A defluoridating agent for mine water, its preparation method and application
By combining aluminum-calcium-magnesium-iron-based quaternary metal materials with chelating agents, hydroxycarboxylic acid compounds, and dispersants, a long-chain porous structure mine water defluoridator is formed, which solves the problem of low defluoridation efficiency in the treatment of high-fluoride mine water and achieves efficient and economical fluoride ion removal.
Patent Information
- Application Number
- CN202511027208.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-07-24
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2045-07-24
AI Technical Summary
Existing technologies for treating high-fluoride mine water suffer from problems such as low defluorination efficiency, poor stability, large reagent dosage, and high operating costs, making it difficult to achieve efficient fluoride ion removal.
Using aluminum-calcium-magnesium-iron-based quaternary metal materials, combined with chelating agents, hydroxycarboxylic acid compounds and dispersants, a long-chain porous structure is formed through a combination of structural coordination, loading flocculation and adsorption technologies. This increases the specific surface area and pore volume, enabling rapid coordination, strong adsorption, precise chelation, flocculation and sedimentation, and thus preparing a defluoridating agent for mine water.
It significantly improves the fluoride ion removal rate and efficiency, reduces sludge volume, and has an economical and efficient fluoride removal effect. It is suitable for the treatment of fluoride-containing mine water in the range of 1-10 mg/L, and solves the shortcomings of traditional fluoride removal technologies.
Smart Images

Figure CN120794124B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of wastewater treatment technology, specifically relating to a defluoridating agent for mine water, its preparation method, and its application. Background Technology
[0002] Coal resource development primarily relies on underground mine development, inevitably generating large quantities of mine water during the process. my country produces approximately 6.9 billion tons of mine water annually, but the average utilization rate is only 35%. Fluoride-containing mine water is a special type of polluted mine water, with fluoride ion concentrations exceeding 10 mg / L in some coal mines, becoming a significant factor restricting the efficient utilization of mine water. Direct discharge of such high-fluoride mine water without proper treatment could cause severe fluoride ion contamination in surrounding groundwater, posing a serious threat to human health. Therefore, developing advanced defluorination technologies for high-fluoride mine water to improve its utilization rate is of great practical significance.
[0003] Currently, defluoridation technologies for fluoride-containing mine water mainly include coagulation and sedimentation, adsorption, ion exchange, and membrane treatment. In practice, most defluoridation technologies are inefficient, uneconomical, and fail to meet emission standards. This is primarily due to the unique chemical properties of fluoride (fluoride ions are difficult to oxidize, precipitate, and crystallize), which makes deep purification challenging. Furthermore, high-fluoride mine water may contain other types of pollutants, and single treatment methods often fail to achieve ideal results, necessitating the research of more efficient combined treatment processes. Polyaluminum chloride (PAC) is commonly used as a defluoridation coagulant. However, in practical engineering applications, it suffers from low defluoridation efficiency, poor stability, high dosage requirements, and high operating costs. Summary of the Invention
[0004] The purpose of this invention is to provide a defluoridating agent for mine water, its preparation method, and its application, so as to solve the problem of low defluoridation efficiency of defluoridating agents.
[0005] The objective of this invention can be achieved through the following technical solutions:
[0006] The first aspect of this invention provides a method for preparing a defluoridating agent for mine water, comprising the following steps:
[0007] Aluminum salts, calcium salts, magnesium salts, and iron salts are added to water and stirred. Then, chelating agents, hydroxycarboxylic acid compounds, and dispersants are added, and the mixture is heated, stirred, and dispersed while maintaining the temperature. The molar ratio of the aluminum salts, calcium salts, magnesium salts, and iron salts is 1:(0.16~0.62):(0.09~0.36):(0.03~0.23).
[0008] In practical defluorination processes, efficiency and economy must be comprehensively considered based on different environments and defluorination requirements. Therefore, a more optimized and efficient defluorination technology is still needed for deep defluorination. This invention combines structural coordination, loading flocculation, and adsorption technologies to design an integrated enhanced flocculation defluorination technology that integrates coordination, flocculation, and sedimentation, offering good economic benefits and application prospects. The enhanced flocculation defluorination technology utilizes the dense, highly active groups on the surface of quaternary metal materials to form strong interactions with fluoride ions. Through chelation, the quaternary metals are assembled into a long-chain porous structure, further increasing the specific surface area and pore volume. This facilitates increased contact area with fluoride ions in mine water. The porous structure adsorbs and complexes the groups, achieving rapid coordination, strong adsorption, precise chelation, flocculation sedimentation, and efficient removal of fluoride from mine water. This achieves highly efficient and selective removal of fluoride ions from fluoride-containing mine water, overcoming the bottlenecks of low efficiency and high cost in traditional deep purification technologies.
[0009] In some possible implementations, heating, stirring, and dispersion are combined with heat preservation: heating to 40–60°C, stirring for 5–10 minutes, and then maintaining the temperature for 1–2 hours.
[0010] In some possible implementations, the mass ratio of chelating agent, hydroxycarboxylic acid compound, and dispersant is 2:2:1.
[0011] In some possible implementations, the mass ratio of aluminum salt, calcium salt, magnesium salt, iron salt, chelating agent, hydroxycarboxylic acid compound, and dispersant is 10:2:1:1.
[0012] In some possible implementations, the mass ratio of aluminum salt, calcium salt, magnesium salt, iron salt, chelating agent, hydroxycarboxylic acid compound and dispersant is 10:2:1:1:0.2:0.2:0.1.
[0013] In some possible implementations, the aluminum salt is at least one of aluminum chloride, aluminum sulfate, and aluminum nitrate;
[0014] The calcium salt is at least one of calcium chloride, calcium nitrate, calcium bicarbonate, and calcium acetate;
[0015] The magnesium salt is at least one of magnesium chloride, magnesium sulfate, magnesium nitrate, and magnesium acetate;
[0016] The iron salt is at least one of ferric chloride, ferric sulfate, ferrous sulfate, ferric ammonium sulfate, and ferric nitrate.
[0017] In some possible implementations, the chelating agent is at least one of sodium tripolyphosphate, sodium EDTA, aminotriacetic acid, and hydroxyethylidene diphosphonic acid;
[0018] In some possible implementations, the hydroxycarboxylic acid compound is at least one of α-hydroxyacetic acid, salicylic acid, citric acid, and lactobionic acid.
[0019] In some possible implementations, the dispersant is at least one selected from ethanol, propanol, polyethylene glycol, sodium silicate, polymethacrylic acid, polyethyleneimine, and sodium dodecyl sulfate.
[0020] A second aspect of the present invention provides a mine water defluoridating agent, which is prepared by the above method.
[0021] A third aspect of the present invention provides the application of the above-mentioned mine water defluoridating agent in mine water defluoridation agents.
[0022] The application of the above-mentioned mine water defluoridating agent in mine water defluoridation includes the following steps:
[0023] The defluorinating agent is added to the fluoride-containing mine water, and after stirring and mixing, a colloidal state is formed. Then, a flocculant is added to make the colloidal substance form flocs. The flocs are allowed to settle and settle to obtain the defluorinated clear liquid.
[0024] In some possible implementations, the fluoride ion concentration in the defluorinated solution is <1 mg / L.
[0025] In some possible implementations, the flocculant is a polyacrylamide flocculant, the fluoride ion concentration in the fluoride-containing mine water is 1–10 mg / L; the dosage of the defluorinating agent is 0.05–0.1 wt%; the stirring speed is 200–300 rpm; the concentration of the polyacrylamide flocculant solution is 0.1 wt%, and the dosage is 0.1–0.2 wt%.
[0026] The beneficial effects of this invention are:
[0027] This invention breaks free from the constraints of traditional calcium salts. By introducing key chelating agents, hydroxycarboxylic acid compounds, and dispersants based on controlled material formulation and synthesis reaction process, it utilizes the excellent fluoride ion adsorption and flocculation sedimentation properties of aluminum-calcium-magnesium-iron-based quaternary metal materials. Under certain temperature conditions, the quaternary metals are assembled into a long-chain porous structure through chelation, further increasing the specific surface area and pore volume. This is beneficial for increasing the contact area with fluoride ions in mine water. The porous structure adsorption complexing groups achieve the purpose of rapid coordination, strong adsorption, precise chelation, flocculation sedimentation, and efficient removal of fluoride from mine water.
[0028] This invention utilizes hydroxycarboxylic acid compounds to create abundant active groups such as hydroxyl and carboxyl groups on the surface of the modified defluorinating agent. These active groups can chemically adsorb fluoride ions, thereby enhancing the defluorination capacity. Furthermore, the hydroxycarboxylic acid compound can form long-chain polyhydroxycarboxylic acids and porous adsorption complexes through its own multiple components and synergistic effects with chelating agents, further improving the fluoride ion removal rate and efficiency. This results in thorough removal, low sludge production, cost-effectiveness, high efficiency, and stable compliance with standards. Simultaneously, the long-chain polyhydroxycarboxylic acid has good compatibility with organic matter; even in wastewater containing organic matter, the defluorinating agent can effectively interact with fluoride ions, thus avoiding the negative impact of organic matter on defluorination efficiency, and has broad application prospects.
[0029] The mine water defluoridator prepared by this invention, exhibiting a synergistic effect of coordination, adsorption, chelation, and flocculation, not only significantly improves the removal rate and efficiency of fluoride ions from fluoride-containing mine water but also disrupts stable dispersion systems in the mine water to achieve flocculation, resulting in excellent settling properties. This defluoridation technology demonstrates good and efficient defluoridation effects for fluoride-containing mine water in the range of 1–10 mg / L, overcoming the shortcomings of existing defluoridation technologies such as low efficiency, poor stability, large reagent dosage, and high operating costs. Attached Figure Description
[0030] The invention will now be further described with reference to the accompanying drawings.
[0031] Figure 1 Here is a SEM image of the defluorinating agent prepared in Example 1 of this invention;
[0032] Figure 2 This is a nitrogen adsorption-desorption curve of the defluorinating agent prepared in Example 1 of the present invention;
[0033] Figure 3 This is the result of treating fluoride-containing mine water (fluoride concentration: 3 mg / L) with the dosage of the defluorinating agent (prepared in Example 1) in Application Example 1 of this invention;
[0034] Figure 4 This is the result of treating fluoride-containing mine water (fluoride concentration: 5 mg / L) with the dosage of the defluorinating agent (prepared in Example 1) in Application Example 2 of the present invention;
[0035] Figure 5 This is the result of treating fluoride-containing mine water (fluoride concentration: 10 mg / L) with the dosage of the defluorinating agent (prepared in Example 1) in Application Example 3 of the present invention. Detailed Implementation
[0036] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.
[0037] The following is a detailed description of a mine water defluoridator, its preparation method, and its application, based on embodiments of this application.
[0038] The following is a detailed description with reference to specific examples.
[0039] Example 1
[0040] This embodiment provides a method for preparing a defluoridating agent for mine water, comprising the following steps:
[0041] Add 200g aluminum chloride, 40g calcium chloride, 20g magnesium chloride, and 20g ferric chloride to 710mL of deionized water, stir at 200rpm for 5min, then add 4g disodium ethylenediaminetetraacetate, 4g α-hydroxyacetic acid, and 2g ethanol, and continue stirring at 60℃ for 10min. After dissolution, keep warm for 1h, and cool to obtain the defluorinating agent.
[0042] The morphology of the defluorinating agent prepared in Example 1 was characterized by scanning electron microscopy (SEM image), as shown below. Figure 1 As shown, the prepared defluorinating agent is a porous structure assembled from nanosheets (characterized by evaporation and drying of the liquid). The specific surface area of the defluorinating agent is characterized by nitrogen adsorption-desorption curves, such as... Figure 2 As shown, the specific surface area of the prepared defluorinating agent is 168.1432 m². 2 / g.
[0043] Application Example 1
[0044] The defluorinating agent with synergistic effects of coordination, adsorption, chelation and flocculation prepared in Example 1 was added to 1L of fluoride-containing mine water with a fluoride ion concentration of 3mg / L at a dosage of 0.05% to 0.01%. After stirring and mixing at 200rpm for 5min, a colloidal state was formed. Then, 1mL of polyacrylamide solution was added and stirred for 3min to form flocs. After standing and settling for 5min, the defluorinated clear liquid was obtained.
[0045] The results of the treatment of fluoride-containing mine water are as follows: Figure 3 As shown, when the fluoride ion concentration in fluoride-containing mine water is 3 mg / L, the fluoride ion concentration in the effluent gradually decreases as the dosage of defluorinating agent increases; when the dosage is 0.05%, the fluoride ion concentration in the effluent can be reduced to below 1 mg / L.
[0046] Application Example 2
[0047] The defluorinating agent with synergistic effects of coordination, adsorption, chelation and flocculation prepared in Example 1 was added to 1L of fluoride-containing mine water with a fluoride ion concentration of 5mg / L at a dosage of 0.05% to 0.01%. After stirring and mixing at 200rpm for 5min, 1mL of polyacrylamide solution was added, and stirring was continued until homogeneous. The mixture was then allowed to settle for 5min to obtain the defluorinated clear liquid.
[0048] The results of the treatment of fluoride-containing mine water are as follows: Figure 4 As shown, when the fluoride ion concentration in fluoride-containing mine water is 5 mg / L, the fluoride ion concentration in the effluent gradually decreases as the dosage of defluorinating agent increases; when the dosage is 0.06%, the fluoride ion concentration in the effluent can be reduced to below 1 mg / L.
[0049] Application Example 3
[0050] The defluorinating agent with synergistic effects of coordination, adsorption, chelation and flocculation prepared in Example 1 was added to 1L of fluoride-containing mine water with a fluoride ion concentration of 10mg / L at a dosage of 0.05% to 0.01%. After stirring and mixing at 200rpm for 5min, 1mL of polyacrylamide solution was added, and stirring was continued until homogeneous. The mixture was then allowed to settle for 5min to obtain the defluorinated clear liquid.
[0051] The results of the treatment of fluoride-containing mine water are as follows: Figure 5 As shown, when the fluoride ion concentration in fluoride-containing mine water is 10 mg / L, the fluoride ion concentration in the effluent gradually decreases as the dosage of defluorinating agent increases; when the dosage is 0.08%, the fluoride ion concentration in the effluent can be reduced to below 1 mg / L.
[0052] Example 2
[0053] This embodiment provides a method for preparing a mine water defluoridator with synergistic effects of coordination, adsorption, chelation, and flocculation, comprising the following steps: adding 200g aluminum sulfate, 40g calcium nitrate, 20g magnesium sulfate, and 20g ferric sulfate to 710mL of deionized water, stirring at 200rpm for 10min, then adding 4g sodium tripolyphosphate, 4g α-hydroxyacetic acid, and 2g polyethylene glycol, and continuing to stir for 5min under heating at 60℃, stirring, and keeping warm for 1h after dissolution, and then cooling to obtain a liquid defluoridator with synergistic effects of coordination, adsorption, chelation, and flocculation.
[0054] The defluoridating agent prepared in Example 2, exhibiting synergistic effects of coordination, adsorption, chelation, and flocculation, was used in defluoridation tests on fluoride-containing mine water with different fluoride ion concentrations, following the methods described in Application Examples 1 to 3. When the fluoride ion concentration in the fluoride-containing mine water was 3, 5, and 10 mg / L, the fluoride agent dosage of 0.05%, 0.06%, and 0.08% reduced the fluoride ion concentration in the effluent to below 1 mg / L.
[0055] Example 3
[0056] This embodiment provides a method for preparing a mine water defluoridator with synergistic effects of coordination, adsorption, chelation, and flocculation, comprising the following steps: adding 200g aluminum nitrate, 40g calcium nitrate, 20g magnesium nitrate, and 20g ferric nitrate to 710mL of deionized water, stirring at 200rpm for 10min, then adding 4g nitric acid, 4g salicylic acid, and 2g sodium silicate, and continuing to stir for 5min under heating at 40℃, dissolving, keeping warm for 2h, and cooling to obtain a mine water defluoridator with synergistic effects of coordination, adsorption, chelation, and flocculation.
[0057] The defluoridating agent prepared in Example 3, which exhibits synergistic effects of coordination, adsorption, chelation, and flocculation, was used to conduct defluoridation tests on fluoride-containing mine water with different fluoride ion concentrations, following the methods described in Application Examples 1 to 3. When the fluoride ion concentration in the fluoride-containing mine water was 3, 5, and 10 mg / L, the fluoride ion concentration in the effluent could be reduced to below 1 mg / L when the dosage of the defluoridating agent was 0.05%, 0.06%, and 0.08%, respectively.
[0058] Example 4
[0059] This embodiment provides a method for preparing a mine water defluoridator with synergistic effects of coordination, adsorption, chelation, and flocculation, comprising the following steps: adding 200g aluminum chloride, 40g calcium chloride, 20g magnesium chloride, and 20g ferric chloride to 710mL of deionized water, stirring at 200rpm for 10min, then adding 4g nitric acid, 4g salicylic acid, and 2g polymethyl methacrylate, and continuing to stir at 40℃ for 10min, dissolving and keeping warm for 2h, and cooling to obtain a mine water defluoridator with synergistic effects of coordination, adsorption, chelation, and flocculation.
[0060] The defluoridating agent prepared in Example 4, exhibiting synergistic effects of coordination, adsorption, chelation, and flocculation, was used in defluoridation tests on fluoride-containing mine water with different fluoride ion concentrations, following the methods described in Application Examples 1 to 3. When the fluoride ion concentration in the fluoride-containing mine water was 3, 5, and 10 mg / L, the fluoride agent dosage of 0.05%, 0.06%, and 0.08% reduced the fluoride ion concentration in the effluent to below 1 mg / L.
[0061] Example 5
[0062] This embodiment provides a method for preparing a mine water defluoridator with synergistic effects of coordination, adsorption, chelation, and flocculation, comprising the following steps: adding 200g aluminum chloride, 40g calcium acetate, 20g magnesium acetate, and 20g ferrous sulfate to 710mL of deionized water, stirring at 200rpm for 10min, then adding 4g hydroxyethylidene diphosphonic acid, 4g citric acid, and 2g polyethyleneimine, and continuing to stir at 60℃ for 5min, dissolving and keeping warm for 1h, and cooling to obtain a mine water defluoridator with synergistic effects of coordination, adsorption, chelation, and flocculation.
[0063] The defluoridating agent prepared in Example 5, which exhibits synergistic effects of coordination, adsorption, chelation, and flocculation, was used to conduct defluoridation tests on fluoride-containing mine water with different fluoride ion concentrations, following the methods described in Application Examples 1 to 3. When the fluoride ion concentration in the fluoride-containing mine water was 3, 5, and 10 mg / L, the fluoride ion concentration in the effluent could be reduced to below 1 mg / L when the dosage of the defluoridating agent was 0.05%, 0.06%, and 0.08%, respectively.
[0064] Example 6
[0065] This embodiment provides a method for preparing a mine water defluoridator with synergistic effects of coordination, adsorption, chelation, and flocculation, comprising the following steps: adding 200g aluminum chloride, 40g calcium bicarbonate, 20g magnesium acetate, and 20g ferric ammonium sulfate to 710mL of deionized water, stirring at 200rpm for 5min, then adding 4g nitric acid, 4g salicylic acid, and 2g sodium dodecyl sulfate, and continuing to stir for 5min under heating at 60℃, dissolving, keeping warm for 1h, and cooling to obtain a mine water defluoridator with synergistic effects of coordination, adsorption, chelation, and flocculation.
[0066] The defluoridating agent with synergistic coordination-adsorption-chelation-flocculation effects prepared in Example 6 was used to conduct defluoridation tests on fluoride-containing mine water with different fluoride ion concentrations, following the methods described in Application Examples 1 to 3. When the fluoride ion concentration in the fluoride-containing mine water was 3, 5, and 10 mg / L, the fluoride agent dosage of 0.05%, 0.06%, and 0.08% reduced the fluoride ion concentration in the effluent to below 1 mg / L.
[0067] Comparative Example 1:
[0068] This comparative example provides a method for preparing a defluoridating agent for mine water, comprising the following steps: adding 160g aluminum chloride, 40g calcium chloride, 40g magnesium chloride, and 40g ferric chloride to 710mL of deionized water, stirring at 200rpm for 5min, then adding 4g disodium ethylenediaminetetraacetate, 4g α-hydroxyacetic acid, and 2g ethanol, continuing to stir under heating at 40℃ for 5min, keeping warm for 1h, and obtaining the defluoridating agent after cooling.
[0069] The defluoridating agent prepared in Comparative Example 1 was used to conduct defluoridation tests on fluoride-containing mine water with different fluoride ion concentrations, following the methods described in Application Examples 1 to 3. The results showed that when the mass ratio of aluminum salts, calcium salts, magnesium salts, iron salts, chelating agents, hydroxycarboxylic acid compounds, and dispersants was not within the range of 10:2:1:1:0.2:0.2:0.1, the defluoridation efficiency of the material decreased significantly. When the fluoride ion concentration in the fluoride-containing mine water was 3, 5, and 10 mg / L, and the dosage of the defluoridating agent was 0.05%, 0.06%, and 0.08%, respectively, the effluent fluoride ion concentrations were 2.6 mg / L, 3.7 mg / L, and 7.9 mg / L, respectively, all failing to reduce to below 1 mg / L.
[0070] Comparative Example 2:
[0071] This comparative example provides a method for preparing a defluoridating agent for mine water, comprising the following steps: adding 200g aluminum chloride, 40g calcium chloride, 20g magnesium chloride, and 20g ferric chloride to 714mL of deionized water, stirring at 200rpm for 5min, then adding 4g disodium ethylenediaminetetraacetate and 2g ethanol, continuing to stir under heating at 40℃ for 5min, keeping warm for 1h, and obtaining the defluoridating agent after cooling.
[0072] The defluoridating agent prepared in Comparative Example 2 was used to conduct defluoridation tests on fluoride-containing mine water with different fluoride ion concentrations, following the methods described in Application Examples 1 to 3. The results showed that without a chelating agent, the material could not form a long-chain porous structure, and the specific surface area of the defluoridating agent decreased to 75.7382 μm. 2 / g. The defluoridation efficiency also decreased significantly. When the fluoride ion concentration in the fluoride-containing mine water was 3, 5, and 10 mg / L, and the dosage of defluoridating agent was 0.05%, 0.06%, and 0.08%, the effluent ion concentration was 1.6 mg / L, 2.9 mg / L, and 6.8 mg / L, respectively, none of which could be reduced to below 1 mg / L.
[0073] Comparative Example 3:
[0074] This comparative example provides a method for preparing a defluoridating agent for mine water, comprising the following steps: adding 200g aluminum chloride, 40g calcium chloride, 20g magnesium chloride, and 20g ferric chloride to 714mL of deionized water, stirring at 200rpm for 5min, then adding 4g disodium ethylenediaminetetraacetate and 2g ethanol, and continuing to stir at 60℃ for 10min, dissolving and keeping warm for 1h, and then cooling to obtain the defluoridating agent.
[0075] The defluoridating agent prepared in Comparative Example 3 was used to conduct defluoridation tests on fluoride-containing mine water with different fluoride ion concentrations, following the methods described in Application Examples 1 to 3. The results showed that without the addition of hydroxycarboxylic acid compounds, the number of active groups on the material surface was significantly reduced, and the defluoridation efficiency also decreased markedly. When the fluoride ion concentration in the fluoride-containing mine water was 3, 5, and 10 mg / L, and the defluoridating agent dosage was 0.05%, 0.06%, and 0.08%, respectively, the effluent fluoride ion concentrations were 1.8 mg / L, 3.4 mg / L, and 7.3 mg / L, respectively, all failing to reduce to below 1 mg / L.
[0076] Comparative Example 4:
[0077] This comparative example provides a method for preparing a defluoridating agent for mine water, comprising the following steps: adding 200g aluminum chloride, 40g calcium chloride, and 20g magnesium chloride to 730mL of deionized water, stirring at 200rpm for 5min, then adding 4g nitric acid triacetic acid, 4g α-hydroxyacetic acid, and 2g sodium silicate, continuing to stir under heating at 40℃ for 5min, keeping warm for 1h, and obtaining the defluoridating agent after cooling.
[0078] The defluoridating agent prepared in Comparative Example 4 was used to conduct defluoridation tests on fluoride-containing mine water with different fluoride ion concentrations, following the methods described in Application Examples 1 to 3. The results showed that without the addition of the flocculant iron salt, the material settling effect was poor, making mud-water separation difficult, and the defluoridation effect also decreased. When the fluoride ion concentration in the fluoride-containing mine water was 3, 5, and 10 mg / L, and the defluoridating agent dosage was 0.05%, 0.06%, and 0.08%, the effluent fluoride ion concentrations were 1.2 mg / L, 2.1 mg / L, and 4.6 mg / L, respectively, all failing to reduce to below 1 mg / L.
[0079] Comparative Example 5:
[0080] This comparative example provides a method for preparing a defluoridating agent for mine water, comprising the following steps: adding 200g aluminum chloride, 40g calcium chloride, and 20g ferric chloride to 730mL of deionized water, stirring at 200rpm for 5min, then adding 4g nitric acid, 4g α-hydroxyacetic acid, and 2g sodium silicate, continuing to stir under heating at 40℃ for 5min, keeping warm for 1h, and obtaining the defluoridating agent after cooling.
[0081] The defluoridating agent prepared in Comparative Example 4 was used to conduct defluoridation tests on fluoride-containing mine water with different fluoride ion concentrations, following the methods described in Application Examples 1 to 3. The results showed that the defluoridation effect of the material decreased even without the addition of magnesium salts. When the fluoride ion concentration in the fluoride-containing mine water was 3, 5, and 10 mg / L, and the dosage of the defluoridating agent was 0.05%, 0.06%, and 0.08%, the effluent fluoride ion concentrations were 1.7 mg / L, 2.5 mg / L, and 5.2 mg / L, respectively, all failing to reduce to below 1 mg / L.
[0082] It should be noted that, in this document, relational terms such as "first" and "second" are used only to distinguish one entity or operation from another, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Furthermore, the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such process, method, article, or apparatus.
[0083] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.
Claims
1. A method for preparing a mine water defluoridation agent, characterized by, The process includes the following steps: aluminum chloride, calcium chloride, magnesium chloride, and ferric chloride are added to water and stirred at 200 rpm for 5 minutes. Then, disodium ethylenediaminetetraacetate, α-hydroxyacetic acid, and ethanol are added, and the mixture is stirred at 60°C for 10 minutes. After dissolution, the mixture is kept at this temperature for 1 hour and then cooled to obtain a mine water defluoridator. The molar ratio of aluminum chloride, calcium chloride, magnesium chloride, and ferric chloride is 1:(0.16~0.62):(0.09~0.36):(0.03~0.23). The mass ratio of aluminum chloride, calcium chloride, magnesium chloride, ferric chloride, disodium ethylenediaminetetraacetate, α-hydroxyacetic acid, and ethanol is 10:2:1:1:0.2:0.2:0.
1.
2. A defluoridating agent for mine water, characterized in that, It is prepared by the preparation method described in claim 1.
3. The application of the mine water defluoridating agent as described in claim 2 in mine water defluorination, characterized in that, The process includes the following steps: adding the mine water defluoridating agent to fluoride-containing mine water, stirring and mixing to form a colloidal state, then adding a flocculant to form flocs, allowing the flocs to settle, and obtaining a clear liquid after defluorination.
4. The application according to claim 3, characterized in that, The flocculant is polyacrylamide flocculant, the fluoride ion concentration in the fluoride-containing mine water is 1-10 mg / L; the dosage of the mine water defluoridator is 0.05-0.1 wt%; the stirring speed is 200-300 rpm; the concentration of the polyacrylamide flocculant solution is 0.1 wt%, and the dosage is 0.1-0.2 wt%.
Citation Information
Patent Citations
Fluorine removal agent, preparation method of fluorine removal agent and method for treating fluorine-containing mine water
CN114590879A
Integrated efficient flocculating agent for desulfurization wastewater and preparation method of integrated efficient flocculating agent
CN116835734A