Buton rock asphalt micro-powder composite waterproof material and preparation method thereof
Through microwave activation and nanomaterial modification of Butun rock asphalt powder, the problems of insufficient weather resistance and high temperature performance of traditional asphalt waterproofing materials have been solved, environmental protection has been improved and costs have been reduced, making it suitable for a variety of waterproofing material applications.
Patent Information
- Application Number
- CN202510832960.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-06-20
- Publication Date
- 2025-10-17
AI Technical Summary
Traditional asphalt waterproofing materials have problems such as insufficient weather resistance, poor high temperature performance, poor environmental protection and high cost, and the dispersibility of Buton rock asphalt powder has not been fully utilized.
Butun rock asphalt micropowder is treated with microwave activation, combined with nanomaterials and silane coupling agents to prepare Butun rock asphalt micropowder composite waterproof material. The dispersibility is improved through particle size control and surface activation, and nano titanium dioxide or boron nitride nanosheets are added to enhance UV resistance and catalytic activity.
It improves the weather resistance and high-temperature stability of the material, reduces VOC emissions, achieves environmental protection goals, and reduces costs by 40%. It is suitable for the preparation of highly weather-resistant and puncture-resistant waterproof membranes and self-healing waterproof coatings.
Smart Images

Figure SMS_1
Abstract
Description
TECHNICAL FIELD
[0001] The present application relates to the technical field of building waterproof materials, in particular to a buton rock asphalt micro-powder composite waterproof material and a preparation method thereof. BACKGROUND
[0002] Asphalt waterproof materials include asphalt-based waterproof coiled materials and asphalt-based waterproof coatings, wherein the asphalt-based waterproof coiled materials refer to coiled materials made of petroleum asphalt impregnated with thick paper or glass silk cloth, asbestos cloth, cotton and linen fabrics, etc., and the asphalt-based waterproof coatings refer to water emulsion type or solvent type waterproof coatings prepared by taking asphalt as a base material.
[0003] The asphalt-based waterproof coatings are water emulsion type or solvent type waterproof coatings prepared by taking asphalt as a base material, and are divided into cold primer, emulsified asphalt waterproof coating, lime emulsified asphalt waterproof coating and water-based asphalt-based waterproof coating.
[0004] The traditional waterproof materials have the following defects: poor weather resistance: the elongation at break of SBS modified asphalt waterproof coiled material is attenuated by 40%-50% after 3000 hours of ultraviolet aging; poor high-temperature performance: the thermal stability of ordinary asphalt is less than 1 hour at 80 DEG C, and it is easy to soften and flow; poor environmental protection: the VOC emission exceeds the standard (≥200 μg / g) due to the synthetic resin modifier; high cost: the price of high-quality modifier is 15-20 thousand yuan / ton, which limits large-scale application.
[0005] In the prior art, buton rock asphalt (BRA) has partially replaced SBS and talc due to its natural anti-aging property, high nitrogen content (≥3%) and carbonate component (more than 70%), but the traditional process does not fully utilize its micronization potential, resulting in uneven dispersion and performance fluctuation.
[0006] Therefore, how to develop a buton rock asphalt micro-powder composite waterproof material with strong weather resistance, high-temperature resistance, environmental protection and low cost and a preparation method thereof is a technical problem to be solved by the person skilled in the art. SUMMARY
[0007] Therefore, the present application provides a buton rock asphalt micro-powder composite waterproof material and a preparation method thereof.
[0008] In order to achieve the above-mentioned purpose, the present application adopts the following technical solutions:
[0009] The buton rock asphalt micro-powder composite waterproof material is a waterproof coiled material coating or a waterproof coating.
[0010] The waterproof coiled material coating comprises the following raw materials by weight:
[0011] Base asphalt 35-45 parts, butte rock asphalt powder 35-50 parts, SBS modifier (styrene-butadiene block copolymer) 8-12 parts, naphthenic oil 3-5 parts, polypropylene 2-5 parts, talc 0-10 parts, nano titanium white powder or boron nitride nanosheet 0-08-0.3 parts;
[0012] The waterproof coating comprises the following raw materials by weight:
[0013] Base asphalt 35-45 parts, butte rock asphalt powder 35-50 parts, SBS modifier 3-8 parts, bentonite paste 5-25 parts, fluorocarbon emulsion 5-20 parts, water 5-15 parts, nano titanium white powder or boron nitride nanosheet 0.08-0.3 parts;
[0014] The preparation method of the butte rock asphalt powder comprises the following steps: crushing blocky butte rock asphalt into powder with a particle size of ≤75 μm, then placing the powder in a microwave irradiation device for microwave activation, and finally adding a silane coupling agent for mixing and drying to obtain the butte rock asphalt powder.
[0015] The butte rock asphalt powder of the present application releases nitrogen element active sites through microwave activation, and the dispersibility of the butte rock asphalt is improved by 3 times, and the specific surface area is increased from 0.8 m 2 / g to 3.5 m 2 / g; the silane coupling agent enhances the interfacial bonding force with asphalt. The addition of nano titanium white powder or boron nitride nanosheet improves the ultraviolet resistance and decomposes nitrogen oxides, and the catalytic activity is ≥82%, and the nano material is compounded with fluorocarbon emulsion, which has the functions of self-cleaning, ultraviolet resistance and catalytic purification.
[0016] Compared with the prior art, the butte rock asphalt powder composite waterproof material of the present application improves the weather resistance and high temperature stability; the dispersibility of butte rock asphalt in asphalt is improved by adding butte rock asphalt powder; more than 50% of SBS and fillers are replaced by butte rock asphalt powder, VOC emission is reduced to below 50 μg / g, VOC emission is reduced by more than 83%, environmental protection target is achieved, cost is reduced by 40%, and comprehensive cost control is 0.8-1.2 yuan / ton; it is especially suitable for preparing high-weather-resistant, puncture-resistant waterproof coiled material and self-healing waterproof coating, and building waterproof coiled material, pavement repair, water conservancy anti-seepage engineering, and adapting to-25℃ to 80℃ environment.
[0017] Further, the power of microwave activation is 3-5 kW, the frequency of microwave activation is 2450 MHz, and the time of microwave activation is 5-10 minutes.
[0018] Further, the silane coupling agent is gamma-aminopropyl triethoxysilane, and the mass ratio of blocky butte rock asphalt to silane coupling agent is 100:(1-2).
[0019] The application also provides a preparation method of the buton rock asphalt micro-powder composite waterproof material, comprising the following steps:
[0020] (1) each raw material is weighed according to the buton rock asphalt micro-powder composite waterproof material;
[0021] (2) the matrix asphalt is heated, then the buton rock asphalt micro-powder is added, and stirring is uniformly carried out to obtain a mixture;
[0022] (3) the mixture obtained in step (2) is heated, then the SBS modifier is added to carry out shearing treatment;
[0023] (4) the mixture after shearing treatment in step (3) is cooled, then the naphthenic oil, polypropylene, talcum powder and nano-titanium white powder or boron nitride nanosheet are added, and finally homogenization treatment is carried out to obtain the waterproof coiled material coating;
[0024] or, the mixture after shearing treatment in step (3) is cooled, then the bentonite paste and hot water are added to carry out heating mixing and stirring to realize pre-gelation, then the fluorocarbon emulsion and nano-titanium white powder or boron nitride nanosheet are added, and finally homogenization treatment is carried out to obtain the waterproof coating.
[0025] The application has the advantages that the preparation method is simple, convenient to operate, and suitable for wide production and application.
[0026] Further, in step (2), the matrix asphalt is heated to 130-160 DEG C, the stirring speed is 300 r / min, and the stirring time is 0.5 hours.
[0027] Further, in step (3), the mixture obtained in step (2) is heated to 185-200 DEG C, the shearing time is 2 hours, and the shearing speed is 3000 r / min.
[0028] Further, in step (4), the temperature of the hot water is 80 DEG C, the heating temperature is 160 DEG C, the stirring speed is 100-200 rpm, and the stirring time is 10-20 min.
[0029] Further, in step (4), the mixture after shearing treatment in step (3) is cooled to 60-80 DEG C, the homogenization time is 5 hours, and the homogenization speed is 2800-2900 r / min. DETAILED DESCRIPTION
[0030] The technical solutions in the embodiments of the application will be clearly and completely described below. Obviously, the described embodiments are only part of the embodiments of the application, rather than all the embodiments. Based on the embodiments in the application, all other embodiments obtained by those skilled in the art without creative labor fall within the protection scope of the application.
[0031] In the examples and comparative examples of the present application:
[0032] The base asphalt is selected as 90# asphalt;
[0033] The butin rock asphalt contains 30% of asphalt;
[0034] The type of SBS modifier is 1301 type SBS modifier;
[0035] The naphthenic oil has the quality specification of softening point ≥ 100℃, pour point ≤ -30℃, CA% ≥ 50%, and flash point greater than 200℃;
[0036] The fluorocarbon emulsion is purchased from BLJ-9988 type fluorocarbon emulsion produced and sold by Shanghai Baolijing New Material Co., Ltd.
[0037] Example 1
[0038] The preparation method of the butin rock asphalt micro-powder composite waterproof coiled material coating material includes the following steps:
[0039] (1) The raw materials are weighed: 40 kg of base asphalt, 40 kg of butin rock asphalt micro-powder, 10 kg of SBS modifier, 4 kg of naphthenic oil, 3 kg of polypropylene, 5 kg of talcum powder, and 0.2 kg of nano titanium white powder;
[0040] The preparation method of the butin rock asphalt micro-powder includes the following steps: the blocky butin rock asphalt is crushed into a powder with a particle size ≤ 75 μm, then is placed in a microwave irradiation device for microwave activation, the power of microwave activation is 4 kW, the frequency of microwave activation is 2450 MHz, the time of microwave activation is 8 minutes, finally is mixed by spraying silane coupling agent γ-aminopropyl triethoxysilane, the mass ratio of blocky butin rock asphalt and silane coupling agent is 100:1, and is dried at 100℃ for 2 hours to obtain the butin rock asphalt micro-powder.
[0041] (2) The base asphalt is heated to 150℃, then the butin rock asphalt micro-powder is added and stirred uniformly, the stirring speed is 300 r / min, and the stirring time is 0.5 hours to obtain a mixture;
[0042] (3) The mixture obtained in step (2) is heated to 190℃, then the SBS modifier is added for shearing treatment, the shearing time is 2 hours, and the shearing speed is 3000 r / min;
[0043] (4) The mixture after shearing treatment in step (3) is cooled to 70℃, then the naphthenic oil, polypropylene, talcum powder, and nano titanium white powder are added, and finally are homogenized, the homogenization time is 5 hours, and the homogenization speed is 2800 r / min to obtain the waterproof coiled material coating material.
[0044] Comparative Example 1
[0045] The preparation method of the Buton rock asphalt micro-powder composite waterproof roll material coating includes the following steps:
[0046] (2) The raw materials are weighed: 40 kg of base asphalt, 40 kg of Buton rock asphalt micro-powder, 10 kg of SBS modifier, 4 kg of naphthenic oil, 3 kg of polypropylene, 5 kg of talcum powder, and 0.2 kg of nano titanium white powder;
[0047] The preparation method of the Buton rock asphalt micro-powder includes the following steps: crushing the blocky Buton rock asphalt into a powder with a particle size of ≤75 μm, and finally spraying and mixing the silane coupling agent γ-aminopropyl triethoxysilane, the mass ratio of the blocky Buton rock asphalt and the silane coupling agent being 100:1, drying at 100°C for 2 hours, to obtain the Buton rock asphalt micro-powder.
[0048] (2) The base asphalt is heated to 150°C, and then the Buton rock asphalt micro-powder is added and stirred uniformly, the stirring speed being 300 r / min and the stirring time being 0.5 hours, to obtain a mixture;
[0049] (3) The mixture obtained in step (2) is heated to 190°C, and then the SBS modifier is added for shearing treatment, the shearing time being 2 hours and the shearing speed being 3000 r / min;
[0050] (4) The mixture after shearing treatment in step (3) is cooled to 70°C, and then the naphthenic oil, the polypropylene, the talcum powder, and the nano titanium white powder are added, and finally homogenized, the homogenization time being 5 hours and the homogenization speed being 2800 r / min, to obtain the waterproof roll material coating.
[0051] Compared with Example 1, the Buton rock asphalt micro-powder in Comparative Example 1 is not subjected to microwave activation.
[0052] Example 2
[0053] The preparation method of the Buton rock asphalt micro-powder composite waterproof roll material coating includes the following steps:
[0054] (3) The raw materials are weighed: 40 kg of base asphalt, 40 kg of Buton rock asphalt micro-powder, 10 kg of SBS modifier, 4 kg of naphthenic oil, 3 kg of polypropylene, 5 kg of talcum powder, and 0.2 kg of nano titanium white powder;
[0055] The preparation method of the Buton rock asphalt micro powder comprises the following steps: crushing blocky Buton rock asphalt into a powder with a particle size of ≤75 μm, then placing the powder in a microwave irradiation device for microwave activation, the microwave activation power is 3 kW, the microwave activation frequency is 2450 MHz, the microwave activation time is 5 minutes, finally spraying and mixing a silane coupling agent γ-aminopropyl triethoxysilane, the mass ratio of the blocky Buton rock asphalt and the silane coupling agent is 100:1, and drying at 100 ℃ for 2 hours to obtain the Buton rock asphalt micro powder.
[0056] (2) heating the matrix asphalt to 130 ℃, then adding the Buton rock asphalt micro powder, uniformly stirring, the stirring speed is 300 r / min, and the stirring time is 0.5 hours to obtain a mixture;
[0057] (3) increasing the temperature of the mixture obtained in step (2) to 185 ℃, then adding an SBS modifier for shearing treatment, the shearing time is 2 hours, and the shearing speed is 3000 r / min;
[0058] (4) decreasing the temperature of the mixture after the shearing treatment in step (3) to 60 ℃, then adding naphthenic oil, polypropylene, talcum powder and nano titanium white powder, and finally homogenizing, the homogenizing time is 5 hours, and the homogenizing speed is 2800 r / min to obtain a waterproof roll coating material.
[0059] Example 3
[0060] The preparation method of the Buton rock asphalt micro powder composite waterproof roll coating material comprises the following steps:
[0061] (4) weighing each raw material: 45 kg of matrix asphalt, 50 kg of Buton rock asphalt micro powder, 12 kg of SBS modifier, 5 kg of naphthenic oil, 5 kg of polypropylene, 10 kg of talcum powder and 0.3 kg of nano titanium white powder;
[0062] The preparation method of the Buton rock asphalt micro powder comprises the following steps: crushing blocky Buton rock asphalt into a powder with a particle size of ≤75 μm, then placing the powder in a microwave irradiation device for microwave activation, the microwave activation power is 5 kW, the microwave activation frequency is 2450 MHz, the microwave activation time is 10 minutes, finally spraying and mixing a silane coupling agent γ-aminopropyl triethoxysilane, the mass ratio of the blocky Buton rock asphalt and the silane coupling agent is 100:1, and drying at 100 ℃ for 2 hours to obtain the Buton rock asphalt micro powder.
[0063] (2) heating the matrix asphalt to 160 ℃, then adding the Buton rock asphalt micro powder, uniformly stirring, the stirring speed is 300 r / min, and the stirring time is 0.5 hours to obtain a mixture;
[0064] (3) the mixture obtained in step (2) is heated to 200°C, and then SBS modifier is added for shearing treatment, the shearing time is 2 hours, and the shearing rate is 3000 r / min;
[0065] (4) the mixture after shearing treatment in step (3) is cooled to 80°C, then naphthenic oil, polypropylene, talcum powder and nano titanium white powder are added, and finally homogenization treatment is performed, the homogenization time is 5 hours, and the homogenization rotation speed is 2800 r / min, to obtain a waterproof roll coating material.
[0066] Example 4
[0067] The preparation method of the Buton rock asphalt micro-powder composite waterproof coating includes the following steps:
[0068] (1) the raw materials are weighed: 40 kg of base asphalt, 40 kg of Buton rock asphalt micro-powder, 5 kg of SBS modifier, 15 kg of bentonite paste, 10 kg of fluorocarbon emulsion, 10 kg of water, and 0.2 kg of nano titanium white powder;
[0069] The preparation method of the Buton rock asphalt micro-powder includes the following steps: the blocky Buton rock asphalt is crushed into a powder with a particle size of ≤75 μm, and then is placed in a microwave irradiation device for microwave activation, the microwave activation power is 4 kW, the microwave activation frequency is 2450 MHz, the microwave activation time is 8 minutes, and finally the Buton rock asphalt is mixed with a silane coupling agent γ-aminopropyl triethoxysilane, the mass ratio of the blocky Buton rock asphalt to the silane coupling agent is 100:1, and the mixture is dried at 100°C for 2 hours to obtain the Buton rock asphalt micro-powder.
[0070] (2) the base asphalt is heated to 140°C, then the Buton rock asphalt micro-powder is added, and stirring is uniformly performed at a stirring rotation speed of 300 r / min for 0.5 hours to obtain a mixture;
[0071] (3) the mixture obtained in step (2) is heated to 190°C, and then SBS modifier is added for shearing treatment, the shearing time is 2 hours, and the shearing rate is 3000 r / min;
[0072] (4) the mixture after shearing treatment in step (3) is cooled to 70°C, then bentonite paste and 80°C hot water are added for pre-gelation by heating and mixing at 160°C, stirring is performed at a stirring rotation speed of 200 r / min for 20 min, then fluorocarbon emulsion and nano titanium white powder are added, and finally homogenization treatment is performed, the homogenization time is 5 hours, and the homogenization rotation speed is 2800 r / min, to obtain a waterproof coating.
[0073] Comparative Example 2
[0074] The preparation method of the Buton rock asphalt micro-powder composite waterproof coating includes the following steps:
[0075] (1) Weigh each raw material: 40 kg of base pitch, 40 kg of Buton rock asphalt powder, 5 kg of SBS modifier, 15 kg of bentonite paste, 10 kg of fluorocarbon emulsion, 10 kg of water, and 0.2 kg of nano titanium white powder;
[0076] The preparation method of the Buton rock asphalt powder includes the following steps: crushing the blocky Buton rock asphalt into a powder with a particle size of ≤75 μm, spraying and mixing silane coupling agent γ-aminopropyl triethoxysilane, the mass ratio of the blocky Buton rock asphalt and the silane coupling agent being 100:1, drying at 100°C for 2 hours, and obtaining the Buton rock asphalt powder.
[0077] (2) Heat the base pitch to 140°C, then add the Buton rock asphalt powder, stir uniformly, the stirring speed being 300 r / min, and the stirring time being 0.5 hours, to obtain a mixture;
[0078] (3) Raise the temperature of the mixture obtained in step (2) to 190°C, then add the SBS modifier for shearing treatment, the shearing time being 2 hours and the shearing speed being 3000 r / min;
[0079] (4) Lower the temperature of the mixture after shearing treatment in step (3) to 70°C, then add the bentonite paste and 80°C hot water for heating mixing and stirring at 160°C to achieve pre-gelation, the stirring speed being 200 r / min and the stirring time being 20 min, then add the fluorocarbon emulsion and the nano titanium white powder, and finally homogenize, the homogenizing time being 5 hours and the homogenizing speed being 2800 r / min, to obtain the waterproof coating.
[0080] Compared with Example 4, the Buton rock asphalt powder in Comparative Example 2 is not subjected to microwave activation.
[0081] Example 5
[0082] The preparation method of the Buton rock asphalt powder composite waterproof coating includes the following steps:
[0083] (1) Weigh each raw material: 40 kg of base pitch, 40 kg of Buton rock asphalt powder, 5 kg of SBS modifier, 15 kg of bentonite paste, 10 kg of fluorocarbon emulsion, 10 kg of water, and 0.2 kg of nano titanium white powder;
[0084] The preparation method of the Buton rock asphalt powder includes the following steps: crushing the blocky Buton rock asphalt into a powder with a particle size of ≤75 μm, then placing it in a microwave irradiation device for microwave activation, the microwave activation power being 3 kW, the microwave activation frequency being 2450 MHz, the microwave activation time being 5 minutes, finally spraying and mixing silane coupling agent γ-aminopropyl triethoxysilane, the mass ratio of the blocky Buton rock asphalt and the silane coupling agent being 100:1, drying at 100°C for 2 hours, and obtaining the Buton rock asphalt powder.
[0085] (2) The base pitch is heated to 130°C, then the Buton rock pitch powder is added and stirred uniformly, the stirring speed is 300 r / min, and the stirring time is 0.5 hours to obtain a mixture;
[0086] (3) The mixture obtained in step (2) is heated to 185°C, then the SBS modifier is added for shearing treatment, the shearing time is 2 hours, and the shearing speed is 3000 r / min;
[0087] (4) The mixture after shearing treatment in step (3) is cooled to 60°C, then the bentonite paste and 80°C hot water are added for heating mixing and stirring at 160°C to realize pre-gelation, the stirring speed is 200 r / min, and the stirring time is 20 min, then the fluorocarbon emulsion and nano titanium white powder are added, and finally homogenization treatment is performed, the homogenization time is 5 hours, and the homogenization speed is 2800 r / min to obtain a waterproof coating.
[0088] Example 6
[0089] The preparation method of the Buton rock pitch powder composite waterproof coating comprises the following steps:
[0090] (1) The raw materials are weighed: base pitch 45 kg, Buton rock pitch powder 50 kg, SBS modifier 8 kg, bentonite paste 25 kg, fluorocarbon emulsion 20 kg, water 15 kg, and boron nitride nanosheet 0.3 kg;
[0091] The preparation method of the Buton rock pitch powder comprises the following steps: the blocky Buton rock pitch is crushed into a powder with a particle size of ≤75 μm, then microwave activation is performed in a microwave irradiation device, the microwave activation power is 5 kW, the microwave activation frequency is 2450 MHz, the microwave activation time is 10 minutes, and finally mixing is performed by spraying silane coupling agent γ-aminopropyl triethoxysilane, the mass ratio of the blocky Buton rock pitch and the silane coupling agent is 100:1, and 100°C drying is performed for 2 hours to obtain the Buton rock pitch powder.
[0092] (2) The base pitch is heated to 160°C, then the Buton rock pitch powder is added and stirred uniformly, the stirring speed is 300 r / min, and the stirring time is 0.5 hours to obtain a mixture;
[0093] (3) The mixture obtained in step (2) is heated to 200°C, then the SBS modifier is added for shearing treatment, the shearing time is 2 hours, and the shearing speed is 3000 r / min;
[0094] (4) the mixture after shearing treatment in step (3) is cooled to 80°C, bentonite paste and 80°C hot water are then added, and heating mixing and stirring are carried out at 160°C to achieve pre-gelation, the stirring speed is 200 r / min, the stirring time is 20 min, fluorocarbon emulsion and nano titanium white or boron nitride nanosheet are then added, and finally homogenization treatment is carried out, the homogenization time is 5 hours, and the homogenization speed is 2800 r / min, to obtain the waterproof coating.
[0095] Effect experiment:
[0096] 1. The waterproof roll material is prepared, the base material is selected as polyester felt, and the waterproof roll coating material of examples 1-3 and comparative example 1 is implemented by dipping coating, and the thickness of the waterproof roll material is 3.5 mm.
[0097] 2. The waterproof coating of examples 4-6 and comparative example 2 is rolled to a thickness of 1.0 mm.
[0098] Table 1 Performance measurement of the waterproof roll coating material and the waterproof coating of examples 1-6 and comparative examples 1-2
[0099]
[0100] The above description of the disclosed examples enables one skilled in the art to make or use the invention. Numerous modifications to these examples will be apparent to those skilled in the art, and the general principles defined herein can be applied to other examples without departing from the spirit or scope of the invention. Therefore, the present invention is not to be limited to the examples shown herein but is to be accorded the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A Butun rock asphalt powder composite waterproof material, characterized in that: It is a waterproof membrane coating material or waterproof coating; The waterproof coiled material coating material comprises the following raw materials in parts by weight: 35-45 parts of matrix asphalt, 35-50 parts of Buton rock asphalt powder, 8-12 parts of SBS modifier, 3-5 parts of naphthenic oil, 2-5 parts of polypropylene, 0-10 parts of talc, 0.08-0.3 parts of nano titanium dioxide or boron nitride nanosheets; The waterproof coating comprises the following raw materials in parts by weight: 35-45 parts of matrix asphalt, 35-50 parts of Buton rock asphalt powder, 3-8 parts of SBS modifier, 5-25 parts of bentonite paste, 5-20 parts of fluorocarbon emulsion, 5-15 parts of water, 0.08-0.3 parts of nano titanium dioxide or boron nitride nanosheets; The preparation method of the Butun rock asphalt powder includes the following steps: crushing the block Butun rock asphalt into powder with a particle size of ≤75μm, then placing it in a microwave radiation device for microwave activation, and finally adding a silane coupling agent for mixing and drying to obtain the Butun rock asphalt powder.
2. The Butun rock asphalt powder composite waterproof material according to claim 1, characterized in that: The power of microwave activation is 3-5 kW, the frequency of microwave activation is 2450 MHz, and the time of microwave activation is 5-10 minutes.
3. The Butun rock asphalt powder composite waterproof material according to claim 1, characterized in that: The silane coupling agent is gamma-aminopropyltriethoxysilane, and the mass ratio of the blocky buton rock asphalt to the silane coupling agent is 100:(1-2).
4. A method for preparing a Butun rock asphalt micropowder composite waterproof material, characterized in that: The following steps are involved: (1) Weigh the raw materials of the Butun rock asphalt powder composite waterproof material according to any one of claims 1 to 3; (2) heating the matrix asphalt, then adding the Buton rock asphalt powder and stirring uniformly to obtain a mixture; (3) heating the mixture obtained in step (2), and then adding an SBS modifier to perform shearing treatment; (4) cooling the mixture after the shearing treatment in step (3), then adding cyclohexane oil, polypropylene, talc powder and nano titanium dioxide or boron nitride nanosheets, and finally homogenizing to obtain the waterproof coiled material coating; Alternatively, the mixture after the shearing treatment in step (3) is cooled, and then bentonite paste and hot water are added and heated, mixed and stirred to achieve pre-gelation, and then fluorocarbon emulsion and nano titanium dioxide or boron nitride nanosheets are added, and finally homogenized to obtain the waterproof coating.
5. The method for preparing a Butun rock asphalt micropowder composite waterproof material according to claim 4, characterized in that: In step (2), the base asphalt is heated to 130-160° C.; the stirring speed is 300 r / min, and the stirring time is 0.5 hour.
6. The method for preparing a Butun rock asphalt micropowder composite waterproof material according to claim 4, characterized in that: In step (3), the mixture obtained in step (2) is heated to 185-200° C.; the shearing time is 2 hours, and the shearing rate is 3000 r / min.
7. The method for preparing a Butun rock asphalt micropowder composite waterproof material according to claim 4, characterized in that: In step (4), the hot water temperature is 80° C., the heating temperature is 160° C., the stirring speed is 100-200 rpm, and the stirring time is 10-20 min.
8. The method for preparing a Butun rock asphalt micropowder composite waterproof material according to claim 4, characterized in that: In step (4), the mixture after the shearing treatment in step (3) is cooled to 60-80° C.; the homogenization time is 5 hours, and the homogenization speed is 2800-2900 r / min.
Citation Information
Patent Citations
Compound buton rock modified asphalt of nano material for heavy-loaded traffic road and preparation technology of compound buton rock modified asphalt
CN104817850A
Buton rock-modified asphalt waterproof rolling material coating material and technological method thereof
CN106009728A
Buton rock modified asphalt waterproof paint and preparation method thereof
CN106085234A
Environment-friendly anti-corrosion paint
CN108384375A
Sound-insulation spraying rapid-solidifying SBS modified asphalt waterproofing coating and preparation and using method thereof
CN109096919A
Cited By
Rock asphalt modified asphalt based on wet activation process and preparation method thereof
CN122103918A