylinder 3 is the punch and die 5, which is also an annular part. The upper end face of the punch and die 5 is an outwardly convex forming surface, which cooperates with the inwardly concave forming surface at the lower end of the ejector cylinder 3 to position the inner and outer surfaces of the deep-drawn part. Both the inner and outer contour edges of the outwardly convex forming surface of the punch and die 5 have cutting edges for cutting away... Figure 3 The inner and outer circular flange edges of the deep-drawn parts. The punch and die 5, the ejector cylinder 3, the lower template, and the rubber ring 7 all have through holes for mating with the punch 2;

[0051] During punching, Figure 3The deep-drawn part is placed between the ejector cylinder 3 and the punch and die 5. During punching, the upper template drives the punch 1, die 4, and ejector cylinder 3 to move downward together. The ejector cylinder 3 and the punch and die 5 come into contact first to position the deep-drawn part with the profile. Then, the two punches 2 cooperate with the punch and die 5 to punch out the round hole and elliptical hole on the top surface. The punch and die 5 cooperate with the punch 1 and die 4 to punch the inner and outer flange edges. There are 3 cutters 6 inside and 3 outside, which contact the punch 1 and die 4 respectively to cut the inner and outer flange edges into three sections, making it convenient for workers to remove the material edges.

[0052] During the punching process, after the ejector cylinder 3 and the die 5 are closed, the surface of the drawn part is limited. Then, 32 punches 2 punch simultaneously to ensure that the elliptical and round holes are of qualified size and consistent position. The inner and outer circular contours of the die 5 are made into punching cutting edge structures, which cooperate with the punch 1 and the die 4 to cut off the inner and outer circular flanges of the drawn part, reducing the amount of machining work of the inner and outer circles when machining the drawn part in the subsequent machining. In addition, the surface of the drawn part can be further corrected by the concave surface of the ejector cylinder 3 and the convex surface of the die 5 during punching. After punching, the relevant dimensions and positional accuracy a of the elliptical and round holes are guaranteed.

[0053] In step 5, after punching, the processing cost of precision elliptical and round holes on the deep-drawn parts is greatly reduced. At the same time, it avoids the defects caused by thermal processing methods such as heat-affected zone, microcracks, and remelted layer that exist in laser processing, and further improves the quality of the parts.

[0054] In step 6, during machining, the deep-drawn part is inverted to ensure that the opening of the C-shaped section is facing upwards, and then placed in the machining fixture. The machining process ensures the inner and outer diameters and the height of the part.

[0055] In step 6, the machining fixture is a conformal fixture (C-shaped cross-section of the deep-drawn part). When clamping, the part is inverted (the opening of the C-shaped cross-section is facing upwards). First, the machining fixture is used to lift the outer surface of the deep-drawn part (i.e., positioning it with the convex surface). Then, the inner surface pressure block is placed to restrict the inner surface of the part (the concave surface) to prevent radial movement. Furthermore, 16 round holes are used to lock the part to prevent circumferential movement.

[0056] In step 7, a five-axis laser cutting machine is used to cut the anti-crack groove. During the cutting process, the machined part is first fixed, and then the center of the deep-drawn part is aligned using the machined round hole. The anti-crack groove is then machined according to the drawing requirements.

[0057] Contents not described in detail in this specification are prior art known to those skilled in the art. Although illustrative specific embodiments of the invention have been described above to facilitate understanding by those skilled in the art, it should be understood that the invention is not limited to the scope of the specific embodiments. Various modifications are readily apparent to those skilled in the art as long as they fall within the spirit and scope of the invention as defined and determined by the appended claims, and all inventions utilizing the concept of this invention are protected.

Claims

1. A method for processing a combustion chamber head fairing, characterized in that, Includes the following steps: Step 1: Prepare the blank by machining a flat, ring-shaped blank from sheet metal; Step 2: Deep drawing. Place the annular blank in the deep drawing die for deep drawing to obtain a deep-drawn part with inner and outer circular flanges. Leave a deep drawing allowance during deep drawing. The deep drawing die consists of a deep drawing die, a deep drawing support plate, a deep drawing punch, a shim, and a deep drawing lower die plate. The lower end face of the deep drawing die includes both a concave surface and an annular plane for forming a blank holder structure. The upper end face of the deep drawing support plate, as part of the blank holder structure, cooperates with the lower end face of the deep drawing die to form a blank holder structure that presses the inner circle end face and the outer circle end face of the annular blank. A drawing allowance is reserved by placing a shim in the drawing die. The shim is placed between the lower drawing die and the drawing support plate. The drawing deformation is controlled by the thickness of the shim, so that it is less than the final height of the combustion chamber head fairing. Step 3: Heat treatment. The deep-drawn parts from Step 2 are subjected to heat treatment to eliminate the stress from the deep-drawing process. Step 4: Shaping. Place the heat-treated drawn part from Step 3 into the drawing die from Step 2, remove the shim placed in Step 2, and use the drawing allowance reserved in Step 2 to achieve shaping by drawing again, and meet the final contour requirements of the combustion chamber head fairing. Step 5: Punching and trimming. Place the drawn part after the shape correction in step 4 into the die on the punch press. Position and clamp the part with the profile of the drawn part. Punch all the elliptical holes and round holes on the combustion chamber head fairing in one go. Simultaneously cut off the inner and outer round flange edges. Step 6: Machining. Machining the inner and outer circles of the deep-drawn part in step 5 to ensure that the height and diameter of the part after machining are consistent with the final height and diameter of the combustion chamber head fairing. Step 7: Cut the anti-crack groove. Align the part machined in Step 6 on the laser cutting machine and cut the anti-crack groove on the inner and outer large end faces of the part machined in Step 6.

2. The processing method of a combustion chamber head fairing according to claim 1, characterized in that: In steps 2 and 4, the same hydraulic press of the same specification is used to drive the same set of drawing dies.

3. The processing method of a combustion chamber head fairing according to claim 1, characterized in that, The die in step 5 includes an upper die plate, a lower die plate, a punch (1), a punch (2), an ejector cylinder (3), a die (4), and a punch and die (5), wherein: The punch (1), ejector cylinder (3), die (4) and die (5) are all ring parts. The punch (1) and die (4) are simultaneously assembled on the upper template, and the punch (1) is located in the inner ring surface of the die (4). The ejector cylinder (3) is slidably assembled between the outer ring surface of the punch (1) and the inner ring surface of the die (4). The lower end face of the ejector cylinder (3) is a concave surface that is consistent with the convex surface of the deep-drawn part. The die (5) is installed on the lower template, and the upper end face of the die (5) is a convex surface that is consistent with the concave surface of the deep-drawn part. The inner and outer contour edges of the convex surface are respectively machined with cutting edges. The end face of the punch (2) that contacts the deep-drawn part is a conforming concave arc surface. The conforming concave arc surface is consistent with the convex surface of the deep-drawn part after the shape is corrected in step 4. The ejector cylinder (3), die (5) and the lower template are all provided with through holes, which are located on the path of the punch (2).

4. The processing method of a combustion chamber head fairing according to claim 3, characterized in that: The die also includes a cutter (6) and a rubber ring (7). The cutter (6) is mounted on the lower template and is located between the punch (1) and the lower template and between the die (4) and the lower template. The rubber ring (7) is placed between the ejector cylinder (3) and the upper template and has a through hole for the punch (2).

5. The processing method of a combustion chamber head fairing according to claim 3, characterized in that, In step 5, a punching die is used to punch and trim the edges of the deep-drawn part after the shape correction in step 4, and the steps include: Step 51: The upper template drives the punch (1), die (4) and ejector cylinder (3) to move downward until the ejector cylinder (3) and the punch and die (5) are closed. The concave surface of the lower end face of the ejector cylinder (3) and the convex surface of the deep-drawn part, as well as the convex surface of the upper end face of the punch and die (5) and the concave surface of the deep-drawn part, together limit the deep-drawn part. Step 52: Simultaneously move all punches (2) to punch all elliptical holes and all round holes on the combustion chamber head fairing in one go. While punching the elliptical holes and round holes, the inner and outer flange edges of the deep-drawn parts are removed through the cutting edge on the die (5).

6. The method for processing a combustion chamber head fairing according to claim 1, characterized in that: In step 6, the end of the deep-drawn part corresponding to the open C-shaped section is placed upward and then into the machining fixture for machining. The machining fixture is used to support the convex surface of the end of the deep-drawn part corresponding to the closed C-shaped section. Then, a pressure block is placed into the end of the deep-drawn part corresponding to the open C-shaped section to limit the inner surface and achieve radial limiting. The circumferential limiting is achieved by locking through the round hole on the deep-drawn part.

7. The method for processing a combustion chamber head fairing according to claim 1, characterized in that: In step 7, a five-axis laser cutting machine is used to fix the machined parts and align the center before cutting the anti-crack groove.

Citation Information

Patent Citations

  • Machining device and machining method for gas turbine fairing wall

    CN108043969A

  • Drawing forming method for aircraft hat-shaped fairing sheet metal part

    CN112474984A