Insulating material for prefabricated cable accessory, preparation method of insulating material and prefabricated cable accessory

By optimizing the formula and process of EPDM rubber insulation materials and adding antioxidants and other components, the problems of existing materials being prone to aging and insufficient mechanical properties in complex environments have been solved, and high-performance insulation materials for prefabricated cable accessories have been achieved.

CN120648112AActive Publication Date: 2025-09-16HANGDA ELECTRIC CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202510916282.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-07-03
Publication Date
2025-09-16
Estimated Expiration
2045-07-03

AI Technical Summary

Technical Problem

Existing prefabricated cable accessories use insulation materials that are prone to aging in high temperature, humidity, and electric field environments, have insufficient mechanical properties, and unstable processing performance, making it difficult to meet the high requirements of modern power systems.

Method used

Using EPDM rubber as the basis, adding antioxidants, reinforcing fillers, plasticizers, cross-linking agents, co-cross-linking agents and processing aids with specific structures, and optimizing the mixing and vulcanization processes to form a synergistic insulating material.

Benefits of technology

The material's environmental aging resistance, mechanical properties and processing performance have been significantly improved, ensuring insulation performance and structural integrity in complex environments, and improving production efficiency and product quality stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120648112A_ABST
    Figure CN120648112A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of insulating materials, and discloses an insulating material for a prefabricated cable accessory, a preparation method of the insulating material and the prefabricated cable accessory. The insulating material for the prefabricated cable accessory consists of the following raw materials in parts by mass: 100 parts of ethylene propylene diene monomer, 40-70 parts of reinforcing filler, 20-40 parts of a plasticizer, 1.5-3.5 parts of a cross-linking agent, 1-3 parts of an assistant cross-linking agent, 1-3 parts of an anti-aging agent and 1-5 parts of a processing aid. By introducing the anti-aging agent with a specific structure, the anti-oxidation and anti-degradation capabilities of the material in complex environments such as high temperature, moisture and electric field are enhanced, the aging process of the insulating material is effectively delayed, and the original performance of the material can be better maintained in long-term use. Through collaborative optimization of formula components and process parameters, the dispersion uniformity of the materials in the mixing process is improved, the pre-crosslinking risk is reduced, and the vulcanization efficiency and the quality stability are improved, so that the production process is more controllable, and the product quality is more consistent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of insulating materials, and in particular to an insulating material for prefabricated cable accessories, a preparation method thereof, and the prefabricated cable accessories. Background Art

[0002] With the continuous development of power systems, the performance requirements for cable accessories are becoming increasingly stringent. As a crucial component of power equipment, the insulation performance of prefabricated cable accessories is directly related to the safety and reliability of power transmission. However, existing insulation materials for prefabricated cable accessories present numerous challenges in practical applications.

[0003] Currently, the insulation material of most prefabricated cable accessories is based on rubber. While this material possesses a certain degree of insulation, it is susceptible to accelerated aging due to environmental factors during long-term operation. For example, in high-temperature environments, the material's molecular chain movement intensifies, which can easily lead to molecular chain breakage or excessive cross-linking, causing the material to become brittle and crack, significantly reducing mechanical properties and subsequently deteriorating insulation performance. In humid environments, moisture easily penetrates the material, causing water tree aging, destroying the material's insulation structure, reducing insulation resistance, and increasing the risk of insulation breakdown. Furthermore, under the long-term influence of electric and magnetic fields, the insulation material can undergo electrical aging, causing changes in internal trap energy levels, increasing carrier mobility, and increasing electrical conductivity, ultimately leading to a loss of insulation performance.

[0004] At the same time, the comprehensive performance of existing insulation materials is also difficult to meet the high requirements of modern power systems. On the one hand, their mechanical properties need to be improved. For example, during installation and operation, cable accessories need to withstand certain mechanical stresses. If the insulation material is not strong enough, it is easy to deform or damage, affecting the sealing and integrity of the cable accessories. On the other hand, in terms of processing performance, existing materials are prone to problems such as uneven dispersion and incomplete vulcanization during processing steps such as mixing and vulcanization, resulting in unstable product quality and limited production efficiency. In addition, as the voltage level of the power system increases and the application scenarios become more complex, the requirements for special properties such as corona resistance and partial discharge resistance of insulation materials are also increasing. However, the performance of existing materials in these aspects is still not ideal.

[0005] Therefore, it is urgent to develop a prefabricated insulation material for cable accessories that can adapt to complex environments and has excellent insulation properties, good mechanical properties and processing properties. Summary of the Invention

[0006] The purpose of the present invention is to provide a prefabricated insulating material for cable accessories that is resistant to environmental aging, has excellent mechanical properties and good processing performance, in response to the problems existing in the prior art.

[0007] To achieve the above object, the technical solution adopted by the present invention is: a prefabricated insulating material for cable accessories, comprising the following raw materials in parts by weight: 100 parts of EPDM rubber, 40-70 parts of reinforcing filler, 20-40 parts of plasticizer, 1.5-3.5 parts of cross-linking agent, 1-3 parts of co-cross-linking agent, 1-3 parts of antioxidant, and 1-5 parts of processing aid; The antioxidant has a structure shown in Formula 1: Formula 1; The R1 is selected from the group consisting of: methyl, ethyl, tert-butyl, and methoxy.

[0008] Furthermore, the reinforcing filler is carbon black.

[0009] Furthermore, the plasticizer is paraffin oil.

[0010] Furthermore, the cross-linking agent is dicumyl peroxide.

[0011] Furthermore, the auxiliary cross-linking agent is triallyl isocyanurate.

[0012] Furthermore, the processing aid is stearic acid.

[0013] Furthermore, the antioxidant is any one of the compounds shown in the following structures: ; .

[0014] A method for preparing an insulating material for a prefabricated cable accessory comprises the following steps: S1. The EPDM rubber, reinforcing filler, and plasticizer were added to an internal mixer and mixed at 70-90 ° C for 5-8 minutes to obtain material A; S2. Add the antioxidant, processing aid, and cross-linking agent to the material A and mix on an open mill at 40 to 60 ° C for 10 minutes to obtain material B; S3. The material B is cooled to 30-40 ℃, the crosslinking agent is added, and the mixture is uniformly mixed and then thinly passed through the sheet to obtain a mixed rubber set; S4. The rubber mixture is placed in a mold, vulcanized at 170-180°C and 10-15 MPa pressure for 15-20 minutes, and cooled to obtain a prefabricated insulating material for cable accessories.

[0015] Furthermore, after the vulcanization in S4, the material is heat-treated in an oven at 150° C. for 2-4 hours.

[0016] Furthermore, the vulcanizing agent is sulfur.

[0017] Furthermore, the rotor speed of the internal mixer in S1 is 30-50 rpm, and the filling factor is 70%-80%.

[0018] Furthermore, the cooling in S4 is air cooling.

[0019] A prefabricated cable accessory comprises a stress cone, an insulating body and a sealing structure. The stress cone and / or the insulating body are made of the above-mentioned insulating material for the prefabricated cable accessory.

[0020] Furthermore, the insulation material has an elongation at break retention rate of ≥85% after aging in an air box at 135° C. for 168 hours.

[0021] Furthermore, the Shore A hardness of the stress cone is ≤68.

[0022] The invention discloses an application of a prefabricated cable accessory at the terminal and / or intermediate connection position of a 10-35kV cross-linked polyethylene cable.

[0023] The antioxidant's mechanism of action is primarily through its chemical structure, which traps free radicals and inhibits oxidation chain reactions, thereby slowing the material's aging process. The large heterocyclic conjugated structure within the molecule provides electronic stability and a resonance effect, effectively absorbing and quenching free radicals, preventing oxidative breakage of the rubber molecular chain and enhancing the material's heat resistance and antioxidant properties. The imino group (-NH-), as a nucleophilic group, readily captures free radicals or participates in hydrogen bond formation, inhibiting the chain propagation of the oxidation reaction. The cyano group (-CN) has strong polarity, enhancing intermolecular interactions, improving the antioxidant's dispersibility and stability, and reducing changes in the material's electrical conductivity under electric fields. Under high temperatures or electric field conditions, insulating materials (EPDM rubber) are prone to generating free radicals. The antioxidant's large heterocyclic conjugated structure and imino group can rapidly react with these free radicals, forming stable intermediates that interrupt the oxidation chain reaction. The cyano group's strong electronegativity helps decompose peroxides, preventing them from initiating material degradation. This is particularly important during high-temperature vulcanization, ensuring uniform cross-linking reactions. The large conjugated structure of the heterocyclic ring forms an electron delocalized system with the cyano group, which enhances the electron affinity of the molecule and reduces the degradation of the material caused by environmental factors (such as ultraviolet rays or humidity).

[0024] The material system based on ethylene propylene diene monomer (EPDM) described in the present invention improves the material's resistance to environmental aging, mechanical properties, and processing properties by adding components such as antioxidants, reinforcing fillers, plasticizers, crosslinking agents, co-crosslinking agents, and processing aids. The innovative structural design of the antioxidant enables it to protect the EPDM chain during high-temperature vulcanization, inhibit water tree aging, and improve the elongation at break after aging; carbon black, as a reinforcing filler, anchors the molecular chain through surface active sites to enhance the material's strength, and its dispersion is affected by paraffin oil lubrication, thereby optimizing the mixing filling coefficient; in the crosslinking system, dicumyl peroxide initiates crosslinking, the antioxidant quenches excess free radicals, the co-crosslinking agent and carbon black co-construct a three-dimensional network, and stearic acid, as a dispersion medium, prevents pre-crosslinking during low-temperature mixing. The synergistic effect between the components improves the overall performance of the material.

[0025] Compared with the prior art, the present invention has the following beneficial effects: 1. Significantly improved environmental aging resistance: By introducing antioxidants with specific structures, the material's antioxidant and degradation resistance in complex environments such as high temperature, humidity, and electric fields is enhanced, effectively delaying the aging process of the insulation material and enabling the material to better maintain its original performance during long-term use.

[0026] 2. Overall optimization of mechanical properties: The material formula and preparation process have been optimized, significantly improving the overall mechanical strength and hardness stability of the insulation material, making it more able to withstand mechanical stress during installation and operation, and maintain structural integrity and sealing.

[0027] 3. Improved processing performance: Through the coordinated optimization of formula components and process parameters, the dispersion uniformity of materials during the mixing process is improved, the risk of pre-crosslinking is reduced, and the vulcanization efficiency and quality stability are improved, thereby making the production process more controllable and the product quality more consistent. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 For the antioxidant 1 of the present invention 1 HNMR spectrum.

[0029] Figure 2 This is a finished product picture of the prefabricated cable accessories described in the present invention. DETAILED DESCRIPTION

[0030] The following will clearly and completely describe the technical solution of the present invention in conjunction with the accompanying drawings. Obviously, the embodiments described are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of the present invention.

[0031] Synthesis example one Synthesis of antioxidant 1: ; The first step: Under a nitrogen atmosphere, 20.00g of raw material 1, 31.90g of raw material 2, 1.03g of tri-tert-butyl phosphine, 0.36g of palladium carbon, 28.03g of anhydrous potassium carbonate and 230g of toluene were added to the reaction system, and the temperature was raised to 120°C and refluxed for 12 hours; after the reaction was completed, the temperature was slightly lowered, and the reaction was filtered using diatomaceous earth. After the filtrate was cooled to room temperature, it was washed three times with water, the organic phase was retained, and the aqueous phase was then extracted with ethyl acetate. After the organic phases were combined, the organic phase was dried over anhydrous magnesium sulfate, filtered, and dried, and subjected to silica gel column chromatography using a mixture of petroleum ether and ethyl acetate as eluent, and dried to obtain 29.53g of intermediate 1.

[0032] Step 2: Under a nitrogen atmosphere, 29.53 g of intermediate 1, 29.61 g of raw material 3, 41.56 g of potassium phosphate trihydrate, 0.1 g of pyridine-2-carboxylic acid, 0.75 g of CuI and 400 g of DMSO were added to the reaction system, and the mixture was heated to 85°C and reacted for 16 hours; after cooling, the reaction mixture was extracted with an ammonia solution and methyl tert-butyl ether, and the organic phase was washed five times with water and twice with a saturated NaCl solution; finally, the combined organic phase was dried over anhydrous Na2SO4, spin-dried, and purified on a silica gel column, using a mixed solution of petroleum ether and ethyl acetate as eluent, and the solution was spin-dried to obtain 38.48 g of antioxidant 1.

[0033] Structure identification: MS (m / z) of intermediate 1: [M+H] + =379; MS (m / z) of antioxidant 1: [M+H] + =614; Antioxidant 1 1 HNMR-CDCl3: δ7.86(m,1H),7.63(d,1H),7.53-7.35(m,4H),7.26-7.04(m,5H),7.0 1-6.64(m,10H),5.94(s,1H),5.55(s,1H),2.91(d,6H),2.49(d,3H),2.35(d,3H).

[0034] Synthesis Example 2 - Synthesis Example 4 In Synthesis Examples 2-4, antioxidants 2-4 were synthesized in sequence, referring to the synthesis method of Synthesis Example 1, replacing raw material 1, and remaining the same as Synthesis Example 1. Specific structures of raw material 1, antioxidants 2-4, and MS (m / z): [M+H] + See Table 1 for data.

[0035] Table 1 Structure of raw material 1, antioxidant 2-antioxidant 4 involved in Synthesis Examples 2-4, MS (m / z): [M+H] + data Example 1 Preparation of insulating material for prefabricated cable accessories: 1. Raw material composition and mass fraction: 100 parts of ethylene propylene diene monomer rubber (EPDM) (Mooney viscosity ML (1+4) at 125°C is 65-75), 55 parts of reinforcing filler (carbon black, carbon black N550), 30 parts of plasticizer (paraffin oil), 2.5 parts of cross-linking agent (dicumyl peroxide), 2 parts of auxiliary cross-linking agent (triallyl isocyanurate), 3 parts of antioxidant (antioxidant 1 synthesized in Synthesis Example 1), and 3 parts of processing aid (stearic acid, industrial grade).

[0036] 2. Preparation method: S1. Add EPDM rubber, reinforcing filler, and plasticizer to an internal mixer. Set the mixer rotor speed to 40 rpm and the fill factor to 75%. Mix at 80°C for 6.5 minutes. During mixing, the materials are evenly dispersed without lumps, yielding Material A.

[0037] S2. Transfer material A to an open mill and add an antioxidant, processing aid, and cross-linking agent. Set the mill temperature to 50°C and mix for 10 minutes. After mixing, the material is a uniform gel with no precipitation or agglomeration, yielding material B.

[0038] S3. Cool material B to 35°C and add a crosslinking agent. Mix the mixture evenly on an open mill and thinly pass it through the mill (thinning 5 times, with a thickness of about 2 mm) to obtain a rubber mix.

[0039] S4. Place the rubber mix in a prefabricated cable accessory mold and vulcanize using sulfur in a flat-plate vulcanizer. Vulcanization conditions: temperature 175°C, pressure 12.5 MPa, time 17.5 minutes. After vulcanization, immediately transfer the sample to an oven and heat treat at 150°C for 3 hours to eliminate internal stress. Cool the sample to room temperature (25°C) using air cooling at a wind speed of 2 m / s, to obtain an insulating material for prefabricated cable accessories.

[0040] Example 2-Example 4 A prefabricated insulating material for cable accessories is prepared by referring to the preparation method of Example 1, wherein the antioxidant is replaced with antioxidant 2 to antioxidant 4 synthesized in Synthesis Examples 2 to 4 in sequence, and the rest remains the same as Example 1.

[0041] Comparative Example 1 The preparation of an insulating material for a prefabricated cable accessory is carried out by referring to the preparation method of Example 1, except that the antioxidant is not added, and the rest of the preparation is the same as that of Example 1.

[0042] Comparative Example 2 A prefabricated insulating material for cable accessories was prepared by referring to the preparation method of Example 1, except that the antioxidant was replaced with comparative compound 1, and the rest remained the same as Example 1.

[0043] Comparative compound 1: .

[0044] Comparative Example 3 An insulating material for a prefabricated cable accessory is prepared by referring to the preparation method of Example 1, except that the mass fraction of the plasticizer is replaced with 10 parts, and the rest remains the same as Example 1.

[0045] Comparative Example 3 An insulating material for a prefabricated cable accessory is prepared by referring to the preparation method of Example 1, except that the mass fraction of the reinforcing filler is replaced with 85 parts, and the rest remains the same as Example 1.

[0046] Performance testing: 1. Tear strength: The tear strength of the prefabricated cable accessory insulation material prepared in the examples and comparative examples was tested with reference to GB / T 529 2008. The data are shown in Table 2.

[0047] 2. Aging Performance Test: The prefabricated cable accessory insulation material prepared in the Examples and Comparative Examples was tested for aging performance (135°C hot air accelerated aging for 168 hours, testing the change in elongation at break) in accordance with GB / T 528-2009. The data are shown in Table 2.

[0048] 3. Hardness test: The hardness of the prefabricated insulating material for cable accessories prepared in the embodiment and the comparative example was tested with reference to GB / T531.1-2008. The data are shown in Table 2.

[0049] Table 2 Performance test data of the prefabricated cable accessories insulation materials prepared in the examples and comparative examples The examples using the antioxidant of the present invention exhibit significantly improved overall performance trends compared to the comparative examples: tear strength is significantly improved, indicating that the material has better mechanical damage resistance; the change rate of elongation at break is smaller, reflecting that the material can better maintain its elasticity after aging and has better aging resistance; and the hardness is also higher, reflecting more stable material rigidity. In contrast, the comparative examples show a downward trend in tear strength, performance retention after aging, and hardness due to the lack of antioxidant or the adjustment of composition, resulting in poor overall performance.

[0050] Application Examples A prefabricated cable accessory (such as Figure 2 The preparation method includes forming a stress cone, an insulating body and a sealing structure, and the specific steps are as follows: 1. Selection of insulation material: Use the prefabricated cable accessory insulation material prepared in Example 1; 2. Stress Cone Forming: The insulating material is placed in a dedicated stress cone mold and vulcanized in a flat vulcanizer under the following conditions: temperature 175°C, pressure 12.5 MPa, and time 17.5 minutes. After vulcanization, the material is immediately transferred to a 150°C oven for heat treatment for 3 hours to eliminate internal stress. The material is then cooled to room temperature by air cooling (wind speed 2 m / s) to produce the stress cone component. The Shore A hardness of the resulting stress cone is 65. 3. Insulation body molding: Using the same insulation material and vulcanization process (same as step 2), molding in the insulation body mold, and obtaining the insulation body component after cooling; 4. Sealing structure assembly: Assemble the vulcanized stress cone and the insulating body through interference fit, and apply silicone sealant on the joint to form a complete sealing structure.

[0051] 5. Performance Verification: Insulation material samples were tested in accordance with GB / T 528-2009 at 135°C for 168 hours in an air box. The elongation at break retention was 94.8%. The prefabricated cable accessories are suitable for 10-35kV cross-linked polyethylene cable terminals.

[0052] While embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions, and variations may be made to these embodiments without departing from the principles and spirit of the invention, and that the scope of the invention is defined by the appended claims and their equivalents.

Claims

1. An insulating material for prefabricated cable accessories, characterized in that: The invention is composed of the following raw materials in parts by mass: 100 parts of EPDM rubber, 40-70 parts of reinforcing filler, 20-40 parts of plasticizer, 1.5-3.5 parts of crosslinking agent, 1-3 parts of co-crosslinking agent, 1-3 parts of antioxidant, and 1-5 parts of processing aid; The antioxidant has a structure shown in Formula 1: Formula 1; The R1 is selected from the group consisting of: methyl, ethyl, tert-butyl, and methoxy.

2. The prefabricated insulating material for cable accessories according to claim 1, characterized in that: The reinforcing filler is carbon black; The plasticizer is paraffin oil; The cross-linking agent is dicumyl peroxide; The auxiliary cross-linking agent is triallyl isocyanurate; The processing aid is stearic acid.

3. The prefabricated insulating material for cable accessories according to claim 1, characterized in that: The antioxidant is any one of the compounds shown in the following structures: ; 。 4. A method for preparing an insulating material for a prefabricated cable accessory according to any one of claims 1 to 3, characterized in that: The following steps are involved: S1. The EPDM rubber, reinforcing filler, and plasticizer were added to an internal mixer and mixed at 70-90 ° C for 5-8 minutes to obtain material A; S2. Add the antioxidant, processing aid, and cross-linking agent to the material A and mix on an open mill at 40 to 60 ° C for 10 minutes to obtain material B; S3. The material B is cooled to 30-40 ℃, the crosslinking agent is added, and the mixture is uniformly mixed and then thinly passed through the sheet to obtain a mixed rubber set; S4. The rubber mixture is placed in a mold, vulcanized at 170-180°C and 10-15 MPa pressure for 15-20 minutes, and cooled to obtain a prefabricated insulating material for cable accessories.

5. The method for preparing an insulating material for prefabricated cable accessories according to claim 4, characterized in that: After the vulcanization in S4, heat treatment is carried out in an oven at 150° C. for 2-4 hours; The vulcanizing agent is sulfur.

6. The method for preparing an insulating material for prefabricated cable accessories according to claim 4, characterized in that: The rotor speed of the internal mixer in S1 is 30-50 rpm, and the filling factor is 70%-80%.

7. The method for preparing an insulating material for prefabricated cable accessories according to claim 4, characterized in that: The cooling in S4 is air cooling.

8. A prefabricated cable accessory, comprising a stress cone, an insulating body and a sealing structure, characterized in that: The stress cone and / or the insulating body are made of the insulating material for prefabricated cable accessories according to any one of claims 1 to 3.

9. The prefabricated cable accessory according to claim 8, characterized in that: The insulation material has an elongation at break retention rate of ≥85% after aging in an air box at 135°C for 168 hours; The Shore A hardness of the stress cone is ≤68.

10. Use of the prefabricated cable accessory according to any one of claims 8 to 9 at the terminal and / or intermediate connection of a 10-35 kV cross-linked polyethylene cable.

Citation Information

Patent Citations

  • Nonlinear ethylene propylene diene monomer composite material and preparation method thereof

    CN109880239A

  • Insulating rubber for modified alternating-current cable accessory and preparation method of insulating rubber

    CN112375302A

  • Ethylene-propylene-diene monomer insulating material with high mechanical property and preparation method thereof

    CN114516990A

  • Rubber composite, processing method, rubber tube applying composite, and manufacturing method

    WO2018130199A1

  • Insulation material for power cable of low-voltage wind turbine generator and preparation method

    WO2025129896A1