A method for preparing helical filament-modified carbon nitride photocatalyst and its application.

Helical filament-modified carbon nitride photocatalysts were prepared by mixing D-aspartic acid and GABA with urea, which solved the problem of insufficient visible light response of carbon nitride photocatalysts in the prior art. This method achieved high efficiency in photodegradation and low energy consumption, with good morphological uniformity.

CN120714685BActive Publication Date: 2025-12-02SHAANXI YANCHANG PETROLEUM GRP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202511221625.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-08-29
Publication Date
2025-12-02
Estimated Expiration
2045-08-29

AI Technical Summary

Technical Problem

Existing carbon nitride photocatalysts have shortcomings in visible light response capabilities. Current modification strategies often focus on optimizing a single performance aspect, and high-temperature calcination consumes a lot of energy and the preparation process is complex.

Method used

A helical filament-modified carbon nitride photocatalyst was prepared by mixing D-aspartic acid and GABA with urea and through the synergistic coordination of intramolecular amino and carboxyl groups. The calcination temperature was reduced to 450-470℃ to form a helical structure and expose more active sites.

Benefits of technology

It improves the visible light utilization rate of the catalyst, has excellent photodegradation performance, good catalytic activity and stability, and the preparation process is energy-saving and environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120714685B_ABST
    Figure CN120714685B_ABST
Patent Text Reader

Abstract

This invention discloses a method for preparing a helical filament modified carbon nitride photocatalyst, comprising the following steps: (1) mixing amino acids and urea, adding water, stirring at 95-100℃ for 1-1.5h, and then drying at 105-110℃ to constant weight to form a copolymer mixture; (2) placing the copolymer mixture in a muffle furnace, heating it at a certain rate to 450-470℃ for calcination for 1-1.5h, naturally cooling it to room temperature, and grinding it. This invention prepares a catalyst with a helical filament structure through the synergistic coordination of amino and carboxyl groups in D-aspartic acid and GABA molecules, as well as the synergistic effect of D-aspartic acid and GABA, which can expose more active sites, has high visible light utilization, can effectively degrade organic matter in water, has excellent photodegradation performance, good catalytic activity, good stability, and low calcination temperature and short time, which has energy-saving advantages. The preparation process is environmentally friendly and simple to operate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of photocatalyst technology, specifically relating to a method for preparing a helical filament modified carbon nitride photocatalyst and its application. Background Technology

[0002] Photocatalytic solar energy conversion technology, as an environmentally friendly advanced oxidation process, has shown significant advantages in achieving water pollution control and renewable energy utilization. This technology utilizes the photoexcitation effect of semiconductor materials to generate photogenerated electrons (electrons) under solar irradiation. - ) and holes (h + This leads to the generation of hydroxyl radicals (·OH) and superoxide radicals (·O2). - Photocatalysts utilize active species such as urea (g-C3N4, CN) to achieve efficient mineralization of pollutants through redox reactions. Among numerous photocatalysts, graphitic carbon nitride (g-C3N4, CN) has become a hot research topic due to its unique graphite-like layered structure, moderate band gap, excellent thermal / chemical stability, and readily available and inexpensive raw materials. In existing technologies, conventional carbon nitride catalysts are obtained by calcining urea at high temperatures, typically above 500℃. Calcination below 500℃ leads to incomplete reactions and affects catalytic performance. Although researchers have developed modification strategies such as morphology control, heterostructure construction, and elemental doping, existing methods often focus on optimizing a single performance characteristic. It is particularly noteworthy that overcoming the visible light response capability of CN materials through simplified preparation processes remains a critical technical bottleneck in this field. Summary of the Invention

[0003] To address the shortcomings of existing technologies, this invention provides a method for preparing helical filament-modified carbon nitride photocatalysts and their applications. By selecting D-aspartic acid and GABA, which have bifunctional groups, and assembling them together with urea, and utilizing the synergistic coordination of the amino and carboxyl groups within the molecules, as well as the synergistic effect of D-aspartic acid and GABA, a helical carbon nitride photocatalyst is prepared in one step. The synthesis temperature is low, energy-saving and environmentally friendly, and the obtained catalyst has good catalytic performance.

[0004] A method for preparing a helical filament-modified carbon nitride photocatalyst includes the following steps:

[0005] (1) Mix amino acids and urea, add water, stir at 95-100℃ for 1-1.5h, and then dry at 105-110℃ to constant weight to form a copolymer mixture;

[0006] (2) Place the copolymer mixture in a muffle furnace, heat it to 450-470℃ and calcine it for 1-1.5 hours, cool it naturally to room temperature, and grind it.

[0007] Preferably, the amino acid is a mixture of D-aspartic acid and GABA.

[0008] Preferably, the ratio of D-aspartic acid to GABA is 3.1-6.2g: 12.6-18.9g.

[0009] Preferably, the ratio of amino acids, urea, and water is 15.7-25.1g: 40-60g: 100-120mL.

[0010] Preferably, the heating rate in step (2) is 6-10℃ / min.

[0011] The application of a spiral filament modified carbon nitride photocatalyst in the photodegradation of organic matter in water, wherein the catalyst is prepared by the preparation method described above in this invention.

[0012] Advantages of this invention:

[0013] (1) This invention prepares a catalyst with a helical filament structure by means of the synergistic coordination of the amino and carboxyl groups in the molecules of D-aspartic acid and GABA, as well as the synergistic effect of D-aspartic acid and GABA. This catalyst can expose more active sites, has high visible light utilization, can degrade organic matter in water, has excellent photodegradation performance, good catalytic activity, and good stability.

[0014] (2) The present invention has low calcination temperature and short time, which has the advantage of energy saving, and the preparation process is environmentally friendly, simple and easy to operate. Attached Figure Description

[0015] Figure 1 Here is a scanning electron microscope image of the catalyst from Example 1;

[0016] Figure 2 Here is a scanning electron microscope image of the catalyst in Example 2;

[0017] Figure 3 Here is a scanning electron microscope image of the catalyst in Example 3;

[0018] Figure 4 The image shows a scanning electron microscope (SEM) image of the catalyst in Comparative Example 1.

[0019] Figure 5 The image shows a scanning electron microscope (SEM) image of the catalyst in Comparative Example 2.

[0020] Figure 6 The image shows a scanning electron microscope (SEM) image of the catalyst in Comparative Example 3.

[0021] Figure 7 The image shows a scanning electron microscope (SEM) image of the catalyst in Comparative Example 4.

[0022] Figure 8 The infrared spectrum of the catalyst in Example 1;

[0023] Figure 9 The infrared spectrum of the carbon nitride photocatalyst in Comparative Example 1 is shown.

[0024] Figure 10 The UV-Vis diffuse reflectance spectrum of the catalyst in Example 1 is shown below.

[0025] Figure 11 The UV-Vis diffuse reflectance spectrum of the carbon nitride photocatalyst in Comparative Example 1 is shown.

[0026] Figure 12 These are the results of the photocatalytic degradation experiment. Detailed Implementation

[0027] Example 1

[0028] A method for preparing a helical filament-modified carbon nitride photocatalyst includes the following steps:

[0029] (1) Mix 3.1 g of D-aspartic acid, 12.6 g of aminobutyric acid and 60 g of urea in a crucible, add 100 mL of water, stir at 100 °C for 1 h, and then dry at 105 °C to constant weight to form a copolymer mixture;

[0030] (2) The above crucible was covered and placed in a muffle furnace, heated to 450°C for 1 hour at a heating rate of 6 °C / min, cooled naturally to room temperature, and ground into powder to obtain a spiral filament modified carbon nitride photocatalyst, denoted as CN-C.

[0031] Example 2

[0032] A method for preparing a helical filament-modified carbon nitride photocatalyst includes the following steps:

[0033] (1) Mix 6.2 g of D-aspartic acid, 18.9 g of aminobutyric acid and 60 g of urea in a crucible, add 120 mL of water, stir at 95 °C for 1.5 h, and then dry at 110 °C to constant weight to form a copolymer mixture;

[0034] (2) The above crucible was covered and placed in a muffle furnace, heated to 450°C at a heating rate of 8°C / min for 1.5h, cooled naturally to room temperature, and ground into powder to obtain spiral filament modified carbon nitride photocatalyst.

[0035] Example 3

[0036] A method for preparing a helical filament-modified carbon nitride photocatalyst includes the following steps:

[0037] (1) Mix 6.2 g of D-aspartic acid, 12.6 g of aminobutyric acid and 40 g of urea in a crucible, add 100 mL of water, stir at 95 °C for 1.5 h, and then dry at 105 °C to constant weight to form a copolymer mixture;

[0038] (2) The above crucible was covered and placed in a muffle furnace, heated to 470°C for 1 hour at a heating rate of 10 °C / min, cooled naturally to room temperature, and ground into powder to obtain a spiral filament modified carbon nitride photocatalyst.

[0039] Comparative Example 1

[0040] A carbon nitride photocatalyst, prepared by the following method:

[0041] 20 g of urea was placed in a crucible, covered, and placed in a muffle furnace. The crucible was heated to 450 °C at a heating rate of 6 °C / min and held for 4 h. After cooling to room temperature, the product was ground into powder to obtain the carbon nitride photocatalyst.

[0042] Comparative Example 2

[0043] The preparation method of conventional carbon nitride photocatalysts is as follows:

[0044] 20 g of urea was placed in a crucible, covered, and placed in a muffle furnace. The crucible was heated to 550 °C at a heating rate of 6 °C / min and held for 4 h. After cooling to room temperature, the product was ground into powder to obtain a conventional carbon nitride photocatalyst, denoted as CN-M.

[0045] Comparative Example 3

[0046] D-aspartic acid was not added; otherwise, it was the same as in Example 1.

[0047] (1) Mix 12.6 g of aminobutyric acid and 60 g of urea in a crucible, add 100 mL of water, stir at 100 °C for 1 h, and then dry at 105 °C to constant weight to form a copolymer mixture;

[0048] (2) The above crucible was covered and placed in a muffle furnace, heated to 450°C for 1 hour at a heating rate of 6 °C / min, cooled naturally to room temperature, and ground into powder to obtain a spiral filament modified carbon nitride photocatalyst, denoted as CN-A.

[0049] Comparative Example 4

[0050] No GABA was added; otherwise, it was the same as in Example 1.

[0051] (1) Mix 3.1 g of D-aspartic acid and 60 g of urea in a crucible, add 100 mL of water, stir at 100 °C for 1 h, and then dry at 105 °C to constant weight to form a copolymer mixture;

[0052] (2) The above crucible was covered and placed in a muffle furnace, heated to 450°C for 1 hour at a heating rate of 6 °C / min, cooled naturally to room temperature, and ground into powder to obtain a spiral filament modified carbon nitride photocatalyst, denoted as CN-T.

[0053] I. Scanning Electron Microscopy

[0054] The catalysts obtained in Examples 1-3 and Comparative Examples 1-4 were examined by scanning electron microscopy, and the results are shown in the figures below. Figure 1-7 .

[0055] Depend on Figure 1-3 It can be seen that the catalyst prepared by the present invention is mainly composed of helical and filamentous structures, with uniform morphology and good dispersibility;

[0056] Depend on Figure 4 It can be seen that when only urea was used to prepare the catalyst in Comparative Example 1 and the calcination temperature was less than 500℃, the catalyst obtained was irregularly shaped and varied in size. It is speculated that the low reaction temperature led to a decrease in the degree of thermal polymerization.

[0057] Depend on Figure 5 It can be seen that the carbon nitride catalyst prepared by conventional methods has an irregular blocky morphology, and the particle size is relatively large and the morphology varies.

[0058] Depend on Figure 6 It can be seen that the carbon nitride photocatalyst without D-aspartic acid prepared in Comparative Example 3 of the present invention is mainly composed of irregular sheet-like and blocky structures with different morphologies and poor dispersibility, which is significantly different from the morphology of Example 1.

[0059] Depend on Figure 7 It can be seen that the carbon nitride photocatalyst without aminobutyric acid prepared in Comparative Example 4 of the present invention is mainly composed of long and thin filamentous structures, which is significantly different from the morphology of Example 1.

[0060] II. Infrared Spectroscopy Detection

[0061] The infrared spectral detection results of Example 1 are shown below. Figure 8 The infrared spectral detection results of the carbon nitride photocatalyst in Comparative Example 2 are shown in [reference needed]. Figure 9 ;

[0062] Depend on Figure 8 It can be seen that the wavenumber in the infrared spectrum of this catalyst is between 3000 and 3500 cm⁻¹. -1 The broad peak at that point corresponds to the stretching vibration modes of -NH and -OH, with wavenumbers ranging from 1200 to 1650 cm⁻¹.-1 The broad peak at 800 cm⁻¹ corresponds to the heptaazine structure, with a wavenumber of 800 cm⁻¹. -1 The characteristic peak at that location corresponds to the triazine unit structure.

[0063] Depend on Figure 9 It can be seen that the wavenumber in the infrared spectrum of this catalyst is between 3000 and 3500 cm⁻¹. -1 The broad peak at that point corresponds to the stretching vibration modes of -NH and -OH, with wavenumbers ranging from 1200 to 1650 cm⁻¹. -1 The broad peak at 800 cm⁻¹ corresponds to the heptaazine structure, with a wavenumber of 800 cm⁻¹. -1 The characteristic peak at 1540-1600 cm⁻¹ corresponds to the triazine unit structure. -1 The relatively broad absorption peak is presumably due to incomplete conversion of -NH3, resulting in stretching vibrations of NH bonds corresponding to different amino group types, thus leading to the presence of multiple peaks.

[0064] III. Ultraviolet-Vis Diffuse Reflectance Spectroscopy Detection

[0065] The UV-Vis diffuse reflectance spectra of the helical filament-modified carbon nitride photocatalyst prepared in Example 1 and the carbon nitride photocatalyst in Comparative Example 2 are shown below. Figure 10 and Figure 11 .Depend on Figure 10-11 It can be seen that the catalyst of Example 1 exhibits a significant redshift, with a maximum value of 1.1 au in the wavelength range of 200-400 nm and a maximum value of 0.2 au in the wavelength range of 500-600 nm. The catalyst of Comparative Example 2 has a maximum value of only 0.8 au in the wavelength range of 200-400 nm and a maximum value of less than 0.1 au in the wavelength range of 500-600 nm, and its light absorption capacity is significantly worse than that of Example 1.

[0066] IV. Photocatalytic performance testing

[0067] The catalysts from Examples 1 and Comparative Examples 1-4 were added to a 20 mg / L methyl orange solution at a dosage of 0.2 g / L. Their photocatalytic degradation performance was tested using a 1000 W xenon lamp as the light source. (See attached figures.) Figure 12 Therefore, it can be seen that the catalyst provided by the present invention has good catalytic degradation performance, with a degradation rate of up to 92% at 48 min. The degradation rate of the catalyst in Comparative Example 1 is 41%, while the degradation rate of the conventional carbon nitride photocatalyst in Comparative Example 2 is only 47%, the degradation rate of the photocatalyst in Comparative Example 3 is only 71%, and the degradation rate of the photocatalyst in Comparative Example 4 is only 62%.

Claims

1. A method for preparing a helical filament-modified carbon nitride photocatalyst, characterized in that: Includes the following steps: (1) Mix amino acids and urea, add water, stir at 95-100℃ for 1-1.5h, and then dry at 105-110℃ to constant weight to form a copolymer mixture; (2) Place the copolymer mixture in a muffle furnace, heat it to 450-470℃ and calcine it for 1-1.5 hours, then let it cool naturally to room temperature and grind it. The amino acid is a mixture of D-aspartic acid and GABA.

2. The method for preparing the helical filament modified carbon nitride photocatalyst according to claim 1, characterized in that: The ratio of D-aspartic acid to GABA is 3.1-6.2g: 12.6-18.9g.

3. The method for preparing the helical filament modified carbon nitride photocatalyst according to claim 2, characterized in that: The ratio of amino acids, urea, and water is 15.7-25.1g: 40-60g: 100-120mL.

4. The method for preparing the helical filament modified carbon nitride photocatalyst according to claim 1, characterized in that: The heating rate in step (2) is 6-10℃ / min.

5. The application of a spiral filament-modified carbon nitride photocatalyst in the photodegradation of organic matter in water, characterized in that: The catalyst is prepared by the preparation method described in any one of claims 1-4.

Citation Information

Patent Citations

  • Preparation method for red carbon nitride photocatalyst with wide spectral response

    CN109772414A

  • Carbon nitride loaded modified palladium-based formic acid hydrogen production catalyst and preparation method and application thereof

    CN118616075A