Device and method for producing engineering plastics through continuous polymerization of rubber liquid

Through the direct coupling process of rubber liquid and the closed-loop recovery technology of solvent, the problems of high energy consumption and low efficiency in the traditional continuous bulk method are solved, the efficient polymerization of rubber liquid and the recycling of solvent are achieved, and the performance and production efficiency of ABS resin are improved.

CN120714560AActive Publication Date: 2025-09-30ZHONGZHE (ZHEJIANG) POLYMER NEW MATERIALS CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202511212250.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-08-28
Publication Date
2025-09-30
Estimated Expiration
2045-08-28

AI Technical Summary

Technical Problem

The traditional continuous bulk process for producing HIPS and ABS resins has problems of high energy consumption, low efficiency and environmental pollution, especially in the rubber pretreatment process, which has low solvent utilization, high energy consumption, uneven particle size and serious dust pollution.

Method used

The rubber liquid direct coupling process is adopted, through the innovative design of the rubber liquid direct transmission system, premixing unit and solvent recovery system, including polymerization kettle, dynamic mixer, devolatilization tower and azeotropic distillation tower, to achieve solvent-loss-free polymerization of rubber liquid and solvent closed-loop recovery, thereby optimizing the polymerization process.

Benefits of technology

It significantly reduces equipment investment and energy consumption, improves solvent recovery rate, shortens process time, improves rubber particle size dispersion and low-temperature toughness of ABS resin, and reduces environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120714560A_ABST
    Figure CN120714560A_ABST
Patent Text Reader

Abstract

The invention provides a device and method for producing engineering plastics through continuous polymerization of a rubber solution, and the device comprises a direct rubber solution conveying system which is provided with a polymerization kettle; the premixing unit comprises a dynamic mixer and a premixing kettle; the solvent recovery system comprises a devolatilization tower and an azeotropic rectification tower; wherein the polymerization kettle is directly connected with the premixing unit through a thermal insulation pipeline. According to the invention, the glue solution is directly used for polymerization production of ABS or HIPS, and the cyclohexane solvent is refined and recycled, so that the problems of high energy consumption, low efficiency, complex flow, environmental pollution and the like in the traditional process can be solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of styrene resins, and in particular to a device and method for producing engineering plastics by continuous polymerization of rubber glue. Background Art

[0002] Acrylonitrile butadiene styrene (ABS) is a general-purpose plastic widely used in construction, transportation, communications, home appliances, electronics, and daily necessities. High fracture toughness is one of the key factors contributing to the widespread application of ABS resin. The structure of a polymer determines its properties. The butadiene component imparts toughness and low-temperature resistance to ABS resin, which in turn enhances its impact resistance. Therefore, the primary factors influencing the impact properties of ABS resin are the composition and structural parameters of the rubber phase. Therefore, the selection of toughening rubber is a key technology in the synthesis and research of ABS resin. In the preparation of high-impact polystyrene resin (HIPS) and ABS, rubbers commonly used as toughening agents include low-cis polybutadiene rubber, high-cis polybutadiene rubber, butadiene-isoprene copolymer, solution-polymerized styrene-butadiene rubber, and styrene-butadiene-styrene copolymer.

[0003] Continuous bulk polymerization is one of the main processes for producing HIPS and ABS resins. Heated rubber is blended with acrylonitrile, styrene, and a solvent, and then appropriate amounts of regulators and initiators are added to complete the graft polymerization. The production principle is that the acrylonitrile and styrene copolymer forms the continuous phase, while the grafted rubber particles form the dispersed phase. After granulation and devolatilization, the final resin product is obtained. However, the continuous bulk polymerization process is relatively complex. To fully incorporate the rubber into the monomer mixture, the polymerization process must be well controlled, and strict control is required for rubber particle size, rubber dosage and type, and grafting rate.

[0004] The traditional continuous bulk process for producing ABS or HIPS generally uses solid polybutadiene rubber or styrene-butadiene rubber as raw material, requiring a lengthy pretreatment process consisting of rubber synthesis, solvent drying, crushing, and dissolution. The rubber synthesis process uses solvents such as cyclohexane, which must be removed through high-temperature drying, resulting in 30% energy consumption and a solvent recovery rate of only 70%-75%. After drying, the rubber must be redissolved in styrene / acrylonitrile monomers, requiring additional ethylbenzene as a diluent. This results in a solvent utilization rate of less than 60%, the introduction of mechanical impurities, and a particle size variability exceeding 40%. The drying process requires heating the rubber to 120°C-150°C, consuming over 30% of the total process energy. The crushing process also generates dust pollution, requiring dust removal equipment, further increasing investment and operating costs.

[0005] It can be seen that the problems of solvent compatibility, high energy consumption and green production in the continuous bulk production of HIPS and ABS need to be urgently solved. Summary of the Invention

[0006] In order to solve the above problems, the present invention provides a device and method for producing engineering plastics by continuous polymerization of rubber liquid, aiming to overcome the technical problems of high energy consumption, low efficiency, complex process and environmental pollution in traditional processes through innovative technical means such as direct coupling process of rubber liquid, closed-loop utilization of solvent and dispersion strengthening mechanism.

[0007] The present invention provides a device for producing engineering plastics by continuous polymerization of rubber liquid, comprising: Glue liquid direct delivery system, the glue liquid direct delivery system is equipped with a polymerization kettle; Premixing unit, the premixing unit includes a dynamic mixer and a premixing kettle; Solvent recovery system, including devolatilization tower and azeotropic distillation tower; The polymerization kettle is directly connected to the premixing unit through an insulated pipe.

[0008] Furthermore, the thickness of the insulation layer of the insulated pipe is 50 mm, and the temperature is controlled at 40°C~50°C.

[0009] Furthermore, the glue liquid direct delivery system also includes a glue liquid buffer tank, which is arranged between the polymerization kettle and the premixing unit to match the rates of synthesis and polymerization reactions.

[0010] Furthermore, the premixing kettle comprises: The first premixing kettle, when using low-cis polybutadiene rubber liquid as the raw material, the temperature of the first premixing kettle is 60°C to 70°C, the pressure is 0.9 MPaG, and the stirring speed is 30 rpm to 40 rpm; when using solution polystyrene butadiene rubber liquid as the raw material, the temperature of the first premixing kettle is 65°C to 75°C, the pressure is 0.8 MPaG, and the stirring speed is 40 rpm to 50 rpm; The second premixing kettle, when using low cis polybutadiene rubber liquid as raw material, the temperature of the second premixing kettle is 100°C~110°C, the pressure is 0.85MPaG, and the stirring rate is 50rpm~60rpm; when using low cis polybutadiene rubber liquid as raw material, the temperature of the second premixing kettle is 110°C~120°C.

[0011] Furthermore, the dynamic mixer comprises: The first-stage high-speed shear unit is used to quickly and evenly mix the polymerized adhesive with polar monomers such as styrene and acrylonitrile; The secondary static mixing unit is used to further achieve uniform dispersion and mixing of the polymerized adhesive with polar monomers such as styrene and acrylonitrile; The three-stage ultrasonic oscillation unit has an oscillation frequency of 20kHz and is used to promote the micron-level dispersion of the polar monomer acrylonitrile in the glue.

[0012] Furthermore, the premixing unit includes a multi-stage polymerizer, which includes at least two reactors connected in series, and the temperature gradient is controlled to be 110°C to 160°C.

[0013] Furthermore, when low-cis polybutadiene rubber solution is used as raw material, the operating temperature of the devolatilization tower is 120°C~130°C and the pressure is 0.5MPaG; when solution-polymerized styrene-butadiene rubber solution is used as raw material, the operating temperature of the devolatilization tower is 160°C and the pressure is 0.4MPaG.

[0014] Furthermore, the azeotropic distillation tower is provided with a solvent heat circulation loop for preheating the distillation feed with the waste heat of the polymerization reaction.

[0015] The present invention also provides a method for producing engineering plastics by continuous polymerization of rubber glue, comprising the following steps: synthesizing rubber; carrying out solvent-loss-free polymerization reaction using the rubber glue as raw material; and closed-loop recovery of the solvent; wherein the rubber glue is at least one of solution-polymerized styrene-butadiene rubber and low-cis polybutadiene rubber.

[0016] Furthermore, the synthesis parameters of the rubber solution include: When preparing the low-cis polybutadiene rubber solution, n-butyl lithium is used as the catalyst with a concentration of 1.5 mol / L~2.0 mol / L, an amount of 0.5‰~1.0‰, a polymerization temperature of 80±5℃, a pressure of 0.6 MPaG, and a reaction time of 4h~5h; When preparing the solution of solution-polymerized styrene-butadiene rubber, n-butyl lithium is used as a catalyst with a concentration of 1.5 mol / L~2.0 mol / L, an amount of 0.5‰~1.0‰, a synthesis temperature of 50℃~65℃, a pressure of 0.3MPaG~0.5MPaG, and a reaction time of 4h~6h.

[0017] Further, the parameters of the polymerization reaction include: When low-cis polybutadiene rubber glue is used as the raw material, the low-cis polybutadiene rubber glue accounts for 25% to 35% of the total mass of the glue, styrene accounts for 45% to 55% of the total mass of the glue, acrylonitrile accounts for 10% to 15% of the total mass of the glue, the dispersant accounts for 1% to 2% of the total mass of the glue, and the initiator accounts for 0.05% to 0.1% of the total mass of the glue; the dispersant is sorbitan oleate, and the initiator is di-tert-butyl peroxide; When solution polymerized styrene-butadiene rubber (SBR) is used as the raw material, the SBR accounts for 30% to 40% of the total mass of the SBR, styrene accounts for 50% to 60% of the total mass of the SBR, acrylonitrile accounts for 10% to 15% of the total mass of the SBR, and chemical additives account for 0.2% to 0.5% of the total mass of the SBR; the chemical additives include initiators, chain transfer agents, and antioxidants.

[0018] After adopting the technical solution of the present invention, the following technical effects can be achieved: 1. The synthesized adhesive liquid is directly fed into the pre-mixing unit through an insulated pipe, eliminating the processes of solvent drying, crushing and dissolving. The processes are seamlessly connected, the process time is shortened to 6 hours, and the equipment investment is reduced by 25%.

[0019] 2. The optimized premixing unit, through a three-stage shear dynamic mixer, namely high-speed shearing, static mixing, and ultrasonic vibration, can improve the dispersion of rubber particles, disperse the solution-polymerized styrene-butadiene rubber liquid to 20μm~30μm, increase the exposure rate of grafting sites by 70%, and improve the low-temperature toughness of ABS resin.

[0020] 3. The solvent recovery system uses cyclohexane from the rubber solution as the polymerization reaction medium. Purification is achieved through a three-stage recovery system consisting of a pre-devolatilization tower and an azeotropic distillation tower, increasing the solvent reuse rate to 99.5%. This reduces energy consumption per unit product by 41.7%, process time by 40%, and equipment investment by 27.3%. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 The present invention is a schematic structural diagram of a device for producing engineering plastics by continuous polymerization of rubber liquid.

[0022] Description of reference numerals: 01-Glue liquid direct delivery system; 02-Premixing unit; 03-Solvent recovery system; 11-Polymerization kettle; 12-Glue liquid buffer tank; 13-Insulated pipeline; 21-Dynamic mixer; 22-First premixing kettle; 23-Second premixing kettle; 24-Multi-stage polymerizer; 31-Devolatilization tower; 32-Azeotropic distillation tower. DETAILED DESCRIPTION

[0023] To make the above-mentioned objects, features, and advantages of the present invention more clearly understood, the technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. All other embodiments obtained by persons of ordinary skill in the art based on the embodiments of the present invention without creative effort shall fall within the scope of protection of the present invention.

[0024] When preparing ABS or HIPS using the traditional continuous bulk method, solid polybutadiene rubber or styrene-butadiene rubber is used as the raw material. After synthesis, it undergoes pretreatment processes such as solvent drying, crushing, and redissolution. This not only makes the process lengthy and increases process time, but also consumes a large amount of energy during the solvent drying process, accounting for up to 30% of energy consumption. When cyclohexane is used as the rubber synthesis solvent, it needs to be removed by high temperature during drying, and the solvent recovery rate can only reach 70% to 75%. In addition, additional ethylbenzene is required when the rubber is redissolved in styrene / acrylonitrile monomers, resulting in a comprehensive solvent utilization rate of less than 60%. The rubber during the crushing process will produce mechanical impurities of varying particle sizes, with a particle size unevenness rate exceeding 40%. The dust pollution generated during the crushing process requires additional dust removal equipment to handle, which increases investment and operating costs.

[0025] To solve the above problems, an embodiment of the present invention provides a device for continuously polymerizing rubber liquid to produce engineering plastics, including: a liquid rubber direct delivery system 01, the liquid rubber direct delivery system 01 is provided with a polymerization kettle 11; a premixing unit 02, the premixing unit 02 is provided with a dynamic mixer 21 and a premixing kettle; a solvent recovery system 03, including a devolatilization tower 31 and an azeotropic distillation tower 32; wherein, the polymerization kettle 11 is connected to the premixing unit 02 via an insulated pipe 13.

[0026] First, the synthesis of rubber liquid is completed in the polymerization reactor 11 of the liquid direct delivery system 01.

[0027] Specifically, when preparing a low-cis polybutadiene rubber solution, polymerization kettle 11 is made of an acid-resistant material, preferably glass-lined, with a capacity of 30 m³, a jacket temperature control system of 80°C to 90°C, and a built-in anchor agitator at a speed of 60 rpm. Polymerization kettle 11 is equipped with a styrene and acrylonitrile monomer droplet feed line, and its metering pump has an accuracy of ±0.3%.

[0028] Furthermore, when preparing the low-cis polybutadiene rubber solution, the insulation pipe 13 is made of stainless steel 304, the insulation layer thickness is 30 mm, and the temperature is controlled at 60°C~70°C to prevent condensation of the polymerization system. The pipeline is equipped with a rotor flowmeter with a range of 0m³ / h~5m³ / h and a pressure sensor with a range of 0MPa~0.8MPa.

[0029] Specifically, when preparing the solution of styrene-butadiene rubber, the polymerization kettle 11 is made of an alkane-resistant material, preferably stainless steel 316L, with a volume of 50m³, and the outlet of the polymerization kettle 11 is directly connected to the ABS premixing unit through the insulation pipe 13.

[0030] Furthermore, when preparing the solution of styrene-butadiene rubber, the thickness of the insulation pipe 13 is 50 mm, the temperature is controlled between 40°C and 50°C, and an electromagnetic flowmeter and a pressure sensor are installed in the insulation pipe 13. The accuracy of the flowmeter is ±0.5%, and the range of the sensor is 0 MPa~1 MPa.

[0031] The design of polymerization reactor 11 fully considers the stability and safety of materials during the synthesis process. Different materials are used to synthesize different rubbers. This not only ensures the corrosion resistance and high temperature resistance of polymerization reactor 11, but also ensures the purity of the materials during the synthesis process, avoiding the incorporation of impurities due to material defects. This not only meets the needs of large-scale production, but also ensures the continuity and stability of the synthesis process.

[0032] The insulated pipe 13 effectively reduces heat loss during material transportation, improving energy efficiency. The appropriate temperature control range ensures material fluidity during transportation while preventing material deterioration and increased energy consumption due to excessively high or low temperatures. The configuration of an electromagnetic flowmeter and pressure sensor enables precise monitoring of material flow and pressure, providing strong support for automated control and optimization of the production process.

[0033] Furthermore, when preparing the low-cis polybutadiene rubber solution, the discharge pump of the polymerization kettle 11 is a gear pump with a flow rate of 3m³ / h~8m³ / h, which is linked to the feed valve of the premixing unit 02 through PLC, and the volume ratio of the rubber solution to the styrene feed is 1:2.5.

[0034] Furthermore, when preparing the solution of styrene-butadiene rubber, the discharge pump of the polymerization kettle 11 is a screw pump with a flow rate of 5m³ / h~10m³ / h, which is linked to the feed valve of the premixing unit 02 to achieve a dynamic ratio of 1:3 between the flow rate of the solution and the amount of styrene feed through a distributed control system.

[0035] The PLC and distributed control system can monitor key parameters such as flow and pressure in real time and automatically adjust the proportions based on production needs, significantly improving production efficiency and product quality. Furthermore, this linkage design makes the entire production process more automated and intelligent, reducing manual intervention, operational complexity, and costs.

[0036] In some embodiments of the present application, the glue liquid direct delivery system further includes a glue liquid buffer tank 12, which is disposed between the polymerization kettle 11 and the premixing unit for matching the rates of synthesis and polymerization reactions.

[0037] Specifically, when using low-cis polybutadiene rubber as the raw material, the rubber buffer tank 12 has a capacity of 5 cubic meters, is equipped with a nitrogen protection system, and has a liquid level interlocking device, with a buffer time of ≤20 minutes. When using solution-polymerized styrene-butadiene rubber as the raw material, the rubber buffer tank 12 has a capacity of 10 cubic meters, is equipped with a nitrogen protection system, and is located between the synthesis and polymerization processes to act as a buffer, with a buffer time of ≤30 minutes.

[0038] This design ensures that the production bottleneck problem that may arise from rate mismatch between the two key processes of synthesis and polymerization is effectively alleviated. The presence of the glue buffer tank 12 allows the glue produced in the synthesis process to be temporarily stored, without causing production stagnation due to deviations in the processing speed of the polymerization process. In addition, the buffer time of less than half an hour not only ensures the continuity of the production process, but also avoids quality problems that may arise from long-term storage of the glue during the temporary storage process.

[0039] In some embodiments of the present application, the premixing kettle includes a first premixing kettle 22 and a second premixing kettle 23. When low-cis polybutadiene rubber is used as the raw material, the temperature of the first premixing kettle 22 is 60°C to 70°C, the pressure is 0.9 MPaG, and the stirring rate is 30 rpm to 40 rpm. When solution-polymerized styrene-butadiene rubber is used as the raw material, the temperature of the first premixing kettle 22 is 65°C to 75°C, the pressure is 0.8 MPaG, and the stirring rate is 40 rpm to 50 rpm. When low-cis polybutadiene rubber is used as the raw material, the temperature of the second premixing kettle 23 is 100°C to 110°C, the pressure is 0.85 MPaG, and the stirring rate is 50 rpm to 60 rpm. When solution-polymerized styrene-butadiene rubber is used as the raw material, the temperature of the second premixing kettle 23 is 110°C to 120°C.

[0040] Specifically, when using low-cis polybutadiene rubber as the raw material, the operating conditions of the first premixing kettle 22 are set to a temperature of 60°C to 70°C, within which the polymerization system remains liquid. The pressure is 0.9 MPaG, the stirring rate is 30 rpm to 40 rpm, and the low-cis polybutadiene rubber liquid is dispersed to 40 μm to 50 μm. The second premixing kettle 23 is heated to 100°C to 110°C, which is lower than the boiling point of the polymerization system of 110.6°C. The pressure is 0.85 MPaG, the stirring rate is 50 rpm to 60 rpm, and the free radical grafting polymerization of styrene and acrylonitrile monomers onto the rubber molecular chains is initiated. The monomer conversion rate is controlled at 20% to 25%.

[0041] Specifically, when using solution-polymerized styrene-butadiene rubber (SBR) as the raw material, the operating conditions of the first premixing kettle 22 are set at a temperature of 65°C to 75°C. Within this temperature range, the cyclohexane remains liquid, ensuring that the SBR solution can be evenly dispersed. Simultaneously, a pressure of 0.8 MPaG and a stirring rate of 40 rpm to 50 rpm work together to precisely control the dispersion size of the SBR solution to between 20 μm and 30 μm. This step provides excellent initial conditions for the subsequent polymerization reaction. The second premixing kettle 23 is heated to 110°C to 120°C, at which point the cyclohexane partially vaporizes, maintaining a vaporization rate of 20% to 30%. This design utilizes the latent heat of solvent vaporization to absorb the heat generated during the polymerization reaction, accounting for 40% of the total heat absorbed, effectively reducing the system's need for external cooling. This also reduces the jacket cooling load by 60%, significantly improving energy efficiency and lowering production costs.

[0042] In some embodiments of the present application, the dynamic mixer 21 includes: a first-level high-speed shearing unit for rapidly and evenly mixing the polymerized glue with polar monomers such as styrene and acrylonitrile; a second-level static mixing unit for further achieving uniform dispersion and mixing of the polymerized glue with polar monomers such as styrene and acrylonitrile; and a third-level ultrasonic oscillation unit with an oscillation frequency of 20 kHz for promoting micron-level dispersion of the polar monomer acrylonitrile in the glue.

[0043] Specifically, when low-cis polybutadiene rubber liquid is used as the raw material, the first-stage high-speed shear unit is a serrated rotor with a rotation speed of 1500rpm, which can crush the low-cis polybutadiene rubber liquid to less than 50μm. It is equipped with a cooling jacket to control the temperature ≤70°C to prevent the volatilization of styrene and acrylonitrile monomers. The second-stage static mixing unit uses 9 groups of left-handed / right-handed alternating Kenis mixing elements to promote the formation of a stable emulsion between low-cis polybutadiene rubber liquid and styrene / acrylonitrile. In addition, sorbitan oleate dispersant needs to be additionally injected, and the metering pump addition rate is 1kg / h~2kg / h.

[0044] Specifically, when the glue of solution-polymerized styrene-butadiene rubber is used as raw material, the dynamic mixer 21 works in coordination to ensure the high efficiency of the mixing process and the quality of the mixture by three-stage shearing. First, the rotating speed of the first-level high-speed shearing unit 2000rpm is operated, and its main function is to break the glue into micron-sized liquid beads, which are evenly dispersed in styrene and acrylonitrile monomers, laying the foundation for subsequent mixing steps. Subsequently, the second-level static mixing unit, i.e., the Kenis mixing element, intervenes. The unit realizes the homogenization of phase distribution through a series of static mixing channels, ensuring that each component in the mixture is fully and evenly mixed. Finally, the three-stage ultrasonic oscillation unit oscillates at a frequency of 20kHz, and this high-frequency oscillation process helps the glue to reach micron-sized dispersion in styrene and acrylonitrile monomers.

[0045] In some embodiments of the present application, the premixing unit includes a multi-stage polymerizer 24, which includes at least two reactors connected in series, and the temperature gradient is controlled to be 110°C to 160°C.

[0046] Specifically, when the raw material is low-cis polybutadiene rubber (PBRD), the multi-stage polymerizer 24 consists of three plug flow reactors (PFRs) connected in series, each with a capacity of 8 m³ and a total effective volume of 24 m³. The inner wall is coated with polytetrafluoroethylene to reduce adhesion of the highly viscous rubber. It is equipped with a jacketed circulating thermal oil system with a temperature control range of 110°C to 150°C. Each reactor stage is equipped with an independent agitator, a combination of anchor and turbine types, with a rotation speed of 10-20 rpm to promote radial mixing of the materials.

[0047] Preferably, when the raw material is a low-cis polybutadiene rubber solution, the temperature of the first-stage polymerizer is 110°C, the pressure is 0.8 MPaG, the residence time is 1.5 h, and the conversion rate is increased to 65%; the temperature of the second-stage polymerizer is 130°C, the pressure is 0.7 MPaG, the residence time is 1.5 h, and the conversion rate is increased to 85%; the temperature of the third-stage polymerizer is 150°C, the pressure is 0.6 MPaG, the residence time is 2 h, and the final conversion rate is ≥99.5%.

[0048] Specifically, when the raw material is solution-polymerized styrene-butadiene rubber (SBR) liquid, a two-stage reactor is used. The first stage is maintained at 130°C to initiate the free radical grafting polymerization of styrene and acrylonitrile onto the SBR molecular chains. The second stage is maintained at 145°C to reinforce the free radical grafting copolymerization of styrene and acrylonitrile onto the SBR molecular chains. The pressure is 0.7 MPaG, and the residence time is 4 to 5 hours. The grafting efficiency of this polymerization reaction is ≥95%, the thickness of the grafted layer on the surface of the SBR particles reaches 15 to 20 nm, and the interfacial adhesion is increased by 40%.

[0049] In some embodiments of the present application, when low-cis polybutadiene rubber solution is used as the raw material, the operating temperature of the devolatilization tower 31 is 120°C~130°C and the pressure is 0.5 MPaG; when solution-polymerized styrene-butadiene rubber solution is used as the raw material, the operating temperature of the devolatilization tower 31 is 160°C and the pressure is 0.4 MPaG.

[0050] Specifically, when using low-cis polybutadiene rubber liquid as the raw material, devolatilization tower 31 is a plate tower with 30 valve trays, operating at a temperature of 120°C to 130°C and a pressure of 0.5 MPaG, capable of separating over 90% of the polymerization system. 15kg to 18kg of liquid are recovered from the polymerization system, with a recovery rate of 88% to 92%. The overhead vapor is liquefied via a tube-and-tube condenser, and the cooling water temperature is maintained at 25°C. Furthermore, a scraper-type agitator is installed in the bottom of the tower to prevent gel deposition.

[0051] Specifically, when low-cis polybutadiene rubber solution is used as raw material, the operating temperature of the devolatilization tower 31 is 160° C. and the pressure is 0.4 MPaG, and more than 90% of cyclohexane can be separated, and a small amount of styrene monomer is contained in the cyclohexane.

[0052] In some embodiments of the present application, the azeotropic distillation tower 32 is provided with a solvent heat circulation loop for preheating the distillation feed with the waste heat of the polymerization reaction.

[0053] Specifically, when the raw material is low-cis polybutadiene rubber (LBBR), the packing of azeotropic distillation tower 32 is ceramic Pall rings with a specific surface area of ​​300 m² / m³, the operating pressure is 0.3 MPaG, the tower top temperature is 105°C to 110°C (the polymerization system-styrene azeotropic temperature), and the reflux ratio is 3:1. Styrene and acrylonitrile monomers are regularly discharged from the bottom of the tower at a frequency of once per day. The residual styrene and acrylonitrile monomers in the recycled polymerization system are ≤50 ppm, meeting the requirements for low-cis polybutadiene rubber synthesis. The solvent is recycled ≥30 times.

[0054] Furthermore, when using low-cis polybutadiene rubber liquid as the raw material, azeotropic distillation tower 32 utilizes the polymerization reaction waste heat (110°C-120°C) to preheat the distillation feed. A finned heat exchanger is also used to improve heat exchange efficiency by 20%. The recovered polymerization system undergoes activated carbon adsorption to remove residual styrene and acrylonitrile monomers, achieving a purity of ≥99.2% for reuse in low-cis polybutadiene rubber polymerization kettle 11.

[0055] Specifically, when the raw material is the solution of styrene-butadiene rubber (SBR), the packing of the azeotropic distillation tower 32 is stainless steel theta rings with a specific surface area of ​​500 m² / m³ and a reflux ratio of 5:1 to ensure optimal separation. The top of the tower is primarily cyclohexane with a purity of up to 99.8%. The heavy components at the bottom of the tower are primarily styrene dimers, which are discharged regularly, with a frequency of ≤1 time / day, to maintain the dynamic balance of the materials in the tower and the stability of the distillation effect. Through the implementation of precision filtration technology, the recovered cyclohexane is filtered to a precision of 5μm. The treated cyclohexane can be directly reused in the SBR polymerization kettle 11, achieving efficient solvent recycling. This method allows the solvent to be recycled more than 50 times, effectively reducing the impact on the environment.

[0056] Furthermore, taking the preparation of ABS using solution-polymerized styrene-butadiene rubber as raw material as an example, the waste heat of the polymerization reaction (140°C~150°C) is used to preheat the distillation feed, which can save energy by 30%; the top condenser uses a plate heat exchanger, which increases the heat exchange efficiency by 25% and the solvent recovery rate from 99% to 99.5%.

[0057] After purification by the three-stage recovery system of the devolatilization tower 31 and the azeotropic distillation tower 32, the solvent reuse rate reaches 99.5%, realizing the zero-emission mode of "recovering and refining solvent-polymerization reaction medium-recycling".

[0058] The invention relates to a method for producing engineering plastics by continuous polymerization of rubber glue, comprising the following steps: synthesizing rubber; subjecting styrene and rubber glue to a polymerization reaction; and recycling the solvent in a closed loop; wherein the rubber glue is one of solution-polymerized styrene-butadiene rubber and low-cis polybutadiene rubber.

[0059] Specifically, the synthesis parameters of the rubber solution include: when preparing the solution of low-cis polybutadiene rubber, the catalyst used is n-butyl lithium, the dosage is 0.5‰~1.0‰, the polymerization temperature is 80±5°C, the pressure is 0.6MPaG, and the reaction time is 4h~5h; when preparing the solution of solution-polymerized styrene-butadiene rubber, the catalyst used is n-butyl lithium, the concentration is 1.5mol / L~2.0mol / L, the dosage is 0.5‰~1.0‰, the synthesis temperature is 50°C~65°C, the pressure is 0.3MPaG~0.5MPaG, and the reaction time is 4h~6h.

[0060] Specifically, the parameters of the polymerization reaction include: when low-cis polybutadiene rubber liquid is used as the raw material, the low-cis polybutadiene rubber liquid accounts for 25%~35% of the total amount of the liquid, styrene accounts for 45%~55% of the total amount of the liquid, acrylonitrile accounts for 10%~15% of the total amount of the liquid, the dispersant accounts for 1%~2% of the total amount of the liquid, and the initiator accounts for 0.05%~0.1% of the total amount of the liquid, the dispersant is sorbitan oleate, and the initiator is di-tert-butyl peroxide; when solution-polymerized styrene-butadiene rubber liquid is used as the raw material, the solution-polymerized styrene-butadiene rubber liquid accounts for 30%~40% of the total amount of the liquid, styrene accounts for 50%~60% of the total amount of the liquid, acrylonitrile accounts for 10%~15% of the total amount of the liquid, and chemical additives account for 0.2%~0.5% of the total amount of the liquid, and the chemical additives include initiators, chain transfer agents, and antioxidants.

[0061] The present invention will be described in detail below through examples.

[0062] Example 1 This embodiment provides a method for producing ABS by continuous polymerization of low-cis polybutadiene rubber solution, which is as follows: The method of this embodiment mainly includes three parts: synthesis of low-cis polybutadiene rubber solution, ABS polymerization reaction and solvent recovery.

[0063] 1. Synthesis of low cis polybutadiene rubber solution 85 kg of butadiene, 0.5 kg of n-butyl lithium, 165 kg of cyclohexane and n-hexane were added into the polymerization reactor 11 as raw materials. The temperature in the reactor was set at 80°C and the pressure was 0.6 MPaG. The reaction was carried out for 4 hours to obtain 250 kg of low-cis polybutadiene rubber solution with a solid content of 34%.

[0064] 2.ABS polymerization 250 kg of low-cis polybutadiene rubber solution, 400 kg of styrene and 120 kg of acrylonitrile were crushed to 40 μm in the first-stage high-speed shear unit of the dynamic mixer 21 and then mixed for 10 minutes in the second-stage static mixing unit to form a stable emulsion.

[0065] The temperature in the first premixing kettle 22 was 65° C. The temperature in the second premixing kettle 23 was 100° C., the pressure was 0.9 MPaG, and the stirring rate was 30 rpm, so that LCBR was graft-copolymerized with styrene and acrylonitrile monomers, and the monomer conversion rate was 25%.

[0066] During the polymerization process, 0.2 kg of di-tert-butyl peroxide and 5 kg of Span (sorbitan oleate) 80 were added. The total residence time in the multi-stage polymerizer 24 was 5 h, the temperature gradient was 110 ° C ~ 130 ° C, the grafting rate was 85%, and the heat taken away by solvent vaporization accounted for 20%.

[0067] 3.Solvent recovery 160 kg of n-hexane and cyclohexane are recovered through the devolatilization tower 31 and the azeotropic distillation tower 32, with a recovery rate of 96.9%, and are reused in the synthesis of low-cis polybutadiene rubber.

[0068] The solvent consumption per unit product in the solvent recovery process is 2kg, and the energy consumption is 0.9kWh / kg.

[0069] The final ABS product has an impact strength of 42kJ / ㎡ at -20℃; a surface gloss of 88%; and a gel impurity content of 0.4%.

[0070] Example 2 This embodiment provides a method for producing HIPS by continuous polymerization of low-cis polybutadiene rubber solution, which is as follows: The method of this embodiment mainly includes three parts: synthesis of low-cis polybutadiene rubber solution, HIPS polymerization reaction and solvent recovery.

[0071] 1. Synthesis of low cis polybutadiene rubber solution 68 kg of butadiene, 132 kg of n-hexane and cyclohexane, and 0.5 kg of n-butyl lithium were added to a polymerization reactor 11. The reactor temperature was set at 80°C and the pressure was 0.6 MPaG. The reaction was allowed to proceed for 4 hours to produce 200 kg of low-cis polybutadiene rubber solution. The resulting solution had a solids content of 34% and contained 68 kg of low-cis polybutadiene rubber and 132 kg of n-hexane and cyclohexane.

[0072] 2.HIPS polymerization 200 kg of low-cis polybutadiene rubber solution and 600 kg of styrene were mixed in a dynamic mixer 21 for 8 min, and the styrene was dissolved in n-hexane and cyclohexane to form a homogeneous solution, wherein the 200 kg of low-cis polybutadiene rubber solution contained 68 kg of low-cis polybutadiene rubber and 132 kg of n-hexane and cyclohexane solvents.

[0073] The outlet temperature of the first premixing kettle 22 was 50°C and the viscosity was 150 mPa·s. The temperature of the second premixing kettle 23 was 120°C and the pressure was 0.7 MPaG. The styrene prepolymerization conversion rate was 30%, forming a low-cis polybutadiene rubber grafted polystyrene core-shell structure.

[0074] During the polymerization process, 0.3 kg of benzoyl peroxide initiator and 0.5 kg of antioxidant were added. The temperature of the multi-stage polymerizer 24 was 150° C., the pressure was 0.5 MPaG, the total residence time was 6 h, and the melt flow rate (MFR) was 8 g / 10 min.

[0075] During the polymerization stage, the heat carried away by vaporization of the polymerization system accounts for 30%.

[0076] 3.Solvent recovery Devolatilization tower 31 operated at a pressure of -0.09 MPaG and a temperature of 200°C, recovering 125 kg of n-hexane and cyclohexane, a recovery rate of 94.7%. The solvent purified in azeotropic distillation tower 32 had a purity of 99.5% and was reused in the synthesis of low-cis polybutadiene rubber.

[0077] The solvent consumption per unit product in the solvent recovery process is 1.5kg, and the energy consumption is 1.1kWh / kg.

[0078] The final HIPS cantilever beam impact strength is 15kJ / m 2 , melt flow rate 8g / 10min, heat deformation temperature 85℃, yellowness index 8.

[0079] Example 3 This embodiment provides a method for producing HIPS by continuous polymerization of solution-polymerized styrene-butadiene rubber solution, which is as follows: The method of this embodiment mainly includes three parts: synthesis of solution-polymerized styrene-butadiene rubber solution, HIPS polymerization reaction and solvent recovery.

[0080] 1. Synthesis of solution-polymerized styrene-butadiene rubber 70 kg of butadiene, 30 kg of styrene, 200 kg of cyclohexane, and 0.35 kg of n-butyl lithium were added to a polymerization reactor 11. The reactor temperature was set at 65°C and the pressure was 0.45 MPaG. The reaction was carried out for 6 hours to produce 300 kg of a solution-polymerized styrene-butadiene rubber solution. The resulting solution had a solids content of 33.3%, contained 100 kg of solution-polymerized styrene-butadiene rubber, and 200 kg of cyclohexane.

[0081] 2.HIPS polymerization 250 kg of solution polymerized styrene butadiene rubber solution and 650 kg of styrene were mixed in a dynamic mixer 21 for 5 min, wherein the 250 kg of solution polymerized styrene butadiene rubber solution contained 83 kg of solution polymerized styrene butadiene and 167 kg of cyclohexane solvent.

[0082] The outlet material of the first premixing kettle 22 has a particle size of 20 μm and a temperature of 55°C. The temperature of the second premixing kettle 23 is 130°C and the pressure is 0.8 MPaG. The boiling point of cyclohexane (80.7°C) is used to control the temperature rise, and the solvent partially vaporizes and removes 40% of the heat.

[0083] During the polymerization reaction, 0.25 kg of di-tert-butyl peroxide and 0.6 kg of antioxidant are added. The temperature of the multi-stage polymerizer 24 is 160° C., the pressure is 0.6 MPaG, the total residence time is 5 h, the grafting rate is 95%, and the heat taken away by cyclohexane vaporization accounts for 50%.

[0084] 3.Solvent recovery After the devolatilization tower 31 and the azeotropic distillation tower 32, 160 kg of cyclohexane is recovered with a recovery rate of 95.8% and a purity of 99.8%, which is reused in the synthesis of solution-polymerized styrene-butadiene rubber.

[0085] The solvent consumption per unit product in the solvent recovery process is 0.8kg, and the energy consumption is 0.75kWh / kg.

[0086] The final HIPS has an Izod impact strength of 18 kJ / m 2 .

[0087] Example 4 This embodiment provides a method for producing ABS by continuous polymerization of a solution-polymerized styrene-butadiene rubber solution, which is as follows: The method of this embodiment mainly includes three parts: synthesis of solution-polymerized styrene-butadiene rubber solution, ABS polymerization reaction and solvent recovery.

[0088] 1. Synthesis of solution-polymerized styrene-butadiene rubber 60 kg of butadiene, 40 kg of styrene, 200 kg of cyclohexane, and 0.3 kg of n-butyl lithium were added to a polymerization reactor at 60°C and 0.4 MPaG. The reaction was allowed to proceed for 5 hours to produce 300 kg of a latex. The latex had a solids content of 33.3% and contained 100 kg of styrene butadiene and 200 kg of cyclohexane.

[0089] 2.ABS polymerization 300 kg of the adhesive, 500 kg of styrene, and 150 kg of acrylonitrile produced in polymerization reactor 11 were mixed in a dynamic mixer 21 for 5 minutes. The adhesive was dispersed through high-speed shearing, static mixing, and ultrasonic vibration. The first stage of high-speed shearing was at a speed of 2000 rpm, the second stage of static mixing achieved uniform phase distribution, and the third stage of ultrasonic vibration had a frequency of 20 kHz. The exiting material had a particle size of 25 μm and a temperature of 55°C.

[0090] The temperature of the first premixing reactor 22 was set at 65°C to 75°C to maintain the cyclohexane in a liquid state, with a pressure of 0.8 MPaG and a stirring rate of 40 rpm to 50 rpm. The temperature of the second premixing reactor 23 was raised to 110°C to 120°C to partially vaporize the cyclohexane, with a vaporization rate of 20% to 30%. The latent heat of vaporization of the solvent was used to absorb the heat of reaction, reducing the need for external cooling. The jacket cooling load was reduced by approximately 60%. During the polymerization reaction, 150 kg of acrylonitrile was added. The total residence time in the multi-stage polymerizer 24 was 4 hours, the grafting rate was 97%, and the heat removed by solvent vaporization accounted for 45%.

[0091] 3.Solvent recovery Devolatilization tower 31 recovers 180 kg of cyclohexane at an operating temperature of 160°C and a pressure of 0.4 MPaG, achieving a recovery rate of 90%. After azeotropic distillation tower 32, 179 kg of pure cyclohexane with a purity of 99.8% is obtained. The recovered cyclohexane is filtered through a 5 μm precision filter and directly reused in the solution-polymerized styrene-butadiene polymerizer.

[0092] The solvent consumption per unit product in the solvent recovery process is 1kg, and the energy consumption is 0.68kWh / kg.

[0093] The final ABS obtained has an impact strength of 52kJ / m at -20℃ 2 , the surface gloss is 93% and the solvent residue is 0.03%.

[0094] Although the present invention is disclosed as above, the present invention is not limited thereto. Any person skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention should be based on the scope defined by the claims.

Claims

1. A device for producing engineering plastics by continuous polymerization of rubber glue, characterized in that: include: A glue liquid direct delivery system, wherein the glue liquid direct delivery system is provided with a polymerization kettle; A premixing unit, comprising a dynamic mixer and a premixing kettle; Solvent recovery system, including devolatilization tower and azeotropic distillation tower; Wherein, the polymerization kettle is directly connected to the premixing unit through an insulated pipe.

2. The device for producing engineering plastics by continuous polymerization of rubber glue according to claim 1, characterized in that: The thickness of the insulation layer of the insulation pipe is 50 mm, and the temperature of the insulation pipe is controlled at 40° C. to 50° C.

3. The device for producing engineering plastics by continuous polymerization of rubber glue according to claim 1, characterized in that: The glue liquid direct delivery system further comprises a glue liquid buffer tank, which is arranged between the polymerization kettle and the premixing unit.

4. The device for producing engineering plastics by continuous polymerization of rubber glue according to claim 1, characterized in that: The premixing kettle comprises: The first premixing kettle, when using a polymerized rubber solution of low-cis polybutadiene rubber as the raw material, the temperature of the first premixing kettle is 60°C to 70°C, the pressure is 0.1 MPaG, and the stirring speed is 30 rpm to 40 rpm; when using a solution polymerized styrene-butadiene rubber solution as the raw material, the temperature of the first premixing kettle is 65°C to 75°C, the pressure is 0.1 MPaG, and the stirring speed is 40 rpm to 50 rpm; The second premixing kettle, when the polymerized rubber liquid of low cis polybutadiene rubber is used as the raw material, the temperature of the second premixing kettle is 100°C~110°C, the pressure is 0.5MPaG, and the stirring rate is 50rpm~60rpm; when the rubber liquid of solution-polymerized styrene-butadiene rubber is used as the raw material, the temperature of the second premixing kettle is 110°C~120°C.

5. The device for producing engineering plastics by continuous polymerization of rubber liquid according to claim 1, characterized in that: The dynamic mixer comprises: The first-stage high-speed shear unit is used to quickly and evenly mix the polymerized adhesive with the polar monomers of styrene and acrylonitrile; The secondary static mixing unit is used to achieve uniform dispersion and mixing of the polymerized adhesive with the polar monomers of styrene and acrylonitrile; The three-stage ultrasonic oscillation unit has an oscillation frequency of 20kHz and is used to promote the micron-level dispersion of the polar monomer acrylonitrile in the glue.

6. The device for producing engineering plastics by continuous polymerization of rubber glue according to claim 1, characterized in that: The premixing unit includes a multi-stage polymerizer, which includes at least two reactors connected in series, and the temperature gradient is controlled to be 110° C. to 160° C.

7. The device for producing engineering plastics by continuous polymerization of rubber liquid according to claim 1, characterized in that: When low-cis polybutadiene rubber solution is used as the raw material, the operating temperature of the devolatilization tower is 120° C. to 130° C. and the pressure is 0.5 MPaG; and / or When solution-polymerized styrene-butadiene rubber solution is used as the raw material, the operating temperature of the devolatilization tower is 160° C. and the pressure is 0.4 MPaG.

8. The device for producing engineering plastics by continuous polymerization of rubber liquid according to claim 1, characterized in that: The azeotropic distillation tower is provided with a solvent heat circulation loop for preheating the distillation feed with the waste heat of the polymerization reaction.

9. A method for producing engineering plastics by continuous polymerization of rubber glue, which is achieved by the apparatus for producing engineering plastics by continuous polymerization of rubber glue as claimed in any one of claims 1 to 8, characterized in that: The method for producing engineering plastics by continuous polymerization of rubber glue comprises the following steps: synthesizing rubber glue; carrying out solvent-free polymerization reaction using the rubber glue as raw material; and recycling the solvent in a closed loop; Wherein, the rubber adhesive is at least one of low-cis polybutadiene rubber adhesive and solution-polymerized styrene-butadiene rubber adhesive.

10. The method for producing engineering plastics by continuous polymerization of rubber liquid according to claim 9, characterized in that: The synthesis parameters of the rubber glue include: When preparing the low-cis polybutadiene rubber solution, n-butyl lithium is used as a catalyst at a concentration of 1.5 mol / L to 2.0 mol / L, an amount of 0.5‰ to 1.0‰, a polymerization temperature of 70°C to 85°C, a pressure of 0.6 MPaG, and a reaction time of 4h to 5h; and / or When preparing the solution-polymerized styrene-butadiene rubber solution, n-butyl lithium is used as a catalyst with a concentration of 1.5 mol / L to 2.0 mol / L, an amount of 0.5‰ to 1.0‰, a synthesis temperature of 50°C to 65°C, a pressure of 0.3 MPaG to 0.5 MPaG, and a reaction time of 4h to 6h.

11. The method for producing engineering plastics by continuous polymerization of rubber liquid according to claim 9, characterized in that: The parameters of the polymerization reaction include: When the low-cis polybutadiene rubber glue is used as the raw material, the low-cis polybutadiene rubber glue accounts for 25% to 35% of the total mass of the glue, styrene accounts for 45% to 55% of the total mass of the glue, acrylonitrile accounts for 10% to 15% of the total mass of the glue, the dispersant accounts for 1% to 2% of the total mass of the glue, and the initiator accounts for 0.05% to 0.1% of the total mass of the glue; the dispersant is sorbitan oleate, and the initiator is di-tert-butyl peroxide; and / or When the solution polymerized styrene-butadiene rubber solution is used as the raw material, the solution polymerized styrene-butadiene rubber solution accounts for 30% to 40% of the total mass of the solution, styrene accounts for 50% to 60% of the total mass of the solution, acrylonitrile accounts for 10% to 15% of the total mass of the solution, and chemical additives account for 0.2% to 0.5% of the total mass of the solution; the chemical additives include initiators, chain transfer agents, and antioxidants.

Citation Information

Patent Citations

  • Industrial-scale high-performance high-impact polystyrene production device and production process

    CN114395067A

  • Continuous production process of CO2-based multipolymer

    CN119570008A

  • High -efficient, high -power diesel oil, marine fuel oil microemulsified device

    CN207025229U

  • Preparation of rubber-modified styrenic resin

    JP2000256430A