A polyurea that imparts self-healing properties to PVC hoses, its preparation method and application
By introducing polyurea with disulfide and hydrogen bonds into PVC hoses, a multi-layer dynamic cross-linked network is formed, which solves the problems of insufficient toughness and inability to self-heal under dynamic stress in PVC hoses. This achieves improved high strength and self-healing performance, while reducing process complexity and environmental pollution risks.
Patent Information
- Application Number
- CN202510724395.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-06-03
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2045-06-03
AI Technical Summary
Traditional PVC hoses lack toughness under dynamic stress and cannot effectively repair large-scale cracks, resulting in poor reliability of the material under complex working conditions and complicated replacement process, wasting materials and manpower.
Polyurea, which incorporates disulfide and hydrogen bonds through solution polymerization, crosslinks with PVC material during high-temperature processing to form a multi-layered dynamic crosslinking network, thus endowing PVC hoses with self-healing properties.
It significantly improves the mechanical strength and self-healing efficiency of PVC hoses, increases tensile strength by 15.5 MPa, increases elongation at break to 422%, and achieves a self-healing efficiency of over 40% within 3 hours at 80℃, avoiding the use of additional repair agents and environmental pollution.
Smart Images

Figure CN120665379B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of polymer materials technology, specifically designing a method for preparing polyurea and its application in the modification of polyvinyl chloride (PVC) hoses. Background Technology
[0002] The material advantages of polyvinyl chloride (PVC) hoses stem from their unique physicochemical properties. The presence of chlorine atoms in their molecular chains endows the material with excellent resistance to corrosion from acids, alkalis, salts, and organic solvents. The material is lightweight, easy to install, and has low processing costs and mature manufacturing processes. Furthermore, PVC hoses possess good electrical insulation and anti-aging properties, demonstrating high cost-effectiveness and long service life in building piping, industrial fluid transportation, and agricultural irrigation. However, with technological advancements and increasingly complex application scenarios, the inherent performance defects of PVC materials are gradually becoming more apparent.
[0003] Traditional PVC hoses, while possessing a certain degree of flexibility due to the addition of large amounts of plasticizers, still suffer from insufficient toughness during long-term service, especially under dynamic stress environments, making them prone to structural failure due to the propagation of microcracks. This limits their reliability under complex working conditions and poses safety hazards for the transportation of hazardous materials. Furthermore, when dealing with large-scale cracks and other damage already formed in the use of such PVC hoses, the only solution is to replace them with new hoses. This approach ignores the value of undamaged parts, resulting in significant material waste and a complex and labor-intensive installation process.
[0004] Traditional modification methods often struggle to balance dynamic toughness and self-healing properties. Patent CN103554729A proposes introducing thermoplastic polyurethane elastomers, utilizing the flexibility of linear polyurethane and the hydrogen bonding interactions within the polyurethane to improve the toughness of PVC pipes and extend the service life of PVC hoses. However, because this method simply replaces traditional rubber with linear polyurethane for toughening, the improved properties are limited. While it can delay crack initiation, it cannot actively repair existing large-scale damage, thus restricting the material's service life under long-term cyclic loading or accidental impacts. Summary of the Invention
[0005] The purpose of this invention is to address the shortcomings of current PVC hoses, such as insufficient toughness under dynamic conditions and inability to repair large-scale cracks, by providing a polyurea that imparts self-healing properties to PVC hoses, along with its preparation method and applications. The polyurea possesses structures including disulfide bonds and hydrogen bonds. In preparation, solution polymerization is used to induce an addition polymerization reaction between diamine dihydrochloride and diisocyanate containing disulfide bonds. The addition of excess triethylamine allows for reaction with hydrogen chloride in the diamine dihydrochloride, improving its solubility. In application, a twin-screw extrusion method is used during thermal processing to mix the polyurea containing disulfide bonds and hydrogen bonds with PVC material. During high-temperature processing, PVC undergoes partial decomposition, generating unsaturated bonds. These unsaturated bonds cross-link with the disulfide bonds in the polyurea at high temperatures, effectively compatibility between the polyurea and PVC, thus improving the overall performance of the pipe. This invention achieves a self-healing efficiency of >40% within 3 hours at 80°C. Compared to traditional encapsulation repair agent technology, this self-healing process requires no additional repair agent, significantly reducing process complexity and avoiding the environmental pollution risks caused by repair agent leakage.
[0006] The technical solution of this invention is as follows:
[0007] A polyurea that imparts self-healing properties to PVC hoses, the polyurea having the following structure:
[0008]
[0009] Where R is the alkyl part of the diisocyanate, and n = 1 to 10000.
[0010] The method for preparing the polyurea that imparts self-healing properties to PVC hoses includes the following steps:
[0011] S1: Dissolve diamine dihydrochloride and triethylamine in a solvent and stir for 0.5–1.5 h to obtain a clear solution;
[0012] The molar ratio of triethylamine to diamine dihydrochloride is (5–15):1; the mass ratio of solvent to triethylamine is (2–10):1.
[0013] The diamine dihydrochloride mentioned is cystamine dihydrochloride;
[0014] The solvent is a ketone solvent, an aromatic solvent, or other organic solvent; specifically, it is one or more of methyl ethyl ketone, acetone, N,N-dimethylformamide, N,N-dimethylacetamide, ethyl acetate, toluene, dimethyl sulfoxide, dichloromethane, tetrahydrofuran, and dioxane.
[0015] S2: Add diisocyanate to the clear solution obtained in S1, heat to 30-80℃ and react for 18-30 h; remove the solvent and finally obtain a white powder product PUS, which is polyurea that gives PVC hoses self-healing properties.
[0016] The molar ratio of the diisocyanate to the diamine dihydrochloride in S1 is (0.9–1.1):1;
[0017] The diisocyanates mentioned include aliphatic diisocyanates, aromatic diisocyanates, or alicyclic diisocyanates;
[0018] Specifically, it includes hexamethylene diisocyanate (HDI), lysine diisocyanate (LDI), toluene diisocyanate (TDI), diphenylmethane diisocyanate (MDI), isoflurone diisocyanate (IPDI), or dicyclohexylmethane diisocyanate (HMDI).
[0019] The specific structure is shown in the figure below;
[0020]
[0021] The application of polyurea, which imparts self-healing properties to PVC hoses, is used in the preparation of PVC hoses;
[0022] Specifically, the steps include the following:
[0023] Polyvinyl chloride resin, a prepared light yellow powdered polyurea, compatibilizer, antioxidant, heat stabilizer, and lubricant are added to a high-speed mixer in proportion and premixed at 100-120℃ for 40-50 minutes. The mixture is then cooled to 30-40℃ to form a premix for later use. The premix is fed into a granulator for granulation, and the granules are transferred to the extruder barrel. The extruder feed section temperature is controlled at 100-120℃, the compression section temperature at 120-140℃, the metering section at 140-160℃, the die temperature at 150-160℃, and the extruder screw speed at 30-35 r / min. After cooling, shaping, traction, and cutting, a self-healing PVC hose is obtained.
[0024] The mass ratio of polyvinyl chloride resin to prepared light yellow powdered polyurea is (80-120): (10-30): (3-8): (1-3): (1-3): (25-15).
[0025] The polyvinyl chloride is a powder with a particle size of 10–30 μm.
[0026] The compatibilizer is maleic anhydride-grafted PVC, the antioxidant is antioxidant 1010, the heat stabilizer is dibutyltin dilaurate, and the plasticizer is dioctyl phthalate.
[0027] The essential features of this invention are:
[0028] This invention addresses the common challenge of traditional modification methods that fail to balance toughness and self-healing properties. By solution polymerization of diisocyanate and diamine hydrochloride, monomers containing dynamic disulfide bonds are introduced into polyurea. These dynamic bonds can crosslink with double bonds generated during thermal processing, thus promoting compatibility between PVC and polyurea. Furthermore, these dynamic disulfide bonds, along with the dynamic hydrogen bonds in the polyurea, form a dynamic crosslinking network. Compared to traditional toughening modifications, the presence of these multiple dynamic bonds not only provides excellent mechanical strength to composite PVC hoses but also endows the material with self-healing properties under thermal stress.
[0029] The beneficial results of this invention are:
[0030] This invention introduces dynamic disulfide bonds into the polyurea backbone through solution polymerization and combines them with urea hydrogen bonds in the polyurea to form a multi-dynamic cross-linking network. (1) During high-temperature processing, the double bonds generated by the partial decomposition of PVC undergo in-situ cross-linking with the disulfide bonds in the dynamic polyurea, significantly reducing the polarity difference between the two phases. Combined with the polar adsorption effect of the compatibilizer maleic anhydride grafted onto PVC, the interfacial bonding strength is significantly improved. Compared with pure physical blending in other materials, the chemical cross-linking strategy of this invention significantly improves the uniformity of the material. Compared with simply adding plasticizer, the tensile strength can be increased from 12.2 MPa to 15.5 MPa; (2) The three-dimensional interpenetrating network of dynamic polyurea is uniformly embedded in the PVC matrix through high shear dispersion by twin screws. While maintaining the rigidity of PVC, the elongation at break increases from 310% to 422%; (3) The synergistic effect of multiple dynamic bonds makes the material self-healing efficiency >40% within 3 hours at 80℃. Compared to traditional encapsulation repair agent technology, this self-healing process requires no external stimuli or additional repair agents, greatly reducing process complexity and avoiding the environmental pollution risk caused by repair agent leakage.
[0031] This invention overcomes the technical bottlenecks of poor compatibility between modified materials and PVC, insignificant toughening effect, and lack of self-healing properties by introducing multiple dynamic bonds and chemical compatibilization strategies. It successfully develops a functional PVC hose with both high mechanical strength and self-healing properties, providing a long-life and low-maintenance solution for the medical, industrial, and intelligent equipment fields. Attached Figure Description
[0032] Figure 1 This is the XPS image of the S element in the polyurea PUS obtained in Example 1. Detailed Implementation
[0033] This invention systematically describes the technical solution through specific embodiments. The examples shown are merely representative implementations of this invention and are not an exhaustive list of all possible implementations. Based on the technical principles disclosed in this invention, any implementation scheme implemented by those skilled in the art through equivalent substitution or conventional technical means without creative effort falls within the protection scope of the patent claims of this invention.
[0034] The reaction formula of this invention is as follows:
[0035]
[0036] Where n = 1 to 10000.
[0037] The polyurea of this invention is used in PVC hoses to impart high toughness and self-healing properties to the hoses. Examples 1-4 illustrate the preparation of self-healing PVC hoses.
[0038] Example 1
[0039] (1) Synthesis of PUS: Cystamine dihydrochloride (90 g, 0.4 mol) was dissolved in 2 L of DMF, and triethylamine (400 g, 4 mol) was added and stirred for 1 h to obtain a clear solution. Then IPDI (88.8 g, 0.4 mol) was added dropwise. The reaction solution was heated to 40 °C and reacted for 24 h. After the reaction was completed, the solvent was removed. The final product, white powder PUS, was obtained with a yield of approximately 68%.
[0040] like Figure 1 As shown, in PUS, S(2p 1 / 2 ) and S(2p 3 / 2 The peaks at 164.50 eV and 163.38 eV indicate that the SS bond was successfully introduced into the polyurea.
[0041] (2) Preparation of PVC-PUS 110-10 Hose: Polyvinyl chloride resin (110 parts, powder, particle size 20μm), PUS (10 parts), maleic anhydride-grafted PVC (4 parts), antioxidant 1010 (2 parts), dibutyltin dilaurate (2 parts), and dioctyl phthalate (20 parts) are added to a high-speed mixer in proportion and premixed at 110℃ for 40 minutes at 100 rpm. The mixture is then cooled to 35℃ to form a premix. The premix is fed into a granulator for granulation. The granules (approximately 3-5 mm) are transferred to the extruder barrel. The extruder feed section temperature is set to 110℃, the compression section temperature to 130℃, the metering section temperature to 150℃, and the die temperature to 160℃. The extruder screw speed is set to 30 rpm. Feeding begins after the temperature stabilizes. After cooling and shaping with tap water, traction, and cutting, a self-healing PVC hose is obtained, named PVC-PUS. 110-10.
[0042] All quantities mentioned are by weight.
[0043] Example 2
[0044] The other steps are the same as in Example 1, except that the polyvinyl chloride resin (110 parts) and PUS (10 parts) are replaced with polyvinyl chloride resin (105 parts) and PUS (15 parts) to obtain PVC-PUS. 105-15 ;
[0045] Example 3
[0046] The other steps are the same as in Example 1, except that the polyvinyl chloride resin (110 parts) and PUS (10 parts) are replaced with polyvinyl chloride resin (100 parts) and PUS (20 parts) to obtain PVC-PUS. 100-20 ;
[0047] Example 4
[0048] The other steps are the same as in Example 1, except that the polyvinyl chloride resin (110 parts) and PUS (10 parts) are replaced with polyvinyl chloride resin (95 parts) and PUS (25 parts) to obtain PVC-PUS. 95-25 ;
[0049] Example 5
[0050] The other steps are the same as in Example 1, except that the polyvinyl chloride resin (110 parts) and PUS (10 parts) are replaced with polyvinyl chloride resin (90 parts) and PUS (30 parts) to obtain PVC-PUS. 90-30 .
[0051] Comparative Example 1
[0052] Preparation of PVC hoses: Polyvinyl chloride resin (120 parts), compatibilizer (4 parts), antioxidant (2 parts), heat stabilizer (2 parts), and plasticizer (20 parts) are added to a high-speed mixer in proportion and premixed at 110℃ for 40 minutes. The mixture is then cooled to 35℃ to form a premix. The premix is then subjected to granulation, extrusion, cooling and shaping, traction, and cutting to obtain the PVC hose, which is named PVC.
[0053] To verify the properties of the materials obtained in Examples 1-5 and Comparative Example 1, relevant characterization and performance tests were performed on them below.
[0054] (I) Tensile Strength
[0055] The tensile strength of the materials prepared in Examples 1-5 and Comparative Example 1 was tested according to the method specified in GB / T1040.2-2006, and the specific data are shown in Table 1.
[0056] (II) Self-healing performance test
[0057] Cut at least three samples in half lengthwise with a blade, press the cut surfaces together and fix them in place. Remove the samples from the oven at 80°C after 3 hours and perform tensile strength testing according to the method specified in GB / T 1040.2-2022. Specific data are shown in Table 1.
[0058] Table 1 Performance of PUS-modified PVC hose in this invention
[0059]
[0060] In this invention, by adding polyurea containing disulfide bonds and hydrogen bonds, not only is the toughness of PVC hoses significantly improved (tensile strength and elongation at break are both increased), but the PVC hoses are also endowed with very good self-healing properties. After optimization, the repair rate can reach more than 40%.
[0061] The embodiments listed in this invention are only used to illustrate several preferred technical solutions and are not intended to limit the scope of protection. The foregoing embodiments are intended to provide exemplary technical guidance, not to exhaustively limit the scope. Any adaptive adjustments made by those skilled in the art, based on the teachings of this invention and without departing from the core design concept of this invention, through equivalent substitutions, structural modifications, or process improvements, including but not limited to adjustments, supplements, or optimizations to composition ratios, implementation steps, or technical parameters, should be considered to fall within the scope of protection of the claims of this invention.
[0062] Matters not covered in this invention are common knowledge.
Claims
1. A polyurea conferring self-repairing properties to PVC hoses, characterized by, The polyurea has the following structure: , Wherein, R is the alkyl part of the diisocyanate, and n = 1~10000; The method for preparing the polyurea that imparts self-healing properties to PVC hoses includes the following steps: S1: Dissolve diamine dihydrochloride and triethylamine in a solvent and stir for 0.5-1.5 h to obtain a reaction solution; The molar ratio of triethylamine to diamine dihydrochloride is (5~15):1; the mass ratio of solvent to triethylamine is (2~10):
1. S2: Add diisocyanate to the reaction solution obtained in S1, heat to 30~80 ℃ and react for 18~30 h to obtain polyurea that imparts self-healing properties to PVC hoses; The molar ratio of the diisocyanate to the diamine dihydrochloride in S1 is (0.9~1.1):1; The diisocyanates mentioned include aliphatic diisocyanates, aromatic diisocyanates, or alicyclic diisocyanates; The diamine dihydrochloride mentioned is cystamine dihydrochloride; The solvent is one or more of methyl ethyl ketone, acetone, N,N-dimethylformamide, N,N-dimethylacetamide, ethyl acetate, toluene, dimethyl sulfoxide, dichloromethane, tetrahydrofuran, and dioxane.
2. The polyurea that imparts self-healing properties to PVC hoses as described in claim 1, characterized in that, In the preparation method, the diisocyanate is hexamethylene diisocyanate, lysine diisocyanate, toluene diisocyanate, diphenylmethane diisocyanate, isoflurone diisocyanate, or dicyclohexylmethane diisocyanate.
3. The application of polyurea as described in claim 1, which imparts self-healing properties to PVC hoses, is characterized in that... Used in the preparation of PVC hoses.
4. The application of polyurea as described in claim 3, which imparts self-healing properties to PVC hoses, is characterized in that... Includes the following steps: Polyvinyl chloride resin, a prepared light yellow powdered polyurea, compatibilizer, antioxidant, heat stabilizer, and lubricant are added to a high-speed mixer in proportion and premixed at 100-120 ℃ for 40-50 min. The mixture is then cooled to 30-40 ℃ to form a premix for later use. The premix is fed into a granulator for granulation, and the granules are transferred to the extruder barrel. The extruder feed section temperature is controlled at 100-120 ℃, the compression section temperature at 120-140 ℃, the metering section temperature at 140-160 ℃, the die temperature at 150-160 ℃, and the extruder screw speed at 30-35 r / min. After cooling, shaping, traction, and cutting, a self-healing PVC hose is obtained. The mass ratio of polyvinyl chloride resin to prepared light yellow powdered polyurea is (80~120): (10~30): (3~8): (1~3): (1~3): (25~15).
5. The application of polyurea as described in claim 4, which imparts self-healing properties to PVC hoses, is characterized in that... The polyvinyl chloride is a powder with a particle size of 10~30 μm.
6. The application of polyurea as described in claim 4, which imparts self-healing properties to PVC hoses, is characterized in that... The compatibilizer is maleic anhydride-grafted PVC, the antioxidant is antioxidant 1010, the heat stabilizer is dibutyltin dilaurate, and the plasticizer is dioctyl phthalate.
Citation Information
Patent Citations
Environment-friendly PVC (polyvinyl chloride) hose material
CN103554729A
Polyurea self-repairing thermoplastic elastomer and preparation method thereof
CN108659188A
High-performance self-repairing polyurea and preparation method thereof
CN114685756A
Self-repairing polyurethane toughened polyvinyl chloride composite material and preparation method thereof
CN117534921A