Adhesive sheet, adhesive sheet with release film, adhesive sheet for constituent member of flexible image display device, laminate for image display device, flexible image display device, photocurable adhesive sheet, and adhesive composition

By using an adhesive composition containing (meth)acrylic copolymers, active species are activated and combined with photocurable compounds, the contradiction between the sensitivity, flexibility, and shape stability of the adhesive sheet in the face of active energy rays is resolved, achieving high sensitivity and rapid curing.

CN120813659APending Publication Date: 2025-10-17MITSUBISHI CHEM CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202480015362.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-03-22
Filing Date
2024-02-26
Publication Date
2025-10-17

AI Technical Summary

Technical Problem

Conventional PSA sheets have difficulty achieving both flexibility and shape stability while ensuring sensitivity to active energy rays.

Method used

An adhesive composition containing (meth)acrylic acid copolymers is used. Active species are excited by irradiation with active energy rays to meet specific requirements for energy storage shear modulus, maximum strain value and recovery rate. Combined with photocurable compounds and photoinitiators, a highly sensitive adhesive sheet is formed.

Benefits of technology

It achieves high sensitivity and efficient curing to active energy rays, possesses excellent flexibility and shape stability, can quickly restore a flat state, and reduces the decrease in cohesion caused by photoinitiator exudation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005569430590000041
    Figure BDA0005569430590000041
  • Figure BDA0005569430590000091
    Figure BDA0005569430590000091
  • Figure BDA0005569430590000451
    Figure BDA0005569430590000451
Patent Text Reader

Abstract

An adhesive sheet which is formed from an adhesive composition containing a (meth) acrylic copolymer (A) that has a structural unit derived from a monomer M that generates an active species excited by irradiation with an active energy ray, and which satisfies the following requirements (1) and (2). Condition (1): the storage shear modulus (G '(-20 DEG C)) at-20 DEG C as determined by dynamic viscoelasticity measurement in a shear mode at a frequency of 1 Hz is 10 kPa or more and 1000 kPa or less, and Condition (2): the maximum strain value (gamma max) when a stress of 2 kPa is applied at 60 DEG C for 600 seconds is less than 80%.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present application relates to an adhesive sheet, an adhesive sheet with a release film, an adhesive sheet for a flexible image display device constituting member, a laminate for an image display device, a flexible image display device, a photocurable adhesive sheet, and an adhesive composition.

[0002] This application claims priority based on Japanese Patent Application No. 2023-045353 filed on March 22, 2023, the contents of which are incorporated herein. BACKGROUND

[0003] In recent years, a flexible image display device including a curved portion using an organic light emitting diode (OLED), a quantum dot (QD), a bendable and rollable flexible image display device is being widely commercialized.

[0004] In such a display device, a plurality of sheet members for forming a laminated structure of a cover lens, a circularly polarizing plate, a touch film sensor, a color filter, a light emitting element, and the like are adhered with a transparent adhesive sheet, and if focusing on a certain adhesive sheet, it can be regarded as a laminate in which a member and an adhesive sheet are laminated.

[0005] In Patent Literature 1, regarding a foldable flexible image display device, an adhesive and an adhesive sheet which can be applied to a repeated bending device by setting a product value of a creep compliance variation value and a relaxation modulus variation value to an appropriate range, and a bending laminated member and a repeated bending device are disclosed.

[0006] In Patent Literature 2, as an adhesive capable of forming an adhesive layer excellent in heat resistance, holding force, and adhesive force, an adhesive of a (meth)acrylic polymer having a weight average molecular weight of 50,000 to 1,000,000 obtained by polymerizing a monomer mixture containing a large molecule monomer having a number average molecular weight of 500 or more and less than 6,000 and a vinyl monomer is disclosed.

[0007] PRIOR ART DOCUMENTS

[0008] PATENT LITERATURE

[0009] Patent Literature 1: Japanese Patent Application Publication No. 2019-123826

[0010] Patent Literature 2: International Publication No. 2015 / 080244 SUMMARY

[0011] PROBLEMS TO BE SOLVED BY THE INVENTION

[0012] For an adhesive sheet used in a flexible image display device, further softening is required. However, there is a concern that the more the adhesive sheet is softened, the lower the sensitivity to active energy rays becomes, or the worse the shape stability becomes. In the conventional adhesive sheet of Patent Document 1, Patent Document 2, it is difficult to ensure the sensitivity to active energy rays while taking into account the softness and the shape stability.

[0013] An object of the present application is to provide an adhesive sheet having high sensitivity to active energy rays, excellent softness and shape stability, and a release-film-attached adhesive sheet, a flexible image display device component adhesive sheet, an image display device laminate, a flexible image display device, a photocurable adhesive sheet, and an adhesive composition each using the aforementioned adhesive sheet.

[0014] Approach for solving the problem

[0015] The present application has the following modes.

[0016] [1] An adhesive sheet formed of an adhesive composition containing a (meth)acrylic copolymer (A),

[0017] wherein the (meth)acrylic copolymer (A) has a structural unit derived from a monomer M that generates an active species that is excited by irradiation of active energy rays, the adhesive sheet satisfying the following requirements (1) and (2).

[0018] (1) A storage shear modulus at -20°C (G'(-20°C)) obtained by dynamic viscoelasticity measurement in a shear mode at a frequency of 1 Hz is 10 kPa or more and 1000 kPa or less; and

[0019] (2) A maximum strain value (γ max ) at the time of application of a stress of 2 kPa for 600 seconds at 60°C is less than 80%.

[0020] [2] The adhesive sheet according to [1], wherein a storage shear modulus at 30°C (G'(30°C)) obtained by dynamic viscoelasticity measurement in a shear mode at a frequency of 1 Hz is 1000 kPa or less.

[0021] [3] The adhesive sheet according to [1] or [2], wherein a glass transition temperature (Tg) defined by a maximum value of Tan δ obtained by dynamic viscoelasticity measurement in a shear mode at a frequency of 1 Hz is -20°C or lower.

[0022] [4] The adhesive sheet according to any one of [1] to [3], wherein a maximum strain value (γ max ) at the time of application of a stress of 2 kPa for 600 seconds at 60°C and a residual strain value (γmin ) the recovery rate calculated by the following formula is 60% or more.

[0023] Recovery rate (%) = 〔(γ max -γ min ) / γ max 〕 x 100

[0024] [5] The adhesive sheet according to any one of [1] to [4], wherein the gel fraction is 30% or more.

[0025] [6] The adhesive sheet according to any one of [1] to [5], wherein the content of the structural unit derived from the monomer M is 0.01 to 20 mass% with respect to the total structural units constituting the aforementioned (meth)acrylic copolymer (A).

[0026] [7] The adhesive sheet according to any one of [1] to [6], wherein the monomer M has a structure that cleaves a single bond thereof to generate a radical when excited by irradiation with active energy rays.

[0027] [8] The adhesive sheet according to any one of [1] to [7], wherein the monomer M has a structure that abstracts hydrogen from a hydrogen donor in the adhesive composition to generate a radical when excited by irradiation with active energy rays.

[0028] [9] The adhesive sheet according to any one of [1] to [8], wherein the monomer M is represented by the following formula (I).

[0029]

[0030] In the formula, R 1 represents a hydrogen atom, a methyl group, or an ethyl group, R 2 represents a linear or branched alkylene group having 1 to 5 carbon atoms, R 3 and R 4 each independently represent a linear or branched alkyl group having 1 to 5 carbon atoms, R 3 and R 4 are optionally bonded to each other to form a ring.

[0031]

[10] The adhesive sheet according to any one of [1] to [9], wherein the (meth)acrylic copolymer (A) has a structural unit derived from a linear or branched alkyl (meth)acrylate (al) having 4 to 30 carbon atoms in the alkyl group.

[0032]

[11] The adhesive sheet according to any one of [1] to

[10] , wherein the (meth)acrylic copolymer (A) is a block copolymer or a graft copolymer.

[0033]

[12] The adhesive sheet according to any one of [1] to

[11] , wherein the (meth)acrylic copolymer (A) contains a structural unit derived from the macromonomer (a9).

[0034]

[13] The adhesive sheet according to

[12] , wherein the macromonomer (a9) contains a structural unit derived from an alkyl (meth)acrylate having an alkyl group having a carbon number of 9 to 30.

[0035]

[14] The adhesive sheet according to any one of [1] to

[13] , wherein the adhesive composition contains a photocurable compound (B).

[0036]

[15] The adhesive sheet according to any one of [1] to

[14] , wherein the adhesive composition contains a photoinitiator (C).

[0037]

[16] The adhesive sheet according to any one of [1] to

[15] , wherein the adhesive composition contains a photocurable compound (B) and a photoinitiator (C).

[0038]

[17] The adhesive sheet according to

[14] , wherein the photocurable compound (B) contains a multifunctional urethane (meth)acrylate.

[0039]

[18] A release-film-attached adhesive sheet comprising the adhesive sheet according to any one of [1] to

[17] and a release film laminated to at least one surface of the aforementioned adhesive sheet.

[0040]

[19] A flexible image display device-constituting member adhesive sheet comprising the adhesive sheet according to any one of [1] to

[17] .

[0041]

[20] An image display device laminate in which two image display device-constituting members are laminated with the adhesive sheet according to any one of [1] to

[17] , at least one of the image display device-constituting members having a step of 2 μm or more in height difference at a contact surface with the adhesive sheet.

[0042]

[21] A flexible image display device comprising the image display device laminate according to

[20] .

[0043]

[22] A photocurable adhesive sheet formed of an adhesive composition containing a (meth)acrylic copolymer (A),

[0044] wherein the (meth)acrylic copolymer (A) has a structural unit derived from a monomer M that generates a radical species that is excited by irradiation with active energy rays,

[0045] The photocurable adhesive sheet satisfies the following requirements (1') and (2').

[0046] Requirement (1'): the storage shear modulus at -20°C (G'(-20°C)) obtained by dynamic viscoelasticity measurement in a shear mode at a frequency of 1 Hz is 10 kPa or more and 1000 kPa or less when active energy rays of wavelength 365 nm are irradiated to the aforementioned photocurable adhesive sheet at an arbitrary irradiation amount in the range of 1000 to 5000 mJ / cm 2

[0047] Requirement (2'): the maximum strain value (γ max ) at 60°C when a stress of 2 kPa is applied for 600 seconds is less than 80% when active energy rays of wavelength 365 nm are irradiated to the photocurable adhesive sheet at an arbitrary irradiation amount in the range of 1000 to 5000 mJ / cm 2

[0048]

[23] An adhesive composition containing a (meth)acrylic copolymer (A),

[0049] wherein the (meth)acrylic copolymer (A) has a structural unit derived from a monomer M that generates an active species that is excited by irradiation of active energy rays,

[0050] The adhesive composition satisfies the following requirements (1") and (2").

[0051] Requirement (1"): the storage shear modulus at -20°C (G'(-20°C)) obtained by dynamic viscoelasticity measurement in a shear mode at a frequency of 1 Hz is 10 kPa or more and 1000 kPa or less when active energy rays of wavelength 365 nm are irradiated to the photocurable adhesive sheet formed by drying the adhesive composition at an arbitrary irradiation amount in the range of 1000 to 5000 mJ / cm 2

[0052] Requirement (2"): the maximum strain value (γ max ) at 60°C when a stress of 2 kPa is applied for 600 seconds is less than 80% when active energy rays of wavelength 365 nm are irradiated to the photocurable adhesive sheet formed by drying the adhesive composition at an arbitrary irradiation amount in the range of 1000 to 5000 mJ / cm 2

[0053] Effects of the Invention

[0054] ​​​​According to the present application, an adhesive sheet having high sensitivity to active energy rays and capable of efficient curing, an adhesive sheet with a release film using the above adhesive sheet, an adhesive sheet for a flexible image display device constituent member, a laminate for an image display device, a flexible image display device, a photocurable adhesive sheet, and an adhesive composition can be provided. DETAILED DESCRIPTION

[0055] The following definitions of the terms apply to the present specification and claims.

[0056] "(Meth)acrylate" is a general term for acrylate and methacrylate. The same applies to "(meth)acryl", "(meth)acrylic acid", "(meth)acrylonitrile", and "(meth)acrylamide".

[0057] "(Meth)acrylic copolymer" refers to a copolymer having a structural unit derived from a (meth)acrylic monomer. The (meth)acrylic copolymer can further have a structural unit derived from a monomer other than a (meth)acrylic monomer (e.g., styrene, etc.).

[0058] "(Meth)acrylic monomer" refers to a monomer having a (meth)acryl group.

[0059] "Vinyl monomer" refers to a compound having an olefinic unsaturated bond (polymerizable carbon-carbon double bond).

[0060] "Graft copolymer" refers to a macromolecule having one or more blocks as a side chain polymer structure connected to a main chain polymer structure. The structures of the main chain polymer and the side chain polymer can be different or the same. As a method for producing a graft copolymer, there are no particular limitations, and methods such as a method in which a macromonomer having a free radical polymerizable double bond at the terminal is produced as a side chain polymer structure, and then subjected to free radical polymerization with a monomer that becomes a structural unit of a main chain polymer; a method in which a macromonomer having a reaction point with a main chain polymer having a reaction point is produced in advance, and then allowed to react; a method in which a side chain polymer structure is produced by generating a free radical on a main chain polymer using an initiator having a hydrogen abstraction ability after the main chain polymer is produced, and allowing a monomer that becomes a structural unit of a side chain polymer to react; and the like can be cited.

[0061] "~" indicating a numerical range means that the lower limit value and the upper limit value described before and after it are included, and also includes the meaning of "preferably greater than the lower limit value" or "preferably less than the upper limit value".

[0062] In addition, in the case where "x or more" (x is an arbitrary number) is described, unless otherwise specified, the meaning of "preferably greater than x" is included, and in the case where "y or less" (y is an arbitrary number) is described, unless otherwise specified, the meaning of "preferably less than y" is also included.

[0063] Further, "x and / or y (x, y are arbitrary constituents)" means at least one of x and y, and means only x, only y, or x and y.

[0064] <Adhesive sheet>

[0065] One embodiment of the present application relates to an adhesive sheet.

[0066] The adhesive sheet of the embodiment is an adhesive sheet formed from an adhesive composition containing a (meth)acrylic copolymer (A).

[0067] The (meth)acrylic copolymer (A) contains a structural unit derived from a monomer M that is excited by irradiation with active energy rays and generates a radical species. Therefore, when the (meth)acrylic copolymer (A) is irradiated with active energy rays, the structural unit derived from the monomer M is excited to generate a radical species, and functions as a photoinitiator.

[0068] Thus, the adhesive composition of the present embodiment is excellent in sensitivity to active energy rays, and is easily cured by irradiation with active energy rays, and an adhesive sheet excellent in shape stability and recovery to a flat state when a folding operation is performed can be obtained.

[0069] Further, since the curing reaction is sufficiently performed without adding a photoinitiator, or by adding a very small amount of a photoinitiator, the exudation of the photoinitiator and the decrease in cohesive force caused by the photoinitiator can be suppressed.

[0070] [(Meth)acrylic copolymer (A)]

[0071] The (meth)acrylic copolymer (A) contains a structural unit derived from a monomer M (hereinafter, also referred to as "monomer M unit").

[0072] The monomer M is excited by irradiation with active energy rays, and generates a radical species. The monomer M can also be said to be a monomer having a structure that is excited by irradiation with active energy rays to generate a radical species.

[0073] The monomer M typically has a structure that is excited by irradiation with active energy rays to generate a radical species and a radical polymerizable functional group. As the radical polymerizable functional group, for example, a functional group having an ethylenic unsaturated bond such as a (meth)acryloyl group, a vinyl group, or the like can be exemplified.

[0074] As the radical species, a radical, a cation, an anion can be exemplified, and from the aspect of reactivity, a radical is preferred.

[0075] As a structure that generates a radical by being excited by irradiation with active energy rays (hereinafter, also referred to as "radical generating group"), a structure derived from a known photoradical generator can be used, for example, an acylphosphine oxide structure, an α-aminophenylacetophenone structure, an α-hydroxyphenylacetophenone structure, a benzil ketal structure, or the like that cleaves its own single bond to generate a radical when excited by irradiation with active energy rays; a benzophenone structure, a thioxanthone structure, an anthraquinone structure, a benzoylformate structure, or the like that generates a radical by abstracting hydrogen from a hydrogen donor in the adhesive composition when excited by irradiation with active energy rays; an oxime ester structure, or the like.

[0076] The hydrogen donor in the adhesive composition can be exemplified by, for example, a group that directly has hydrogen on carbon among the functional groups contained in the structural unit of the (meth)acrylic copolymer (A), or a hydroxyl group, an amino group, an organic functional group having an ether bond, or the like that is generally used as a hydrogen-donating group. In particular, from the aspect of easy supply of hydrogen, a hydroxyl group, an amino group, and a functional group having an ether bond are preferred. Note that the ether bond has a tendency that hydrogen of a hydrocarbon structure adjacent to the ether bond is easily abstracted, and the hydrogen-donating group containing an ether bond is preferably a structure having hydrogen. In addition, a compound having the above functional group can be additionally added as a hydrogen donor.

[0077] From the viewpoint of suppressing generation of a decomposition product, the above radical generating group is preferably a structure that generates a radical by abstracting hydrogen from a hydrogen donor in the adhesive composition when excited by irradiation with active energy rays, and from the viewpoint of suppressing coloring, a benzophenone structure, a benzoylformate structure, and particularly a benzophenone structure are preferred.

[0078] On the other hand, from the viewpoint of improving the sensitivity of the adhesive sheet to active energy rays and the adhesive force, the above radical generating group is preferably a structure that generates a radical by cleaving its own single bond when excited by irradiation with active energy rays, and from the viewpoint of suppressing coloring, an α-hydroxyphenylacetophenone structure, a benzil ketal structure, and particularly an α-hydroxyphenylacetophenone structure are preferred.

[0079] As the monomer M, a monomer represented by the following formula (I) is preferred.

[0080]

[0081] In the above formula (I), R 1 represents a hydrogen atom, a methyl group, or an ethyl group. Among them, a hydrogen atom or a methyl group is preferred, and a methyl group is particularly preferred.

[0082] In the above formula (I), R 2represents a linear or branched alkylene group having 1 to 5 carbon atoms. Among them, ethylene, propane-1, 3-diyl, butane-1, 3-diyl, and butane-1, 4-diyl are preferable from the viewpoint of polymerizability and reactivity with the ethylenically unsaturated group at the time of obtaining the (meth)acrylic copolymer (A).

[0083] In the above formula (I), R 3 and R 4 each independently represents a linear or branched alkyl group having 1 to 5 carbon atoms.

[0084] R 3 and R 4 may optionally be bonded to each other to form a ring. R 3 and R 4 The carbon number of the ring formed is preferably 5 to 8, more preferably 6.

[0085] R 3 and R 4 are each independently a methyl group or an ethyl group, or R 3 and R 4 are bonded to each other and form a cyclohexane ring together with the carbon atom to which R 3 and R 4 are bonded, more preferably at least one of R 3 and R 4 is a methyl group, and further preferably both of R 3 and R 4 are methyl groups.

[0086] Specific examples of the monomer represented by formula (I) include 2-[4-(2-hydroxy-2-methyl-1-oxopropyl)phenoxy]ethyl methacrylate, 2-[4-(2-hydroxy-2-methyl-1-oxopropyl)phenoxy]ethyl acrylate, and the like.

[0087] The content of the monomer M unit in the (meth)acrylic copolymer (A) is preferably 0.01 to 20 mass%, more preferably 0.03 to 10 mass%, further preferably 0.05 to 5 mass%, particularly preferably 0.08 to 3 mass%, and most preferably 0.1 to 2 mass%, relative to 100 mass% of the total structural units constituting the (meth)acrylic copolymer (A). When the content of the monomer M unit is equal to or greater than the above lower limit, the sensitivity to active energy rays and the shape stability are more excellent, and when it is equal to or less than the above upper limit, the compatibility with other components is more excellent.

[0088] For the (meth)acrylic copolymer (A), in terms of obtaining softness, in addition to the monomer M unit, it is preferable to contain a structural unit derived from an alkyl (meth)acrylate (a1) having an alkyl group having a carbon number of 4 to 30 (hereinafter, also referred to as "(a1) unit").

[0089] In addition, in terms of obtaining excellent adhesive properties, in addition to the monomer M unit and the (a1) unit, it is preferable to contain a structural unit derived from any one or more selected from the group consisting of a carboxyl group-containing monomer (a2), a hydroxyl group-containing monomer (a3), a nitrogen-containing monomer (a4), an epoxy group-containing monomer (a5), a vinyl monomer (a6), an alkyl (meth)acrylate monomer (a7) having an alkyl group having a carbon number of 1 to 3, an alicyclic monomer (a8), a macromonomer (a9), and other copolymerizable monomers (a10).

[0090] Among the above copolymerizable monomers, it is preferable to contain any one or more selected from the group consisting of the carboxyl group-containing monomer (a2), the hydroxyl group-containing monomer (a3), and the nitrogen-containing monomer (a4).

[0091] In addition, it is more preferable to not contain the carboxyl group-containing monomer (a2) and to contain any one or more selected from the group consisting of the hydroxyl group-containing monomer (a3) and the nitrogen-containing monomer (a4). By not containing the carboxyl group-containing monomer (a2) and containing any one or more selected from the group consisting of the hydroxyl group-containing monomer (a3) and the nitrogen-containing monomer (a4), it is possible to have both corrosion resistance when the adherend contains a component having corrosion properties such as metal, adhesiveness, and moisture heat whitening resistance.

[0092] Further, it is preferable as long as at least one of the hydroxyl group-containing monomer (a3) and the nitrogen-containing monomer (a4) is contained in terms of improving cohesive force by forming a non-covalent bond such as a hydrogen bond.

[0093] The above alkyl (meth)acrylate (a1) is a linear or branched alkyl (meth)acrylate having an alkyl group having a carbon number of 4 to 30, represented by the following formula (II).

[0094] CH2=CR 5 -COOR 6

[0095] (II) (in the formula, R 5 represents a hydrogen atom or a methyl group, and R 6 represents a linear or branched alkyl group having a carbon number of 4 to 30).

[0096] As the alkyl (meth) acrylate represented by Formula (II), for example, the following can be given: n-butyl (meth) acrylate, n-pentyl (meth) acrylate, n-hexyl (meth) acrylate, n-heptyl (meth) acrylate, n-octyl (meth) acrylate, n-nonyl (meth) acrylate, n-decyl (meth) acrylate, undecyl (meth) acrylate, lauryl (meth) acrylate, n-tridecyl (meth) acrylate, n-tetradecyl (meth) acrylate, cetyl (meth) acrylate, stearyl (meth) acrylate, arachidyl (meth) acrylate, heneicosyl (meth) acrylate, behenyl (meth) acrylate, and the like (linear alkyl (meth) acrylate); sec-butyl (meth) acrylate, isobutyl (meth) acrylate; t-butyl (meth) acrylate, isoamyl (meth) acrylate, neo-pentyl (meth) acrylate, 2-ethylhexyl (meth) acrylate, isooctyl (meth) acrylate, isononyl (meth) acrylate, isodecyl (meth) acrylate, isostearyl (meth) acrylate, isobehenyl (meth) acrylate, butyloctyl (meth) acrylate, isotetradecyl (meth) acrylate, isocetyl (meth) acrylate, hexyldodecyl (meth) acrylate, isostearyl (meth) acrylate, octyldodecyl (meth) acrylate, octyldodecyl (meth) acrylate, isobehenyl (meth) acrylate, and the like (branched alkyl (meth) acrylate), and the like. One or two or more kinds thereof can be used in combination.

[0097] Among them, from the viewpoint of achieving a balance between adhesiveness and softness, a linear or branched alkyl (meth) acrylate having a carbon number of the alkyl group of 4 to 20, further 5 to 18, particularly 6 to 16, especially 7 to 14 is preferable, for example, n-butyl (meth) acrylate, n-pentyl (meth) acrylate, n-hexyl (meth) acrylate, n-octyl (meth) acrylate, n-nonyl (meth) acrylate, decyl (meth) acrylate, lauryl (meth) acrylate, sec-butyl (meth) acrylate, isobutyl (meth) acrylate, t-butyl (meth) acrylate, isoamyl (meth) acrylate, neo-pentyl (meth) acrylate, 2-ethylhexyl (meth) acrylate, isooctyl (meth) acrylate, isononyl (meth) acrylate, isodecyl (meth) acrylate, and the like are preferable.

[0098] In addition, from the viewpoint of achieving a balance between softness and recovery, it is particularly preferable to use a linear alkyl (meth) acrylate and a branched alkyl (meth) acrylate.

[0099] The content of the (a1) unit in the (meth)acrylic copolymer (A) is preferably 5 to 95% by mass, more preferably 10 to 90% by mass, further preferably 15 to 85% by mass, and particularly preferably 20 to 80% by mass, relative to 100% by mass of the total structural units constituting the (meth)acrylic copolymer (A). When the content of the (a1) unit is equal to or greater than the above lower limit, there is a tendency that the softness is excellent, and even in the case where the adherend has unevenness, there is a tendency that the unevenness followability is excellent. When the content of the (a1) unit is equal to or less than the above upper limit, there is a tendency that the effect of easily obtaining a copolymerizable monomer, the adhesion, and the cohesion are excellent. The lower limit and the upper limit of the content of the (a1) unit can be arbitrarily combined.

[0100] As the above carboxyl group-containing monomer (a2), for example, (meth)acrylic acid, 2-propenoyloxyethyl hexahydrophthalate, 2-(meth)acryloyloxyethyl maleate, 2-(meth)acryloyloxypropyl maleate, 2-(meth)acryloyloxyethyl succinate, 2-(meth)acryloyloxypropyl succinate, crotonic acid, fumaric acid, maleic acid, itaconic acid can be exemplified. One or two or more kinds thereof can be combined.

[0101] As the above hydroxyl group-containing monomer (a3), for example, (meth)acrylic acid 2-hydroxyethyl ester, (meth)acrylic acid 4-hydroxybutyl ester, (meth)acrylic acid 5-hydroxypentyl ester, (meth)acrylic acid 6-hydroxyhexyl ester, (meth)acrylic acid 8-hydroxyoctyl ester and the like (meth)acrylic acid hydroxyalkyl ester, caprolactone-modified 2-hydroxyethyl (meth)acrylate and the like caprolactone-modified hydroxy (meth)acrylate, diethylene glycol (meth)acrylate, polyethylene glycol (meth)acrylate and the like alkylene oxide-modified (meth)acrylate, 2-propenoyloxyethyl-2-hydroxyethyl phthalate and the like primary hydroxyl group-containing (meth)acrylate; (meth)acrylic acid 2-hydroxypropyl ester, (meth)acrylic acid 2-hydroxybutyl ester, (meth)acrylic acid 3-chloro-2-hydroxypropyl ester and the like secondary hydroxyl group-containing (meth)acrylate; (meth)acrylic acid 2,2-dimethyl-2-hydroxyethyl ester and the like tertiary hydroxyl group-containing (meth)acrylate; 2-hydroxyethyl vinyl ether, diethylene glycol monovinyl ether, 4-hydroxybutyl vinyl ether and the like vinyl ether can be exemplified. One or two or more kinds thereof can be used alone or in combination.

[0102] By the hydroxyl group-containing monomer (a3), the adhesion of the adhesive sheet can be improved, and the hygrothermal whitening can be suppressed.

[0103] Among the above-mentioned hydroxyl group-containing monomers (a3), hydroxyl group-containing monomers having a hydroxylalkyl group having a carbon number of 1 to 10, further 1 to 6, especially 2 to 4, are preferable, such as 2-hydroxyethyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxyethyl vinyl ether, diethylene glycol monovinyl ether, 4-hydroxybutyl vinyl ether, and the like, and (meth)acrylates containing primary hydroxyl groups, such as 2-hydroxyethyl (meth)acrylate and 4-hydroxybutyl (meth)acrylate, are particularly preferable.

[0104] From the viewpoint of imparting adhesion and resistance to hygrothermal whitening, the content of the structural unit derived from the above-mentioned hydroxyl group-containing monomer (a3) in the (meth)acrylic copolymer (A) is preferably 0.1 to 30% by mass, more preferably 0.5 to 25% by mass, further preferably 1 to 10% by mass, and particularly preferably 2 to 7% by mass, relative to 100% by mass of the total structural units constituting the (meth)acrylic copolymer (A).

[0105] As the above-mentioned nitrogen-containing monomer (a4), for example, amino group-containing monomers, amide group-containing monomers, isocyanate group-containing monomers, and (meth)acrylonitrile can be exemplified. By the nitrogen-containing monomer (a4), the cohesive force of the adhesive sheet is improved, and hygrothermal whitening can be suppressed. They can be combined by one or two or more kinds.

[0106] As the above-mentioned amino group-containing monomers, for example, (meth)acrylates containing primary amino groups such as aminomethyl (meth)acrylate and aminoethyl (meth)acrylate; (meth)acrylates containing secondary amino groups such as t-butylaminoethyl (meth)acrylate and t-butylaminopropyl (meth)acrylate; (meth)acrylates containing tertiary amino groups such as ethylaminoethyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, dimethylaminopropyl (meth)acrylate, diethylaminopropyl (meth)acrylate, and dimethylaminopropyl acrylamide; N-vinylpyrrolidone, methylvinylpyrrolidone, vinylpyridine, vinylpiperidone, vinylpyrimidine, vinylpiperazine, vinylpyrazine, vinylpyrrole, vinylimidazole, vinyloxazole, vinylmorpholine, (meth)acryloylmorpholine, N-vinylacetamide, N-vinylcaprolactam, and the like can be exemplified.

[0107] As the above-mentioned amide group-containing monomer, for example, (meth)acrylamide; N-methyl(meth)acrylamide, N-ethyl(meth)acrylamide, N-propyl(meth)acrylamide, N-n-butyl(meth)acrylamide, diacetone(meth)acrylamide, N,N'-methylenebis(meth)acrylamide, and the like N-alkyl(meth)acrylamides; N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N,N-dipropyl(meth)acrylamide, N,N-ethylmethyl(meth)acrylamide, N,N-diallyl(meth)acrylamide, and the like N,N-dialkyl(meth)acrylamides; N-hydroxymethyl(meth)acrylamide, N-hydroxyethyl(meth)acrylamide, and the like hydroxyalkyl(meth)acrylamides; N-methoxymethyl(meth)acrylamide, N-(n-butoxymethyl)(meth)acrylamide, and the like alkoxyalkyl(meth)acrylamides; maleimide or a derivative thereof, and the like can be exemplified.

[0108] As the above-mentioned isocyanate group-containing monomer, for example, 2- (meth)acryloyloxyethyl isocyanate, an alkylene oxide adduct thereof, and the like can be exemplified. The isocyanate group can be protected with a blocking agent such as methyl ethyl ketone oxime, 3,5-dimethylpyrazole, 1,2,4-triazole, diethyl malonate, and the like.

[0109] Among them, from the viewpoint of the sensitization of the above-mentioned hydrogen abstraction reaction and as a result of the effective formation of crosslinks, it is preferable to have a tertiary nitrogen atom, and particularly preferable are, for example, (meth)acrylates containing a tertiary amino group, N,N-dialkyl(meth)acrylamides, N-vinylpyrrolidone, acryloyl morpholine, and the like.

[0110] From the viewpoint of imparting cohesive force and moisture heat whitening resistance, the content of the structural unit derived from the above-mentioned nitrogen-containing monomer (a4) in the (meth)acrylic copolymer (A) is preferably 0.1 to 15 mass%, more preferably 0.5 to 13 mass%, further preferably 1 to 10 mass%, and particularly preferably 2 to 7 mass% with respect to 100 mass% of the total structural units constituting the (meth)acrylic copolymer (A).

[0111] As the above-mentioned epoxy group-containing monomer (a5), for example, glycidyl (meth)acrylate, methyl glycidyl (meth)acrylate, 3,4-epoxycyclohexylmethyl (meth)acrylate, 4-hydroxybutyl glycidyl ether (meth)acrylate can be exemplified. One or two or more kinds thereof can be combined.

[0112] As the above-mentioned vinyl monomer (a6), a compound having a vinyl group in the molecule can be given. As such a compound, vinyl ester monomers such as vinyl acetate, vinyl propionate, vinyl laurate, and vinyl stearate, and aromatic vinyl monomers such as styrene, chlorostyrene, chloromethylstyrene, α-methylstyrene, and other substituted styrenes can be given. One or two or more kinds thereof can be combined.

[0113] As the above-mentioned alkyl (meth) acrylate monomer (a7) having an alkyl group having a carbon number of 1 to 3, (meth) acrylate monomers such as methyl (meth) acrylate, ethyl (meth) acrylate, n-propyl (meth) acrylate, and isopropyl (meth) acrylate can be given. One or two or more kinds thereof can be combined.

[0114] From the viewpoint of imparting cohesion to the adhesive sheet, the content of the structural unit derived from the above-mentioned alkyl (meth) acrylate monomer (a7) in the (meth) acrylic copolymer (A) is preferably 0.1 to 15% by mass, more preferably 0.5 to 13% by mass, further preferably 1 to 10% by mass, and particularly preferably 2 to 7% by mass, relative to 100% by mass of the total structural units constituting the (meth) acrylic copolymer (A).

[0115] As the above-mentioned alicyclic monomer (a8), (meth) acrylate monomers such as cyclohexyl (meth) acrylate, 3,3,5-trimethylcyclohexyl (meth) acrylate, isobornyl (meth) acrylate, dicyclopentyl (meth) acrylate, dicyclopentenyloxyethyl (meth) acrylate, t-butylcyclohexyl (meth) acrylate, and adamantyl (meth) acrylate can be given. One or two or more kinds thereof can be combined.

[0116] From the viewpoint of imparting cohesion to the adhesive sheet, the content of the structural unit derived from the above-mentioned alicyclic monomer (a8) in the (meth) acrylic copolymer (A) is preferably 0.1 to 15% by mass, more preferably 0.5 to 13% by mass, further preferably 1 to 10% by mass, and particularly preferably 2 to 7% by mass, relative to 100% by mass of the total structural units constituting the (meth) acrylic copolymer (A).

[0117] The above-mentioned macromonomer (a9) is a monomer that can easily extend the carbon number of the side chain, for example, to 20 or more when it becomes the (meth) acrylic copolymer (A) by polymerization. By using the macromonomer (a9), the (meth) acrylic copolymer can be made into a graft copolymer having a segment containing a structural unit derived from the macromonomer (a9). By making it into a graft copolymer, it is preferable from the viewpoint of improving the cohesion of the (meth) acrylic copolymer (A) and easily improving the cohesion of the adhesive sheet.

[0118] The properties of the main chain and side chain of the graft copolymer can be changed by the selection of the macromonomer (a9) and the monomers other than the same, and the compounding ratio.

[0119] In the present application, the total content of the monomer M units and the (a1) to (a9) units is not more than 100 mass %.

[0120] As the macromonomer (a9), the backbone component is preferably composed of an acrylic copolymer or a vinyl polymer. As the backbone component of the macromonomer, for example, there can be mentioned the substances exemplified in the monomer M, the alkyl (meth) acrylate monomer (a1) in which the carbon number of the alkyl group is 4 to 30, the vinyl monomer (a6), the alkyl (meth) acrylate monomer (a7) in which the carbon number of the alkyl group is 1 to 3, and the alicyclic monomer (a8).

[0121] Among them, from the viewpoint of being able to produce an adhesive sheet having excellent cohesive force, it is preferable to use an alkyl (meth) acrylate in which the carbon number of the alkyl group is 1 to 8, an alicyclic monomer, a styrene-based aromatic monomer, and the like.

[0122] On the other hand, from the viewpoint of being able to produce an adhesive sheet having moderate cohesive force and excellent flexibility, it is preferable to use an alkyl (meth) acrylate in which the carbon number is 9 to 30.

[0123] They can be used alone or in combination of two or more.

[0124] The macromonomer has a radical polymerizable functional group, or a functional group such as a hydroxyl group, an isocyanate group, an epoxy group, a carboxyl group, an amino group, an amide group, a thiol group, and the like. As the macromonomer, a macromonomer having a radical polymerizable functional group capable of copolymerizing with other monomers is preferable. The radical polymerizable functional group can contain one or two or more, of which one is particularly preferable. When the macromonomer has a functional group, the functional group can contain one or two or more, of which one is particularly preferable.

[0125] In addition, either one of the radical polymerizable functional group and the functional group can be contained, or both can be contained.

[0126] The weight average molecular weight of the macromonomer (a9) is preferably 1000 or more and 40000 or less, more preferably 1500 or more and 20000 or less, and further preferably 2000 or more and 15000 or less.

[0127] The weight average molecular weight of the macromonomer (a9) is a value converted to standard polystyrene by gel permeation chromatography (GPC).

[0128] The macromonomer (a9) can be used a macromonomer produced by a publicly known method, or a commercially available macromonomer (for example, a macromonomer manufactured by Toagosei Co., Ltd., etc.).

[0129] The content of the structural unit derived from the aforementioned macromonomer (a9) in the (meth)acrylic copolymer (A) is preferably 1 to 30% by mass, more preferably 3 to 20% by mass, and further preferably 5 to 15% by mass, relative to 100% by mass of the total structural units constituting the (meth)acrylic copolymer (A). When the aforementioned lower limit value or more, there is a tendency that the phase separation of the segment containing the structural unit derived from the macromonomer (a9) and the segment formed of the other structural units becomes stronger, and the shape retention of the adhesive sheet at the time of non-adhesion becomes more excellent. When the aforementioned upper limit value or less, there is a tendency that the concave-convex followability at the time of adhesion becomes more excellent. The lower limit and the upper limit of the aforementioned content can be arbitrarily combined.

[0130] As the other copolymerizable monomer (a10), for example, methoxydiethylene glycol (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, butoxypolyethylene glycol (meth)acrylate, methoxypolypropylene glycol (meth)acrylate, butoxypolypropylene glycol (meth)acrylate, methoxypolytetramethylene glycol (meth)acrylate, butoxypolytetramethylene glycol (meth)acrylate, methoxypolyoxyethylene polyoxypropylene glycol (meth)acrylate, butoxypolyoxyethylene polyoxypropylene glycol (meth)acrylate, and the like having an alkoxyalkylene glycol skeleton, a heterocycle-containing (meth)acrylate such as tetrahydrofurfuryl (meth)acrylate, and the like can be exemplified. They can be used alone or in combination of two or more.

[0131] The weight average molecular weight (Mw) of the (meth)acrylic copolymer (A) is preferably 50,000 or more and 2,000,000 or less, more preferably 100,000 or more and 1,500,000 or less, and further preferably 300,000 or more and 1,000,000 or less. When the weight average molecular weight of the (meth)acrylic copolymer (A) is the aforementioned lower limit value or more, there is a tendency that the durability after adhesion of the adhesive sheet becomes good. When the weight average molecular weight of the (meth)acrylic copolymer (A) is the aforementioned upper limit value or less, there is a tendency that the moldability at the time of production of the adhesive sheet becomes good. The lower limit and the upper limit of the aforementioned weight average molecular weight can be arbitrarily combined.

[0132] The weight average molecular weight of the (meth)acrylic copolymer (A) is a value converted to a standard polystyrene by gel permeation chromatography (GPC).

[0133] The melt viscosity at 130°C of the (meth)acrylic copolymer (A) is preferably 20 Pa-s or more and 800 Pa-s or less, more preferably 50 Pa-s or more and 600 Pa-s or less, and further preferably 100 Pa-s or more and 500 Pa-s or less. If the melt viscosity at 130°C of the (meth)acrylic copolymer (A) is within the above range, the adhesive composition containing the (meth)acrylic copolymer (A) can be coated by a hot melt method in which the adhesive composition is directly heated and coated. The lower limit and the upper limit of the melt viscosity can be combined arbitrarily.

[0134] The melt viscosity can be measured, for example, using a viscoelasticity measuring device Rheosol-G5000 manufactured by UBM Co., Ltd.

[0135] The method for producing the (meth)acrylic copolymer (A) is not particularly limited, and a publicly known polymerization method can be used.

[0136] As the polymerization method, a publicly known polymerization method such as a solution polymerization method, a suspension polymerization method, and an emulsion polymerization method can be used. In order to be used as an adhesive sheet, a solution polymerization method is preferable.

[0137] The content of the (meth)acrylic copolymer (A) in the adhesive composition for forming the adhesive sheet according to the embodiment is preferably 50 to 99.5% by mass, more preferably 75 to 99% by mass, and further preferably 90 to 98% by mass, relative to 100% by mass of the adhesive composition. The lower limit and the upper limit of the content of the (meth)acrylic copolymer (A) can be combined arbitrarily.

[0138] [Photocurable compound (B)]

[0139] The adhesive composition for forming the adhesive sheet preferably contains the photocurable compound (B) in addition to the (meth)acrylic copolymer (A).

[0140] By containing the photocurable compound (B), the curing efficiency based on active energy rays can be improved, and the cohesion after the active energy ray curing is improved, and the shape stability and the recovery can be improved.

[0141] In the case where the copolymer (A) can form a sufficient crosslinked structure in at least either of the intramolecular and the intermolecular of the (meth)acrylic copolymer (A) by the action of the monomer M unit in the copolymer (A), the photoinitiator (C) described later, or the like, the photocurable compound (B) is not necessarily contained.

[0142] The photocurable compound (B) is a compound having one or more radical polymerizable groups. As the radical polymerizable group, a (meth)acryloyl group is preferable.

[0143] As the photocurable compound (B), for example, monofunctional (meth)acrylates and polyfunctional (meth)acrylates can be cited. From the aspect of being able to efficiently form a crosslinked structure, polyfunctional (meth)acrylates are preferred. As the monofunctional (meth)acrylates, monofunctional (meth)acrylate monomers and monofunctional (meth)acrylate oligomers can be cited. As the polyfunctional (meth)acrylates, polyfunctional (meth)acrylate monomers and polyfunctional (meth)acrylate oligomers can be cited. These can be combined by one or two or more kinds.

[0144] As the polyfunctional (meth)acrylate monomers, for example, 1,4-butanediol di(meth)acrylate, glycerol di(meth)acrylate, neopentyl glycol di(meth)acrylate, glycerol glycidyl ether di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, tricyclodecane dimethanol di(meth)acrylate, tricyclodecane dimethanol di(meth)acrylate, bisphenol A polyethoxy di(meth)acrylate, bisphenol A polypropoxy di(meth)acrylate, bisphenol F polyethoxy di(meth)acrylate, ethylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, trimethylolpropane trioxaethyl (meth)acrylate, ε-caprolactone-modified tris(2-hydroxyethyl) isocyanurate tri(meth)acrylate, pentaerythritol tri(meth)acrylate, propoxylated pentaerythritol tri(meth)acrylate, ethoxylated pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, propoxylated pentaerythritol tetra(meth)acrylate, ethoxylated pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, polytetramethylene glycol di(meth)acrylate, tris(acryloyloxyethyl) isocyanurate, dipentaerythritol hexa(meth)acrylate, dipentaerythritol penta(meth)acrylate, tri-pentaerythritol hexa(meth)acrylate, tri-pentaerythritol penta(meth)acrylate, hydroxypivalic acid neopentyl glycol di(meth)acrylate, di(meth)acrylate of the ε-caprolactone adduct of hydroxypivalic acid neopentyl glycol ester, trimethylolpropane tri(meth)acrylate, trimethylolpropane polyethoxy tri(meth)acrylate, di(trimethylolpropane) tetra(meth)acrylate, and the like can be cited.

[0145] Among these, from the viewpoint of imparting moderate toughness to the cured product, polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, polytetramethylene glycol di(meth)acrylate, and the like having an alkylene glycol skeleton are more preferred.

[0146] The molecular weight of the multifunctional (meth)acrylate monomer is preferably 200 or more, more preferably 300 or more, further preferably 400 or more, and particularly preferably 500 or more, from the viewpoint of imparting moderate softness to the cured product. The upper limit of the molecular weight of the multifunctional (meth)acrylate monomer is usually 3000 or less, and preferably 2000 or less.

[0147] As the multifunctional (meth)acrylate oligomer, for example, a polyester (meth)acrylate, an epoxy (meth)acrylate, a urethane (meth)acrylate, a polyether (meth)acrylate, and the like can be exemplified.

[0148] Among them, a urethane (meth)acrylate is preferred from the viewpoint of imparting moderate toughness to the cured product.

[0149] The above multifunctional urethane (meth)acrylate can be obtained by reacting a polyol, a polyisocyanate, and a (meth)acrylate containing a hydroxyl group.

[0150] The above polyol is only required to be a compound having 2 or more hydroxyl groups, and for example, an aliphatic polyol, an alicyclic polyol, a polyether-based polyol, a polyester-based polyol, a polycarbonate-based polyol, a polyolefin-based polyol, a polybutadiene-based polyol, a polyisoprene-based polyol, a (meth)acrylic-based polyol, a polysiloxane-based polyol, and the like can be exemplified.

[0151] Among them, a polyether-based polyol is preferred from the viewpoint of obtaining excellent softness, and among them, a polyethylene glycol, a polypropylene glycol, and a polytetramethylene glycol are preferred.

[0152] The above polyol compound can be used alone or in combination with two or more.

[0153] As the above polyisocyanate, only a compound having 2 or more isocyanate groups is required, and for example, a toluene diisocyanate, a diphenylmethane diisocyanate, a polyphenylmethane polyisocyanate, a modified diphenylmethane diisocyanate, a xylylene diisocyanate, a tetramethylxylylene diisocyanate, a phenylene diisocyanate, a naphthalene diisocyanate, and the like aromatic-based polyisocyanates, a pentamethylene diisocyanate, a hexamethylene diisocyanate, a trimethylhexamethylene diisocyanate, a lysine diisocyanate, a lysine triisocyanate, and the like aliphatic-based polyisocyanates, a hydrogenated diphenylmethane diisocyanate, a hydrogenated xylylene diisocyanate, an isophorone diisocyanate, a norbornene diisocyanate, and the like alicyclic-based polyisocyanates, or a trimer compound or a multimer compound of these polyisocyanates, a uretonimine-based polyisocyanate, a biuret-based polyisocyanate, a water-dispersible polyisocyanate, and the like can be exemplified.

[0154] Among them, from the viewpoint of stability at the time of urethane formation reaction, diisocyanate is preferred, and aliphatic diisocyanate such as pentamethylene diisocyanate, hexamethylene diisocyanate, trimethylhexamethylene diisocyanate, lysine diisocyanate, hydrogenated diphenylmethane diisocyanate, hydrogenated xylylene diisocyanate, isophorone diisocyanate, norbornene diisocyanate, and alicyclic diisocyanate such as 1,3-bis(isocyanatomethyl)cyclohexane are particularly preferred.

[0155] The above isocyanate can be used alone or in combination with two or more kinds.

[0156] The above hydroxyl group-containing (meth)acrylate is a compound having a hydroxyl group and a (meth)acryloyl group. The number of hydroxyl groups is preferably 1 to 5, and particularly preferably 1.

[0157] As the above hydroxyl group-containing (meth)acrylate, for example, (meth)acrylic acid 2-hydroxyethyl ester, (meth)acrylic acid 2-hydroxypropyl ester, (meth)acrylic acid 2-hydroxybutyl ester, (meth)acrylic acid 4-hydroxybutyl ester, (meth)acrylic acid 6-hydroxyhexyl ester, and the like (meth)acrylic acid hydroxyalkyl esters, 2-hydroxyethyl acryloyl phosphate, 2-(meth)acryloyloxyethyl-2-hydroxypropyl phthalate, caprolactone-modified 2-hydroxyethyl (meth)acrylate, dipropylene glycol mono(meth)acrylate, fatty acid-modified glycidyl (meth)acrylate, polyethylene glycol mono(meth)acrylate, polypropylene glycol mono(meth)acrylate, 2-hydroxy-3-(meth)acryloyloxypropyl (meth)acrylate, dimethylolcyclohexyl mono(meth)acrylate, hydroxy caprolactone (meth)acrylate, and the like hydroxyl group-containing (meth)acrylates containing one (meth)acryloyl group; glycerol di(meth)acrylate, 2-hydroxy-3-acryloyloxypropyl methacrylate, and the like hydroxyl group-containing (meth)acrylates containing two (meth)acryloyl groups; pentaerythritol tri(meth)acrylate, caprolactone-modified pentaerythritol tri(meth)acrylate, oxirane-modified pentaerythritol tri(meth)acrylate, dipentaerythritol penta(meth)acrylate, caprolactone-modified dipentaerythritol penta(meth)acrylate, oxirane-modified dipentaerythritol penta(meth)acrylate, and the like hydroxyl group-containing (meth)acrylates containing three or more (meth)acryloyl groups, and the like can be exemplified. One kind or two or more kinds in combination can be used.

[0158] Among them, a hydroxyl group-containing (meth) acrylate having 2 or less (meth) acryloyl groups is preferable, and a compound having 1 (meth) acryloyl group such as hydroxyethyl (meth) acrylate, hydroxypropyl (meth) acrylate, hydroxybutyl (meth) acrylate, dimethylolcyclohexyl mono(meth) acrylate, hydroxy caprolactone (meth) acrylate, and the like is preferable, and hydroxyethyl (meth) acrylate, hydroxypropyl (meth) acrylate, and hydroxybutyl (meth) acrylate are further preferable.

[0159] From the viewpoint of obtaining a cured product having high toughness when the adhesive composition is cured, in other words, a cured product having moderate flexibility, the molecular weight of the multifunctional (meth) acrylate oligomer is preferably 3000 or more, more preferably 5000 or more, further preferably 8000 or more, and particularly preferably 10000 or more. Note that the upper limit of the molecular weight is usually 100000 or less, and is preferably 50000 or less.

[0160] The monofunctional (meth) acrylate is a compound having 1 (meth) acryloyl group. By including a monofunctional (meth) acrylate, the molecular weight between crosslinking points of the cured product can be increased, and thus it is preferable from the viewpoint of increasing the freedom of movement of the molecular chain and easily obtaining a cured product having excellent stress relaxation properties.

[0161] As the monofunctional (meth) acrylate monomer, a monomer listed as a monomer forming the (meth) acrylate copolymer (A) can be exemplified.

[0162] As the monofunctional (meth) acrylate oligomer, for example, a polyester (meth) acrylate, an epoxy (meth) acrylate, a urethane (meth) acrylate, a polyether (meth) acrylate, and the like can be exemplified. Among them, from the viewpoint of flexibility, a (meth) acrylate oligomer having an alkylene glycol skeleton is preferable.

[0163] As the aforementioned (meth) acrylate oligomer having an alkylene glycol skeleton, for example, a monofunctional (meth) acrylate oligomer represented by the following formula (III) can be exemplified.

[0164] CH2=CR 7 -COO-R 8 -Y-(R 9 O) k -R 10 ···(III)

[0165] In formula (III), R 7 represents a hydrogen atom or a methyl group.

[0166] R 8 represents an alkenyl group having a carbon number of 1 to 20, and can have an ether bond or a cyclic structure in the chain.

[0167] Y represents a bonding group selected from any of a urethane bond, an ester bond, an ether bond, a carbonate bond, an amide bond, and a urea bond. As Y, from the viewpoint of imparting moderate toughness to the cured product, a urethane bond, an amide bond, or a urea bond is preferable, and a urethane bond is particularly preferable.

[0168] R 9 represents an alkylene group which is an ethylene group or a propylene group. Thus, (R 9 O) k may be represented by [(C2H4O) r (C3H6O) s ]. r is an integer of 0 or more, and s is an integer of 0 or more, and r + s = k. In [(C2H4O) r (C3H6O) s ], when the oxyethylene structure (C2H4O) and the oxypropylene structure (C3H6O) coexist, it can be either random or block.

[0169] k represents the number of repeating units of (R 9 O), that is, the total number of repeating units of (C2H4O) r and (C3H6O) s , and is an integer of 1 to 500.

[0170] R 10 represents an alkyl group having a carbon number of 1 to 20, and can have an ether bond or a cyclic structure in the chain.

[0171] For the photocurable compound (B), from the viewpoints of maintaining high recoverability when bent and reducing the storage shear modulus at low temperatures, the glass transition temperature of a polymer obtained by homopolymerization, that is, by polymerizing only the photocurable compound (B), is preferably -20°C or lower, more preferably -25°C or lower, further preferably -30°C or lower, and particularly preferably -40°C or lower. On the other hand, from the viewpoints of shape stability, paste exudation, and the like, the glass transition temperature of the polymer obtained by homopolymerization is preferably -80°C or higher, more preferably -75°C or higher, further preferably -70°C or higher, and particularly preferably -65°C or higher. Specifically, the glass transition temperature is preferably -80°C or higher and -20°C or lower, more preferably -75°C or higher and -25°C or lower, further preferably -70°C or higher and -30°C or lower, and particularly preferably -65°C or higher and -40°C or lower.

[0172] From the viewpoint of maintaining high recovery when bent and reducing the storage shear modulus at low temperatures, the weight average molecular weight (Mw) of the monofunctional (meth)acrylate oligomer is preferably 30,000 or less, more preferably 28,000 or less, and further preferably 25,000 or less. On the other hand, from the viewpoint of preventing a decrease in adhesiveness, the lower limit is preferably 3,000 or more, more preferably 4,000 or more, and further preferably 5,000 or more. Specifically, the weight average molecular weight of the monofunctional (meth)acrylate oligomer is preferably 3,000 or more and 30,000 or less, more preferably 4,000 or more and 28,000 or less, and further preferably 5,000 or more and 25,000 or less.

[0173] The weight average molecular weight of the monofunctional (meth)acrylate oligomer is a value converted to standard polystyrene by gel permeation chromatography (GPC).

[0174] From the viewpoint of being able to impart excellent shape stability and recovery, the content of the photocurable compound (B) in the adhesive composition forming the adhesive sheet is preferably 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, further preferably 1.0 parts by mass or more, and particularly preferably 1.2 parts by mass or more, relative to 100 parts by mass of the (meth)acrylic acid-based copolymer (A). On the other hand, from the viewpoint of ensuring the softness and adhesiveness of the adhesive sheet, the content of the photocurable compound (B) is preferably 50 parts by mass or less, more preferably 30 parts by mass or less, further preferably 25 parts by mass or less, particularly preferably 10 parts by mass or less, and most preferably 5 parts by mass or less, relative to 100 parts by mass of the (meth)acrylic acid-based copolymer (A). The lower limit and the upper limit of the content of the above-described photocurable compound (B) can be arbitrarily combined. Specifically, the content of the above-described photocurable compound (B) is preferably 0.1 parts by mass or more and 50 parts by mass or less, more preferably 0.5 parts by mass or more and 30 parts by mass or less, further preferably 1.0 parts by mass or more and 25 parts by mass or less, particularly preferably 1.2 parts by mass or more and 10 parts by mass or less, and most preferably 1.0 parts by mass or more and 5 parts by mass or less, relative to 100 parts by mass of the (meth)acrylic acid-based copolymer (A).

[0175] [Photoinitiator (C)]

[0176] The adhesive composition forming the adhesive sheet can contain a photoinitiator (C) other than the (meth)acrylic acid-based copolymer (A), as needed. By including the photoinitiator (C) in the adhesive composition, the efficiency of curing based on active energy rays can be further improved.

[0177] The photoinitiator (C) is a compound that generates an active radical species by irradiation of light such as ultraviolet rays, visible rays, and more specifically light having a wavelength of 200 nm to 780 nm.

[0178] The photoinitiator (C) can be appropriately selected from publicly known photoinitiators, and for example, cleavage-type photoinitiators, hydrogen abstraction-type photoinitiators can be mentioned.

[0179] As the cleavage-type photoinitiator, for example, 2,2-dimethoxy-1,2-diphenyl-ethan-1-one, 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenyl-propan-1-one, 1-(4-(2-hydroxyethoxy)phenyl)-2-hydroxy-2-methyl-1-propan-1-one, 2-hydroxy-1-[4-{4-(2-hydroxy-2-methyl-propionyl)benzyl}phenyl]-2-methyl-propan-1-one, oligo(2-hydroxy-2-methyl-1-(4-(1-methylethenyl)phenyl)propanone), 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butan-1-one, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one, 2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholinyl)phenyl]-1-butanone, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, (2,4,6-trimethylbenzoyl)ethoxyphenylphosphine oxide, bis(2,6-dimethoxybenzoyl)2,4,4-trimethylpentylphosphine oxide, and derivatives thereof can be mentioned.

[0180] As the hydrogen abstraction-type photoinitiator, for example, benzophenone, 4-methyl-benzophenone, 2,4,6-trimethylbenzophenone, 4-phenylbenzophenone, 3,3'-dimethyl-4-methoxybenzophenone, 4-(meth)acryloyloxybenzophenone, methyl 2-benzoylbenzoate, 4-[(4-methylphenyl)thio]benzophenone, 4-acryloyloxybenzophenone, 4-acryloyloxyethoxybenzophenone, 4-acryloyloxy-4'-methoxybenzophenone, 4-acryloyloxyethoxy-4'-methoxybenzophenone, 4-acryloyloxy-4'-bromobenzophenone, 4-acryloyloxyethoxy-4'-bromobenzophenone, 4-methacryloyloxybenzophenone, 4-methacryloyloxyethoxybenzophenone, 4-methacryloyloxy-4'-methoxybenzophenone, 4-methacryloyloxyethoxy-4'-methoxybenzophenone, 4-methacryloyloxy-4'-bromobenzophenone, 4-methacryloyloxyethoxy-4'-bromobenzophenone, and the like intermolecular hydrogen abstraction-type photoinitiators; methyl benzoylformate, oxyphenyl acetic acid-2-(2-oxo-2-phenyl-acetyloxy-ethoxy)ethyl ester, oxyphenyl acetic acid-2-(2-hydroxy-ethoxy)ethyl ester, and the like intramolecular hydrogen abstraction-type photoinitiators can be mentioned.

[0181] Either the cleavage-type photoinitiator or the hydrogen abstraction-type photoinitiator can be used, or both can be used in combination. Furthermore, either one of the cleavage-type photoinitiator and the hydrogen abstraction-type photoinitiator can be used alone, or two or more of each can be used in combination.

[0182] The photoinitiator (C) preferably contains a hydrogen abstraction-type photoinitiator. When the photoinitiator (C) contains a hydrogen abstraction-type photoinitiator, a hydrogen abstraction reaction also occurs from the (meth)acrylic copolymer (A), and a crosslinked structure having a large number of crosslinking points can be formed. In addition, in the hydrogen abstraction-type photoinitiator, the intramolecular hydrogen abstraction-type photoinitiator not only can be a hydrogen donor in the system, but also can be a starting point of radical generation itself, and thus is preferred.

[0183] When the adhesive composition contains the photoinitiator (C), the content of the photoinitiator (C) in the adhesive composition forming the adhesive sheet is preferably 0.1 parts by mass or more, more preferably 0.3 parts by mass or more, further preferably 0.5 parts by mass or more, and particularly preferably 1 part by mass or more, relative to 100 parts by mass of the (meth)acrylic copolymer (A), from the viewpoint of improving the curing efficiency, and the viewpoint of the recovery and shape stability of the cured product. On the other hand, from the viewpoint of compatibility or inhibition of bleeding, the content of the photoinitiator (C) is preferably 10 parts by mass or less, more preferably 5 parts by mass or less, further preferably 3 parts by mass or less, and particularly preferably 2 parts by mass or less, relative to 100 parts by mass of the copolymer (A). The lower limit and the upper limit of the content of the above-described photoinitiator (C) can be combined arbitrarily. Specifically, the content of the photoinitiator (C) is preferably 0.1 parts by mass or more and 10 parts by mass or less, more preferably 0.3 parts by mass or more and 5 parts by mass or less, further preferably 0.5 parts by mass or more and 3 parts by mass or less, and particularly preferably 1 part by mass or more and 2 parts by mass or less, relative to 100 parts by mass of the (meth)acrylic copolymer (A).

[0184] [Other Components]

[0185] The adhesive composition forming the adhesive sheet can further contain other components in addition to the (meth)acrylic copolymer (A), the photocurable compound (B), and the photoinitiator (C), as needed. As the other components, various additives such as a silane coupling agent, a tackifying resin, a plasticizer, an antioxidant, a light stabilizer, a metal deactivator, an anti-aging agent, a moisture absorbent, a polymerization inhibitor, an ultraviolet absorber, a rust preventive, an inorganic particle, a sensitizer, a pigment, and the like can be exemplified. The content of the additive is typically preferably set in a manner that does not adversely affect the curing of the adhesive sheet, or in a manner that does not adversely affect the physical properties of the adhesive sheet.

[0186] [Method for Manufacturing Adhesive Sheet]

[0187] The method for manufacturing the adhesive sheet of the embodiment is not particularly limited.

[0188] For example, a prescribed amount of the (meth)acrylic copolymer (A), a photo-curable compound (B) used as necessary, a photoinitiator (C), and an additive or the like are mixed, an adhesive composition is prepared, the adhesive composition is shaped into a sheet, it is crosslinked and cured by a radical reaction, and processing is appropriately performed as necessary, whereby an adhesive sheet of the embodiment can be obtained. Alternatively, an adhesive composition can be prepared as described above, it can be applied to an image display device constituent member, and the adhesive composition can be cured, whereby an adhesive sheet of the embodiment can be formed.

[0189] As a method of mixing the components, for example, a method using a single-screw extruder, a twin-screw extruder, a planetary mixer, a twin-screw mixer, a pressurized kneader, or the like can be given.

[0190] As a method of shaping the adhesive composition into a sheet, for example, a wet lamination method, a dry lamination method, an extrusion casting method using a T-die, an extrusion lamination method, a calendering method, a blow molding method, an injection molding method, a liquid injection curing method can be given.

[0191] An adhesive sheet of the embodiment can also be formed by dissolving an adhesive composition in an appropriate solvent, applying it using various application methods, and irradiating it with active energy rays.

[0192] Curing of the adhesive composition can be performed by irradiation with active energy rays. For example, by irradiating a shaped body of the adhesive composition, for example, a shaped body obtained by shaping the adhesive composition into a sheet, an adhesive sheet of the embodiment can be manufactured. Note that, in addition to the irradiation with active energy rays, further heating can be performed to achieve curing.

[0193] The irradiation energy, irradiation time, irradiation method, and the like of the active energy rays are not particularly limited, as long as a radical derived from the structural unit from the monomer M is generated by activation of the photoinitiator to form a crosslinked structure.

[0194] As the active energy rays for irradiation, for example, ionizing radiation such as α-rays, β-rays, γ-rays, neutron rays, electron beams, ultraviolet rays, visible rays can be given. Among these, from the viewpoint of suppressing damage to the image display device constituent member and controlling the reaction, ultraviolet rays are preferred.

[0195] As the light source at the time of irradiation with active energy rays, for example, a high-pressure mercury lamp, a metal halide lamp, a xenon lamp, a halogen lamp, an LED lamp, a fluorescent lamp can be given.

[0196] From the viewpoint of efficient curing, the irradiation amount of the active energy rays is preferably 6000 mJ / cm 2 More preferably, it is 5000 mJ / cm2 Further preferably, 4000 mJ / cm 2 Particularly preferably, 3000 mJ / cm 2 From the viewpoint of sufficient curing, the irradiation amount of the active energy ray is preferably 100 mJ / cm 2 More preferably, 250 mJ / cm 2 Further preferably, 500 mJ / cm 2 Particularly preferably, 1000 mJ / cm 2 The lower limit and the upper limit of the irradiation amount of the active energy ray described above can be arbitrarily combined.

[0197] [Properties of the Adhesive Sheet]

[0198] Hereinafter, the properties of the adhesive sheet of one example of the embodiment will be described.

[0199] The adhesive sheet of one example of the embodiment satisfies the following requirement (1).

[0200] (1) The storage modulus at -20°C (G'(-20°C)) obtained by dynamic viscoelasticity measurement in a shear mode at a frequency of 1 Hz is 10 kPa or more and 1000 kPa or less.

[0201] The adhesive sheet satisfying the requirement (1) is also soft at low temperatures, and is excellent in flexibility. For example, even when repeated folding operations are performed at a low temperature of -20°C, cracks or breakage are less likely to occur in the member of the adherend as the adhesive sheet.

[0202] From the viewpoint of shape retention of the adhesive sheet when not attached, the G'(-20°C) of the requirement (1) is preferably 30 kPa or more, more preferably 50 kPa or more, and further preferably 100 kPa or more. On the other hand, from the viewpoint of softness of the adhesive sheet in a low-temperature environment, the G'(-20°C) of the requirement (1) is preferably 800 kPa or less, more preferably 600 kPa or less, further preferably 400 kPa or less, and particularly preferably 300 kPa or less. The lower limit and the upper limit of the G'(-20°C) of the requirement (1) can be arbitrarily combined. Specifically, it is preferably 30 kPa or more and 800 kPa or less, more preferably 50 kPa or more and 600 kPa or less, further preferably 100 kPa or more and 400 kPa or less, and particularly preferably 100 kPa or more and 300 kPa or less.

[0203] In order to accurately measure the storage shear modulus G', it is necessary to avoid variation in the measurement results due to the influence of the measurement jig caused by insufficient thickness of the adhesive sheet. The requirement (1) is a value measured after the thickness is adjusted to the range of 0.7 to 1.0 mm, and thus the storage shear modulus G' can be accurately measured without being influenced by the measurement jig.

[0204] Note that the aforementioned "thickness of 0.7 to 1.0 mm" means that, in the case where the thickness of the adhesive sheet serving as a measurement sample is not within the range, the thickness of the measurement sample is adjusted to the range by overlapping several sheets or the like. The same applies to the case where the thickness of the measurement sample is specified in other tests.

[0205] The measurement of G' (-20°C) of the requirement (1) is performed, for example, as follows.

[0206] After the adhesive sheet is repeatedly laminated to adjust the thickness to 0.7 to 1.0 mm (for example, 0.8 mm), a sample in the shape of a circle having a diameter of 8 mm is punched out. For the obtained sample, a dynamic viscoelasticity measurement is performed using a rheometer under the conditions of a measurement jig: a 8 mm diameter parallel plate, a frequency: 1 Hz, a measurement temperature: -50°C to 150°C, a temperature increase rate: 5°C / minute, and the value of the storage shear modulus G' at -20°C is read.

[0207] As a method of adjusting G' (-20°C) of the requirement (1) in the adhesive sheet to the aforementioned range, for example, a method of adjusting the composition, the molecular weight of the (meth)acrylic copolymer (A), the kind, and the amount of addition of the photocurable compound (B) can be exemplified. However, it is not limited to these methods.

[0208] The adhesive sheet of one example of the embodiment also satisfies the following requirement (2).

[0209] (2) The maximum strain value (γ max ) at the time of application of a stress of 2 kPa for 600 seconds at 60°C is less than 80%.

[0210] The adhesive sheet satisfying the requirement (2) is excellent in shape stability.

[0211] The adhesive sheet used in a flexible image display device particularly requires softness, but the conventional adhesive sheet has a tendency that the softer it is, the worse the shape stability is. However, if it is an adhesive sheet satisfying both the aforementioned requirement (1) and requirement (2), it is possible to produce an adhesive sheet which is soft and excellent in shape stability.

[0212] From the viewpoint of shape stability, the maximum strain value (γ max ) of the requirement (2) is preferably 75% or less, more preferably 70% or less, further preferably 60% or less, particularly preferably 50% or less, and most preferably 40% or less.

[0213] On the other hand, the maximum strain value (γ max ) is usually 0% or more, and from the viewpoint of excellent following of unevenness when unevenness exists on the surface of an adherend, the maximum strain value (γ max) is preferably 1% or more, more preferably 2% or more, and further preferably 3% or more.

[0214] The maximum strain value (γ max ) can be combined arbitrarily. Specifically, the maximum strain value (γ max ) is preferably from 1% to 75%, more preferably from 2% to 70%, further preferably from 3% to 60%, particularly preferably from 5% to 50%, and most preferably from 8% to 40%.

[0215] The maximum strain value (γ max ) is measured, for example, as follows.

[0216] After repeatedly laminating the adhesive sheets to adjust the thickness to 0.7-1.0 mm, circular samples with a diameter of 8 mm were punched out. The obtained samples were subjected to a rheometer and the strain value after applying a pressure of 2 kPa at 60°C for 600 seconds was read as the maximum strain value (γ max ).

[0217] As the maximum strain value (γ max ) within the above range, for example, the composition and molecular weight of the (meth)acrylic copolymer (A), the type and amount of the photocurable compound (B), and the amount of active energy ray irradiation can be adjusted. However, the present invention is not limited to these methods.

[0218] The pressure-sensitive adhesive sheet according to one embodiment preferably further satisfies the following requirement (3).

[0219] (3) The storage shear modulus at 30° C. (G′(30° C.)) obtained by dynamic viscoelasticity measurement in a shear mode at a frequency of 1 Hz is 1000 kPa or less.

[0220] The adhesive sheet satisfying requirement (3) is soft, and for example, even in the case where unevenness is present on the adherent surface, the following property is excellent: the unevenness is followed. From this viewpoint, the G' (30°C) of requirement (3) is preferably 500 kPa or less, more preferably 200 kPa or less, further preferably 100 kPa or less, particularly preferably 50 kPa or less, most preferably 40 kPa or less. On the other hand, from the viewpoint of handleability and shape stability, the G' (30°C) of requirement (3) is preferably 1 kPa or more, more preferably 2 kPa or more, further preferably 5 kPa or more, particularly preferably 10 kPa or more. The upper limit and the lower limit of the G' (30°C) of the above requirement (3) can be combined arbitrarily. Specifically, it is preferably 1 kPa or more and 500 kPa or less, more preferably 2 kPa or more and 200 kPa or less, further preferably 5 kPa or more and 100 kPa or less, particularly preferably 10 kPa or more and 50 kPa or less, most preferably 15 kPa or more and 40 kPa or less.

[0221] The adhesive sheet of one example of the embodiments preferably further satisfies the following requirement (4).

[0222] (4) The storage shear modulus at 80°C (G' (80°C)) obtained by dynamic viscoelasticity measurement in a shear mode at a frequency of 1 Hz is 10 kPa or more.

[0223] The adhesive sheet satisfying requirement (4) is excellent in shape stability and durability at high temperature. From this viewpoint, the G' (80°C) of requirement (4) is preferably 20 kPa or more, more preferably 30 kPa or more, further preferably 40 kPa or more, particularly preferably 50 kPa or more, most preferably 60 kPa or more. On the other hand, from the viewpoint of adhesiveness and stress relaxation, the G' (80°C) of requirement (4) is preferably 500 kPa or less, more preferably 400 kPa or less, further preferably 300 kPa or less, particularly preferably 200 kPa or less. The lower limit and the upper limit of the G' (80°C) of the above requirement (4) can be combined arbitrarily. Specifically, the G' (80°C) of requirement (4) is preferably 20 kPa or more and 500 kPa or less, more preferably 30 kPa or more and 400 kPa or less, further preferably 40 kPa or more and 300 kPa or less, particularly preferably 50 kPa or more and 200 kPa or less, most preferably 60 kPa or more.

[0224] The measurement method of the G' (30°C) in requirement (3) and the measurement method of the G' (80°C) in requirement (4) are the same as the measurement of the G' (-20°C) of requirement (1), except that the values of the storage shear modulus (G') at 30°C and 80°C are read.

[0225] Examples of methods for adjusting the storage shear modulus G' of the PSA sheet to the above range include adjusting the composition and molecular weight of the (meth)acrylic copolymer (A); adjusting the type and amount of the photocurable compound (B) and the photoinitiator (C); and adjusting the dose of active energy rays. However, these methods are not limiting.

[0226] The pressure-sensitive adhesive sheet according to one embodiment preferably further satisfies the following requirement (5).

[0227] (5) The glass transition temperature (Tg) defined by the maximum value of Tan δ obtained by dynamic viscoelasticity measurement in a shear mode at a frequency of 1 Hz is -20°C or lower.

[0228] The PSA sheet satisfying requirement (5) has excellent flexibility.

[0229] From the viewpoint of obtaining excellent flexibility, the Tg of the requirement (5) is preferably -25°C or lower, more preferably -28°C or lower, further preferably -30°C or lower, and particularly preferably -35°C or lower. On the other hand, the lower limit is usually -80°C. Specifically, the Tg of the requirement (5) is preferably -80°C or higher and -20°C or lower, more preferably -80°C or higher and -25°C or lower, further preferably -75°C or higher and -28°C or lower, particularly preferably -70°C or higher and -30°C or lower, and most preferably -65°C or higher and -35°C or lower.

[0230] The measurement of Tg in the requirement (5) is carried out, for example, as follows.

[0231] After repeatedly laminating the PSA sheets to a thickness of 0.7 to 1.0 mm (e.g., 0.8 mm), circular samples with a diameter of 8 mm were punched out. The resulting samples were subjected to dynamic viscoelasticity measurements using a rheometer with an 8 mm diameter parallel plate, a frequency of 1 Hz, a measurement temperature of -50°C to 150°C, and a heating rate of 5°C / minute. The tan delta value was determined by reading the temperature at which it reached a maximum from the resulting dynamic viscoelasticity spectrum.

[0232] Examples of methods for adjusting the Tg of requirement (5) to the above range include, for example, adjusting the composition and molecular weight of the (meth)acrylic copolymer (A), adjusting the type and amount of the photocurable compound (B) and the photoinitiator (C), and adjusting the dose of active energy rays. However, the present invention is not limited to these methods.

[0233] The pressure-sensitive adhesive sheet according to one embodiment preferably further satisfies the following requirement (6).

[0234] (6) Maximum strain value (γ) when a stress of 2 kPa is applied for 600 seconds at 60°Cmax ) and the residual strain value (γ min ) 600 seconds after the stress is removed thereafter is 60% or more.

[0235] Recovery rate (%) = 〔(γ max - γ min ) / γ max 〕 x 100

[0236] The adhesive sheet satisfying the requirement (6) is excellent in recovery at the time of bending.

[0237] The recovery rate of the requirement (6) is preferably 70% or more, more preferably 80% or more, further preferably 85% or more, particularly preferably 87% or more, and most preferably 90% or more, from the viewpoint of obtaining an adhesive sheet excellent in recovery at the time of bending. On the other hand, the upper limit is usually 100%, and the recovery rate of the requirement (6) is preferably 99% or less, and more preferably 98% or less, from the viewpoint of improvement in adhesive strength. The lower limit and the upper limit of the recovery rate of the above requirement (6) can be combined arbitrarily. Specifically, the recovery rate is preferably 60% or more and 100% or less, more preferably 70% or more and 99% or less, further preferably 80% or more and 98% or less, further preferably 85% or more and 98% or less, particularly preferably 87% or more and 98% or less, and most preferably 90% or more and 98% or less.

[0238] The measurement of the recovery rate of the requirement (6) is carried out, for example, as follows.

[0239] After the adhesive sheet is repeatedly laminated to adjust the thickness to 0.7 to 1.0 mm, a sample in the shape of a circle having a diameter of 8 mm is punched out. For the obtained sample, using a rheometer, the strain (γ max ) 600 seconds after the application of a pressure of 2 kPa at 60°C and the strain (γ min ) 600 seconds after the stress is removed thereafter are measured. The obtained values are substituted into the following formula to calculate the recovery rate.

[0240] Recovery rate (%) = 〔(γ max - γ min ) / γ max 〕 x 100

[0241] As a method of adjusting the recovery rate of the requirement (6) to the above range, for example, in addition to the method of adjusting the composition, the molecular weight of the (meth)acrylic copolymer (A), the method of adjusting the kind, the amount of addition of the photocurable compound (B) and the photoinitiator (C), the method of adjusting the amount of irradiation of active energy rays can be exemplified. However, it is not limited to these methods.

[0242] The adhesive sheet of one example of the embodiment preferably further satisfies the following requirement (7).

[0243] (7) The gel fraction is 30% or more.

[0244] The adhesive sheet satisfying the requirement (7) is excellent in cohesive force.

[0245] The gel fraction of the requirement (7) is preferably 35% or more, more preferably 40% or more, and further preferably 45% or more from the viewpoint of improving the cohesive force. On the other hand, the gel fraction of the requirement (7) is preferably 98% or less, more preferably 95% or less, and further preferably 92% or less from the viewpoint of obtaining the adhesive force. The lower limit and the upper limit of the gel fraction of the above requirement (7) can be combined arbitrarily. Specifically, the gel fraction is preferably 30% or more and 98% or less, more preferably 35% or more and 98% or less, further preferably 40% or more and 95% or less, and particularly preferably 45% or more and 92% or less.

[0246] The gel fraction of the requirement (7) is measured, for example, as follows.

[0247] The adhesive sheet weighed in advance is wrapped with a 150-mesh SUS-made metal mesh, and immersed in ethyl acetate at 23°C for 24 hours. Then, it is dried at 70°C for 4.5 hours, and the mass of the adhesive before and after the ethyl acetate immersion is measured, respectively, and the difference between the two masses is taken as the mass of the insoluble adhesive remaining in the metal mesh (post-immersion mass). The percentage of the mass of the insoluble adhesive remaining in the metal mesh (post-immersion mass) with respect to the mass of the adhesive before the ethyl acetate immersion (pre-immersion mass) is calculated as the gel fraction (%) of the requirement (6).

[0248] As a method of adjusting the gel fraction of the requirement (7) to the above range, for example, a method of adjusting the composition, the molecular weight of the (meth)acrylic copolymer (A), the kind, the amount of addition of the photo-curable compound (B), and a method of adjusting the amount of active energy ray irradiation can be exemplified. However, it is not limited to these methods.

[0249] The adhesive sheet of the embodiment preferably further satisfies the requirement of the following (8).

[0250] (8) The adhesive force to the surface of the aforementioned polyester film at 23°C, 50% RH, a peeling angle of 180°, a peeling speed of 300 mm / minute when the adhesive sheet is attached to the polyester film is 0.5 N / cm or more.

[0251] The adhesive sheet satisfying the requirement (8) is excellent in adhesive property, and even if a laminate obtained by attaching an adherend such as a component constituting an image display device is bent, delamination is not easily caused, and thus the durability is excellent.

[0252] The adhesive force of the requirement (8) is preferably 1 N / cm or more, more preferably 2 N / cm or more, further preferably 3 N / cm or more, and particularly preferably 4 N / cm or more, from the viewpoint of the adhesiveness of the adhesive sheet. The upper limit of the adhesive force of the requirement (8) is not particularly limited, and can be, for example, 20 N / cm or less. Specifically, the adhesive force of the requirement (8) is preferably 1 N / cm or more and 20 N / cm or less, more preferably 2 N / cm or more and 20 N / cm or less, further preferably 3 N / cm or more and 18 N / cm or less, and particularly preferably 4 N / cm or more and 18 N / cm or less.

[0253] The adhesive force of the requirement (8) is measured, for example, as follows.

[0254] A polyester film serving as a backing film of the adhesive sheet was attached to a sodium calcium glass, and a test piece was cut out in a long strip shape of 10 mm in width and 150 mm in length. A pressure vessel treatment (60°C, 0.2 MPa in gauge pressure, 20 minutes) was performed on the polyester film to which the test piece was attached, to produce an adhesive force measurement sample. The adhesive force measurement sample thus obtained was peeled from the polyester film attached to the sodium calcium glass at a peeling angle of 180° and a peeling speed of 300 mm / minute in an environment of 23°C and 50% RH, and the tensile strength (N / cm) was measured with a load cell as the adhesive force.

[0255] The adhesive sheet according to the embodiment preferably further satisfies the requirement of the following (9).

[0256] (9) The adhesive force to the surface of a polyester film when the adhesive sheet is attached to the polyester film is 0.1 N / cm or more at 60°C, 10% RH, a peeling angle of 180°, and a peeling speed of 300 mm / minute.

[0257] The adhesive sheet satisfying the requirement (9) is excellent in durability at high temperatures.

[0258] The adhesive force of the requirement (9) is preferably 0.2 N / cm or more, more preferably 0.3 N / cm or more, further preferably 0.4 N / cm or more, and particularly preferably 0.5 N / cm or more, from the viewpoint of the durability of the adhesive sheet. The upper limit of the adhesive force of the requirement (9) is not particularly limited, and can be, for example, 20 N / cm or less. Specifically, the adhesive force of the requirement (9) is preferably 0.2 N / cm or more and 20 N / cm or less, more preferably 0.3 N / cm or more and 20 N / cm or less, further preferably 0.4 N / cm or more and 18 N / cm or less, and particularly preferably 0.5 N / cm or more and 18 N / cm or less.

[0259] The adhesion of the requirement (9) was measured in the same manner as the adhesion of the requirement (8), except that the test environment was set to 60°C, 10% RH.

[0260] As a method of adjusting the adhesion, for example, a method of adjusting the composition, the molecular weight of the (meth)acrylic copolymer (A), a method of adjusting the kind, the added amount of the photocurable compound (B) and the photoinitiator (C), and a method of adjusting the amount of the active energy ray irradiation can be exemplified. However, the methods are not limited to these.

[0261] The adhesive sheet of the embodiment preferably further satisfies the requirement of the following (10).

[0262] (10) The total light transmittance is 80% or more.

[0263] The adhesive sheet satisfying the requirement (10) is excellent in transparency, and is useful in applications requiring transparency such as image display devices.

[0264] The total light transmittance of the requirement (10) is preferably 85% or more, and more preferably 90% or more. The higher the total light transmittance of the requirement (10) is, the more preferable it is, and the upper limit is not particularly limited. Specifically, the total light transmittance of the requirement (10) is preferably 85% or more and 100% or less, and more preferably 90% or more and 100% or less.

[0265] The total light transmittance of the requirement (10) is measured in accordance with the standard of JIS-K 7361-1 (ISO-13468-1).

[0266] The adhesive sheet of the embodiment preferably further satisfies the requirement of the following (11).

[0267] (11) The haze is 5% or less.

[0268] The adhesive sheet satisfying the requirement (11) is excellent in transparency, and is useful in applications requiring transparency such as image display devices.

[0269] The haze of the requirement (11) is preferably 4% or less, more preferably 2% or less, and further preferably 1% or less. The lower the haze of the requirement (11) is, the more preferable it is, and the lower limit is not particularly limited. Specifically, the haze of the requirement (11) is preferably 0% or more and 4% or less, more preferably 0% or more and 2% or less, and further preferably 0% or more and 1% or less.

[0270] The haze of the requirement (11) is measured in accordance with the standard of JIS-K 7136 (ISO-14782).

[0271] As a method of adjusting the total light transmittance as the adjustment requirement (10) and the haze as the requirement (11), for example, the composition of the (meth)acrylate copolymer can be adjusted, or a non-colored photoinitiator can be used, or a coloring agent can be omitted. Alternatively, an antioxidant can be used to suppress deterioration of the coloring over time accompanying heating. However, the method is not limited to these.

[0272] The adhesive sheet of the embodiment can be composed of a single layer or multiple layers. In the case of multiple layers, the multiple layers are each formed of an adhesive composition containing the (meth)acrylic copolymer (A).

[0273] The thickness of the adhesive sheet of the embodiment is preferably 5 μm or greater, more preferably 10 μm or greater, further preferably 15 μm or greater, and particularly preferably 20 μm or greater, from the viewpoint of good workability and easy achievement of excellent concave-convex following properties. The thickness of the adhesive sheet of the embodiment is preferably 100 μm or less, more preferably 80 μm or less, further preferably 70 μm or less, and particularly preferably 60 μm or less, from the viewpoint of easy relaxation of stress at the time of bending, easy bending, and easy thinning of a flexible image display device to which the adhesive sheet is applied. The lower limit and the upper limit of the thickness of the aforementioned adhesive sheet can be combined arbitrarily. Specifically, the thickness of the adhesive sheet is preferably 5 μm or greater and 100 μm or less, more preferably 10 μm or greater and 80 μm or less, further preferably 15 μm or greater and 70 μm or less, and particularly preferably 20 μm or greater and 60 μm or less.

[0274] <Adhesive sheet with release film>

[0275] Another embodiment of the present application relates to an adhesive sheet with a release film.

[0276] The adhesive sheet of the embodiment preferably has a release film laminated on at least one surface thereof before attachment, and more preferably has a release film laminated on both surfaces thereof.

[0277] In the case where a release film is provided on both surfaces of the adhesive sheet, it is preferable to produce a laminate in which a light release film having relatively low release force and a heavy release film having relatively high release force are laminated. In the case of using an adhesive sheet with a release film provided on both surfaces, first, one release film (light release film) is peeled off to expose one surface of the adhesive sheet, and attachment to an image display device constituent member (as a first member) is performed. Then, the other release film (heavy release film) is peeled off to expose the other surface of the adhesive sheet, and an image display device constituent member (as a second member) is attached to the exposed surface.

[0278] As the release film, for example, a polyester film, a polyolefin film, a polycarbonate film, a polystyrene film, an acrylic film, a cellulose triacetate film, and a fluororesin film can be mentioned. Among them, a polyester film and a polyolefin film are preferable, and a polyester film is more preferable.

[0279] In addition, from the viewpoint that the adhesive sheet after irradiation with active energy rays is also easily peeled, the release film is preferably a film having a peeling force of 0.1 N / cm or less as measured at a peeling angle of 180° and a peeling speed of 300 mm / min.

[0280] From the viewpoint of processability and operability, the thickness of the release film is preferably 25 μm or more and 500 μm or less, more preferably 38 μm or more and 250 μm or less, and further preferably 50 μm or more and 200 μm or less. The lower limit and the upper limit of the thickness of the release film can be combined arbitrarily.

[0281]

[0282] Another embodiment of the present application relates to a laminate for image display devices.

[0283] In the laminate for image display devices of the embodiment, two image display device-constituting members are laminated by means of the adhesive sheet of the present application.

[0284] The adhesive sheet of the present application is excellent in softness, and thus is excellent in concave-convex followability, and can be deformed to follow even if the surface of the image display device-constituting member has a step, and absorb the step and adhere the two image display device-constituting members.

[0285] As the image display device-constituting member constituting the laminate for image display devices, for example, a flat panel image display device-constituting member, a flexible image display device-constituting member can be cited. As such an image display device-constituting member, for example, a flexible display such as a liquid crystal display, an organic electroluminescence (EL) display, a cover glass (cover film), a polarizing plate, a polarizing sheet, a phase difference film, a barrier film, a viewing angle compensation film, a brightness enhancement film, a contrast improvement film, a diffusion film, a semi-transmissive reflective film, an electrode film, a transparent conductive film, a metal mesh film, a touch sensor film, a light emitting element, a PSA, a color filter, a flexible printed circuit board, and the like can be cited. Any one of them or a combination of two of them can be used. As an example of the combination, a combination of a flexible display and another image display device-constituting member, a combination of a cover glass and another image display device-constituting member can be cited.

[0286] The material of the image display device-constituting member is not particularly limited. For example, a resin sheet in which a urethane resin, a cyclic olefin resin, a cellulose triacetate resin, a (meth)acrylate resin, an epoxy resin, a polyimide resin, a polyester resin, or the like is used as a main component, a film glass, a metal, and the like can be cited.

[0287] ​Note that the flexible image display device constituting member refers to a member that can be bent, and refers to a member used in an image display device having a curved shape, a member that can be repeatedly bent. A member that can be fixed in a bent shape having a radius of curvature of 25 mm or more is particularly preferred, and in particular, a member that can withstand bending with a radius of curvature of less than 25 mm, and more preferably a radius of curvature of less than 3 mm is particularly preferred.

[0288] As the material of the member, a resin sheet in which at least one resin selected from the group consisting of urethane resin, cyclic olefin resin, cellulose triacetate resin, (meth)acrylate resin, epoxy resin, polyimide resin, polyester resin, and the like is used as a main component is preferred. As the resin, at least one selected from the group consisting of polyimide resin, polyester resin, and cyclic olefin resin is preferred, and among them, polyester resin, and in particular, polyethylene naphthalate (PEN), polybutylene terephthalate (PBT), and polyethylene terephthalate (PET) resin are preferred.

[0289] Here, the "main component" refers to a component having the largest mass ratio among the components constituting the resin sheet. The main component is preferably 50% by mass or more, more preferably 55% by mass or more, and further preferably 60% by mass or more, with respect to the mass of the resin sheet.

[0290] As described above, the image display device member can have steps on the surface. For example, on the contact surface of the image display device constituting member and the adhesive sheet, various irregularities can exist by wiring, printing, pattern development, surface treatment, embossing, and the like.

[0291] The height difference of the image display device constituting member is preferably 2 μm or more, more preferably 3 μm or more, and further preferably 4 μm or more, and on the other hand, is preferably 10 μm or less, more preferably 8 μm or less, and further preferably 7 μm or less, and particularly preferably 6 μm or less. The lower limit and the upper limit of the height difference of the steps described above can be combined arbitrarily. Specifically, the height difference is preferably 2 μm or more and 8 μm or less, more preferably 3 μm or more and 7 μm or less, and further preferably 4 μm or more and 6 μm or less.

[0292] The steps on the contact surface of the image display device constituting member and the adhesive sheet can be, for example, irregularities having a height difference of 2 μm to 10 μm and being provided at intervals of 10 mm or less.

[0293] The thickness of the image display device laminate of the embodiment is preferably 0.02 mm or more, more preferably 0.03 mm or more, and further preferably 0.05 mm or more from the viewpoint of operability. The thickness of the image display device laminate of the embodiment is preferably 1.0 mm or less, more preferably 0.7 mm or less, and further preferably 0.5 mm or less from the viewpoint of thinness of the laminate. The lower limit and the upper limit of the thickness of the image display device laminate described above can be combined arbitrarily. Specifically, the thickness described above is preferably 0.02 mm or more and 1.0 mm or less, more preferably 0.03 mm or more and 0.7 mm or less, and further preferably 0.05 mm or more and 0.5 mm or less.

[0294] The method for producing the image display device laminate of the embodiment is not particularly limited.

[0295] For example, the adhesive composition can be applied to the image display device constituent member to form an adhesive sheet, or an adhesive sheet with a release film can be formed in advance and then attached to the image display device constituent member.

[0296] The method for attaching the adhesive sheet to the surface of the image display device constituent member having a step is not particularly limited, and known methods such as roll attachment, press attachment using parallel plates, diaphragm attachment, and the like can be used. As the attachment environment, either of atmospheric attachment in which attachment is performed under normal pressure and vacuum attachment in which attachment is performed under reduced pressure can be used.

[0297] When the adhesive sheet is attached, a heating treatment can be performed. The heating temperature at the time of the heating treatment is preferably 40°C or higher and 100°C or lower, more preferably 50°C or higher and 90°C or lower, and further preferably 55°C or higher and 85°C or lower.

[0298] When the adhesive sheet is attached, a press pressure can be applied to the laminate together with the heating treatment.

[0299] In addition, when the adhesive sheet is attached, a pressurization treatment using an autoclave can be performed together with the heating treatment.

[0300] <Flexible image display device>

[0301] Another embodiment of the present application relates to a flexible image display device.

[0302] The "flexible image display device" refers to an image display device that does not leave a bending trace even when bending, bending operation, and winding operation are repeated, and that can quickly return to the state before the operation when the bending state, the bending state, and the winding state are released, and that can display an image without strain.

[0303] The flexible image display device of the embodiment is provided with the image display device laminate of the present application. In the flexible image display device of the embodiment, the image display device laminate is disposed on the side opposite to the viewing side of the image display panel, i.e., the light source side.

[0304] In the flexible image display device of the embodiment, other members can be further laminated between the image display panel and the image display device laminate of the present application, or on the side of the image display device laminate opposite to the image display panel. As the other members, the same members as exemplified in the description of the image display device laminate of the embodiment can be exemplified.

[0305] In the flexible image display device of the embodiment, even if a step having a height difference of 2 μm or more exists in the contact surface of the image display device constituent member with the adhesive sheet, the adhesive sheet follows the step and absorbs the step, and the generation of bubbles is suppressed. In addition, even if bending, folding, or winding operations are performed in a low-temperature environment, delamination or breakage is suppressed.

[0306] <Photocurable adhesive sheet>

[0307] Another embodiment of the present application relates to a photocurable adhesive sheet.

[0308] The photocurable adhesive sheet of the embodiment is a photocurable adhesive sheet before irradiation of light to the adhesive sheet, and is formed from an adhesive composition containing a (meth)acrylic copolymer (A).

[0309] Further, the photocurable adhesive sheet of the present application is a photocurable adhesive sheet in which the above-described (meth)acrylic copolymer (A) has a structural unit derived from a monomer M that generates an active species that is excited by irradiation of active energy rays.

[0310] Element (1'): the storage shear modulus at -20°C (G'(-20°C)) obtained by dynamic viscoelasticity measurement in a shear mode at a frequency of 1 Hz is 10 kPa or more and 1000 kPa or less when the above-described photocurable adhesive sheet is irradiated with active energy rays having a wavelength of 365 nm at an arbitrary irradiation amount in the range of 1000 to 5000 mJ / cm 2 Element (2'): the maximum strain value (γmax) at the time of application of a stress of 2 kPa for 600 seconds at 60°C is less than 80% when the above-described photocurable adhesive sheet is irradiated with active energy rays having a wavelength of 365 nm at an arbitrary irradiation amount in the range of 1000 to 5000 mJ / cm

[0311] Element (2'): the maximum strain value (γmax) at the time of application of a stress of 2 kPa for 600 seconds at 60°C is less than 80% when the above-described photocurable adhesive sheet is irradiated with active energy rays having a wavelength of 365 nm at an arbitrary irradiation amount in the range of 1000 to 5000 mJ / cm 2 Element (2'): the maximum strain value (γmax) at the time of application of a stress of 2 kPa for 600 seconds at 60°C is less than 80% when the above-described photocurable adhesive sheet is irradiated with active energy rays having a wavelength of 365 nm at an arbitrary irradiation amount in the range of 1000 to 5000 mJ / cm

[0312] Further, the details of the photocurable adhesive sheet are the same as those described in the adhesive sheet.

[0313] <Adhesive composition>

[0314] Still another embodiment of the present application relates to an adhesive composition.

[0315] The adhesive composition of the embodiments for forming a photocurable adhesive sheet and an adhesive sheet contains a (meth)acrylic copolymer (A).

[0316] The adhesive composition is the same as that described in the adhesive sheet.

[0317] In addition, the present application is not limited to the above-described embodiments. Within the scope of the gist of the present application, the constituent elements in the above-described embodiments can be appropriately replaced with known constituent elements, and the above-described modifications can also be appropriately combined.

[0318] Examples

[0319] Hereinafter, the present application will be further explained in detail by examples and comparative examples. However, the present application is not limited by any of these examples. In addition, "parts" in the examples refer to "mass parts".

[0320] The measurement and evaluation in the examples were performed by the following methods.

[0321] (Molecular weight of macromonomer)

[0322] A 0.2 mass% tetrahydrofuran solution of the macromonomer was prepared, and the weight average molecular weight (Mw) based on a standard polystyrene was calculated under the following conditions.

[0323] • GPC device: "HLC-8320" manufactured by Tosoh Corporation

[0324] • Column: The following columns manufactured by Tosoh Corporation were connected in series and used. A guard column used was "TSKguard column Super HZ-L" (4.6 mm ID x 2.0 cm L) manufactured by Tosoh Corporation. "TSKgel Super HZM-M" (4.6 mm ID x 15 cm L) x 2, "TSKgel Super HZ2000" (4.6 mm ID x 15 cm L) x 1

[0325] • Injection amount: 10 μL

[0326] • Eluent: Tetrahydrofuran (stabilizer BHT)

[0327] • Flow rate: 0.35 mL / minute

[0328] • Column temperature: 40°C

[0329] Molecular weight of (meth)acrylic copolymer

[0330] A 0.27 mass% tetrahydrofuran solution of the (meth)acrylic copolymer was prepared, and the weight average molecular weight (Mw) based on a standard polystyrene was determined under the following conditions.

[0331] • GPC device: "HLC-8320" manufactured by Tosoh Corporation

[0332] • Column: Two columns "TSKgel SuperHZM-H" (6.0 mm ID x 15 cm L) manufactured by Tosoh Corporation were connected in series and used. A guard column was used "TSKguard column SuperHZ-H" (4.6 mm ID x 3.5 cm L) manufactured by Tosoh Corporation.

[0333] • Injection amount: 10 μL

[0334] • Eluent: Tetrahydrofuran (stabilizer BHT)

[0335] • Flow rate: 0.5 mL / minute

[0336] • Column temperature: 40°C

[0337] (Non-volatile component, volatile component)

[0338] About 1 g of the sample was placed on an aluminum dish, dried in an oven at 105°C with a blower for 2 hours, and the mass before and after drying was measured with an electronic balance, and the non-volatile component concentration was determined by the following formula.

[0339] Non-volatile component concentration (%) = (mass of the sample after drying (g) / mass of the sample before drying (g)) x 100

[0340] From the determined non-volatile component concentration, the volatile component concentration was determined by the following formula.

[0341] Volatile component concentration (%) = 100 - non-volatile component concentration (%)

[0342] (Adhesive force)

[0343] The adhesive sheet with release film prepared from each example was removed of the release film on the single side, and a polyethylene terephthalate (PET) film (thickness 50 μm) was attached as a backing film using a hand roller. This was cut into a long strip of width 10 mm x length 150 mm, and the adhesive face exposed by peeling the remaining release film was attached to a PET film (manufactured by Mitsubishi Chemical Corporation, DIAFOIL S-100, thickness 50 μm) that had been previously attached to a soda lime glass using a hand roller. The resulting laminate was subjected to autoclave treatment (60°C, 0.2 MPa gauge pressure, 20 minutes) and final attachment, and an adhesive strength measurement sample was prepared.

[0344] For the resulting adhesive strength measurement sample, the adhesive sheet was peeled from the PET film attached to the soda lime glass together with the backing film at a peel rate of 300 mm / minute while being stretched to form an angle of 180° under an atmosphere of 23°C, 50% RH or 60°C, 10% RH, and the tensile strength (N / cm) was measured as the adhesive strength using a load cell.

[0345] (Equivalent shear modulus G')

[0346] The adhesive sheet with release film prepared from each example was removed of the release film on the single side, and the operation of layering using a hand roller was repeated to adjust the thickness to about 0.8 mm, and punched into a circular shape of diameter 8 mm, which was used as a sample. The resulting sample was set in a rheometer ("DHR-2" manufactured by T.A. Instruments), and dynamic viscoelasticity measurement was performed under the following conditions: measuring jig: 8 mm diameter parallel plate, frequency: 1 Hz, measurement temperature: -50°C to 150°C, temperature increase rate: 5°C / minute, and the value of the storage shear modulus G' at -20°C, 25°C, 30°C, 60°C and 80°C was read.

[0347] (Glass transition temperature)

[0348] From the dynamic viscoelastic spectrum obtained in the measurement of the storage shear modulus G' described above, the temperature at which tan δ reached a maximum was read as the glass transition temperature (Tg).

[0349] (Creep test)

[0350] The adhesive sheet with release film prepared from each example was removed of the release film on the single side, and the operation of layering using a hand roller was repeated to adjust the thickness to about 0.8 mm, and punched into a circular shape of diameter 8 mm, which was used as a sample. The resulting sample was set in a rheometer ("DHR-2" manufactured by T.A. Instruments), and stress was applied under the following conditions: measuring jig: 8 mm diameter parallel plate, temperature: 60°C, pressure: 2 kPa, and the strain (%) after 600 seconds was measured, and this value was used as the maximum strain value (γ max). Then, the stress was released, and the strain (%) after 600 seconds was measured, and this value was taken as the residual strain value (γ min ), and the recovery rate was calculated from the following equation.

[0351] Recovery rate (%) = 〔(γ max - γ min ) / γ max 〕 x 100

[0352] (Gel fraction)

[0353] The adhesive sheet with the release film removed from each example was removed from the release film, and this was used as a sample.

[0354] A previously weighed sample was wrapped with a 150-mesh SUS-made metal mesh, and immersed in ethyl acetate at 23°C for 24 hours. Then, it was dried at 70°C for 4.5 hours, and the mass of the insoluble sample remaining in the metal mesh after the ethyl acetate immersion was measured. The mass percentage of the insoluble sample remaining in the metal mesh with respect to the mass of the sample before the ethyl acetate immersion was calculated as the gel fraction (%).

[0355] Note that when the conditions for the active energy ray irradiation of the adhesive composition (light source, cumulative light amount, etc.) are the same, it can be said that the higher the gel fraction of the adhesive sheet, the higher the sensitivity of the adhesive composition to the active energy ray.

[0356] (Used materials)

[0357] MBP: 4-methacryloyloxybenzophenone (monomer M having a structure that generates a radical by abstraction of hydrogen from a hydrogen donor by excitation).

[0358] HHMPMA: 2-[4-(2-hydroxy-2-methyl-l-oxopropyl)phenoxy]ethyl methacrylate (monomer M having a structure that generates a radical by cleavage of its own single bond by excitation).

[0359] 2EHA: 2-ethylhexyl acrylate.

[0360] nBA: n-butyl acrylate.

[0361] 4HBA: 4-hydroxybutyl acrylate.

[0362] SLMA: mixture of an alkyl methacrylate having an alkyl group with a carbon number of 12 and an alkyl methacrylate having an alkyl group with a carbon number of 13 ("ACRYESTER SL" manufactured by Mitsubishi Chemical Corporation).

[0363] AMBN: 2,2'-azobis(2-methylbutyronitrile)

[0364] <Photocurable compound (B)>

[0365] B-1: 2-functional urethane acrylate ("I-Quart UV-3700B" manufactured by Mitsubishi Chemical Corporation, Mw: 38000)

[0366] B-2: propoxylated pentaerythritol tri- and tetraacrylate ("ATM-4PL" manufactured by Shin-Nakamura Chemical Co., Ltd.)

[0367] B-3: mono-functional urethane acrylate having a polypropylene glycol skeleton (containing a small amount of 2-functional) ("PEM-X264" manufactured by AGC, Mw: 15000)

[0368] <Photoinitiator (C)>

[0369] C-1: mixture of 4-methyldibenzophenone and 2,4,6-trimethyldibenzophenone (hydrogen abstraction type) ("Esacure TZT" manufactured by IGM Resins)

[0370] (Production Example 1)

[0371] Into a four-necked flask equipped with a stirring device, a thermometer, a condenser tube, and a nitrogen inlet, 100 parts of SLMA, 0.00075 parts of bis[(difluoroboryl)diphenyl glyoxime] cobalt (II) as a chain transfer agent, and 58 parts of ethyl acetate were charged, and oxygen was replaced by bubbling nitrogen. Next, 0.4 parts of AMBN as a polymerization initiator and 2 parts of ethyl acetate were added. Next, the outside temperature was raised to 90°C with a water bath, and the reaction was performed under reflux for 2 hours. Next, 0.2 parts of AMBN, 20 parts of ethyl acetate were added dropwise over 1 hour, and then further maintained under reflux for 2 hours. Then, the reaction liquid was cooled to 40°C to obtain a solution containing a macromonomer (SLMA-MM). The non-volatile content concentration was adjusted to 50% by mass by adding ethyl acetate to the solution. The weight average molecular weight of the macromonomer (SLMA-MM) was 9420.

[0372] [Example 1]

[0373] <Production of (Meth)acrylic Copolymer>

[0374] In a four-necked flask equipped with a stirrer, a thermometer, a condenser, and a nitrogen inlet, 25 parts of ethyl acetate, 2 parts of isopropyl alcohol (IPA), and 6.8 parts of a solution of a macromonomer (SLMA-MM) (concentration: 50 mass%) were placed, and the temperature was raised to 85°C with a water bath under nitrogen. After the reflux state was stabilized, a mixture containing 20 parts of ethyl acetate, 28 parts of 2EHA, 61 parts of nBA, 4 parts of 4HBA, 0.2 parts of MBP, 0.13 parts of NYPER BK40MT (manufactured by NOF Corporation) was added dropwise over 4 hours. After 1 hour from the completion of the dropwise addition, a mixture containing 0.3 parts of PEROCTA O (manufactured by NOF Corporation) and 15 parts of ethyl acetate was added over 1 hour. Then, after 2 hours, 0.5 parts of "IRGANOX 1010" (trade name, manufactured by BASF Corporation) as an antioxidant and 23 parts of ethyl acetate were added, and the mixture was cooled to room temperature to obtain a composition containing a (meth)acrylic copolymer (SLMA-MM / 2EHA / nBA / 4HBA / MBP (mass ratio) = 6.8 / 28 / 61 / 4 / 0.2, weight average molecular weight (Mw): 700,000).

[0375] <Manufacture of Adhesive Sheet>

[0376] The composition obtained in the manufacture of the (meth)acrylic copolymer described above was directly used as an adhesive composition. The adhesive composition was spread on a release film (manufactured by Mitsubishi Chemical Corporation, PET film subjected to silicone release treatment) having a thickness of 100 μm in such a manner that the thickness after drying was 50 μm. Next, the sheet-shaped adhesive composition together with the release film was put in a drier heated to 90°C and kept for 10 minutes to dry the adhesive composition (to volatilize the solvent contained in the adhesive composition). Next, a release film (manufactured by Mitsubishi Chemical Corporation, PET film subjected to silicone release treatment) having a thickness of 75 μm was laminated on the sheet-shaped adhesive composition after drying.

[0377] Next, using a high-pressure mercury lamp, the aforementioned adhesive composition was irradiated with active energy rays through the aforementioned release film in such a manner that the cumulative light quantity at a wavelength of 365 nm became 4000 mJ / cm 2 to obtain an adhesive sheet with release film in which a release film was laminated on both the front and back sides of an adhesive sheet having a thickness of 50 μm.

[0378] (Examples 2 to 16, Comparative Example 1)

[0379] A pressure-sensitive adhesive sheet with a release film was prepared in the same manner as in Example 1, except that the copolymerization composition of the (meth)acrylic copolymer (A), the amount of the pressure-sensitive adhesive composition, and the amount of active energy ray exposure were changed as shown in Tables 1 and 2. In Tables 1 and 2, the amounts of the photocurable compound (B) and the photoinitiator (C) added are expressed as parts relative to 100 parts of the (meth)acrylic copolymer.

[0380] Tables 1 and 2 show the results of measurements and evaluations of the PSA sheets of each example.

[0381] [Table 1]

[0382]

[0383] [Table 2]

[0384]

[0385] As shown in Tables 1 and 2, the PSA sheets of Examples have high sensitivity to active energy rays and are excellent in flexibility and shape stability.

[0386] Among them, the PSA sheets of Examples 9 to 16 in which the monomer M had a structure in which its own single bond was cleaved by excitation to generate free radicals tended to have improved adhesive strength compared to the PSA sheets using the monomer M having a hydrogen abstraction type free radical generating group.

[0387] On the other hand, the maximum strain value (γ) of the PSA sheet of the comparative example when a stress of 2 kPa was applied at 60°C for 600 seconds was max ) is high and the shape stability is poor.

[0388] Industrial applicability

[0389] The present invention can provide a PSA sheet that is highly sensitive to active energy rays and can be cured efficiently, a PSA sheet with a release film using the PSA sheet, a PSA sheet for a flexible image display device component, a laminate for an image display device, and a flexible image display device.

Claims

1. A pressure-sensitive adhesive sheet comprising a pressure-sensitive adhesive composition comprising a (meth)acrylic acid copolymer (A). in, The (meth)acrylic copolymer (A) has a structural unit derived from a monomer M, and the monomer M generates an active species excited by irradiation with active energy rays. The PSA sheet satisfies the following requirements (1) and (2): Requirement (1): The storage shear modulus at -20°C (G'(-20°C)) obtained by dynamic viscoelasticity measurement in a shear mode at a frequency of 1 Hz is 10 kPa or more and 1000 kPa or less; as well as Requirement (2): Maximum strain value (γ) when a stress of 2 kPa is applied at 60°C for 600 seconds max ) is less than 80%.

2. The adhesive sheet according to claim 1, wherein The storage shear modulus at 30° C. (G′(30° C.)) obtained by dynamic viscoelasticity measurement in a shear mode at a frequency of 1 Hz was 1000 kPa or less.

3. The adhesive sheet according to claim 1, wherein The glass transition temperature (Tg) defined by the maximum value of Tan δ obtained by dynamic viscoelasticity measurement in a shear mode at a frequency of 1 Hz is -20°C or lower.

4. The adhesive sheet according to claim 1, wherein The maximum strain value (γ max ) and the residual strain value (γ min ) The recovery rate calculated by the following formula is 60% or more, Recovery rate (%) = (γ max -γ min ) / γ max 〕×100.

5. The adhesive sheet according to claim 1, wherein The gel fraction is 30% or more. The adhesive sheet according to claim 1 , wherein The content of the structural unit derived from the monomer M is 0.01 to 20% by mass based on the total structural units constituting the (meth)acrylic copolymer (A).

7. The adhesive sheet according to claim 1, wherein The monomer M has a structure in which, when excited by irradiation with active energy rays, its own single bond is cleaved to generate a free radical.

8. The adhesive sheet according to claim 1, wherein The monomer M has a structure that, when excited by irradiation with active energy rays, abstracts hydrogen from a hydrogen donor in the adhesive composition to generate a free radical.

9. The adhesive sheet according to claim 1, wherein The monomer M is represented by the following formula (I): Where R 1 represents a hydrogen atom, a methyl group, or an ethyl group, R 2 represents a linear or branched alkylene group having 1 to 5 carbon atoms, R 3 and R 4 Each independently represents a linear or branched alkyl group having 1 to 5 carbon atoms, R 3 and R 4 They are optionally bonded to each other to form a ring.

10. The adhesive sheet according to claim 1, wherein The (meth)acrylic copolymer (A) has a structural unit derived from a linear or branched alkyl (meth)acrylate (a1) having an alkyl group with 4 to 30 carbon atoms.

11. The adhesive sheet according to claim 1, wherein The (meth)acrylic copolymer (A) is a block copolymer or a graft copolymer.

12. The adhesive sheet according to claim 1, wherein The (meth)acrylic copolymer (A) includes a structural unit derived from a macromonomer (a9).

13. The adhesive sheet according to claim 12, wherein The macromonomer (a9) includes a structural unit derived from an alkyl (meth)acrylate having an alkyl group with 9 to 30 carbon atoms.

14. The adhesive sheet according to claim 1, wherein The adhesive composition includes a photocurable compound (B).

15. The adhesive sheet according to claim 1, wherein The adhesive composition includes a photoinitiator (C).

16. The adhesive sheet according to claim 1, wherein The adhesive composition includes a photocurable compound (B) and a photoinitiator (C).

17. The adhesive sheet according to claim 14, wherein The photocurable compound (B) contains a polyfunctional urethane (meth)acrylate. 18 . A release film-attached pressure-sensitive adhesive sheet comprising the pressure-sensitive adhesive sheet according to claim 1 and a release film laminated on at least one surface of the pressure-sensitive adhesive sheet. 19 . A pressure-sensitive adhesive sheet for a flexible image display device component, comprising the pressure-sensitive adhesive sheet according to claim 1 .

20. A laminate for an image display device, wherein: Two image display device components are stacked via the adhesive sheet according to any one of claims 1 to 17, wherein at least one of the image display device components has a step with a height difference of 2 μm or more on a contact surface with the adhesive sheet. 21 . A flexible image display device comprising the laminate for an image display device according to claim 20 .

22. A photocurable adhesive sheet, comprising an adhesive composition containing a (meth)acrylic copolymer (A). in, The (meth)acrylic copolymer (A) has a structural unit derived from a monomer M, and the monomer M generates an active species excited by irradiation with active energy rays. The adhesive sheet satisfies the following requirements (1') and (2'), Requirement (1'): The cumulative light intensity is 1000 to 5000 mJ / cm 2 When the photocurable adhesive sheet is irradiated with active energy rays having a wavelength of 365 nm at any irradiation dose within a range of , the storage shear modulus at -20°C (G'(-20°C)) obtained by dynamic viscoelasticity measurement in a shear mode at a frequency of 1 Hz is 10 kPa or more and 1000 kPa or less; and Requirement (2'): The cumulative light intensity is 1000 to 5000 mJ / cm 2 The maximum strain value (γ) when the photocurable adhesive sheet is irradiated with an active energy ray having a wavelength of 365 nm and a stress of 2 kPa is applied at 60° C. for 600 seconds is max ) is less than 80%.

23. An adhesive composition comprising a (meth)acrylic copolymer (A), in, The (meth)acrylic copolymer (A) has a structural unit derived from a monomer M, and the monomer M generates an active species excited by irradiation with active energy rays. The adhesive composition satisfies the following requirements (1") and (2"), Requirement (1"): When the adhesive composition is dried to form a photocurable adhesive sheet, the accumulated light intensity is 1000 to 5000 mJ / cm 2 When the photocurable adhesive sheet is irradiated with active energy rays having a wavelength of 365 nm at any irradiation dose within a range of , the storage shear modulus at -20°C (G'(-20°C)) obtained by dynamic viscoelasticity measurement in a shear mode at a frequency of 1 Hz is 10 kPa or more and 1000 kPa or less; and Requirement (2"): When the adhesive composition is dried to form a photocurable adhesive sheet, the accumulated light intensity is 1000 to 5000 mJ / cm 2 When the photocurable adhesive sheet is irradiated with active energy rays having a wavelength of 365 nm at any irradiation dose within a range of , the maximum strain value (γ) when a stress of 2 kPa is applied at 60° C. for 600 seconds is obtained. max ) is less than 80%.

Citation Information

Patent Citations

  • Adhesive for repeated flexure device, adhesive sheet, repeated flexure laminate member, and repeated flexure device

    JP2019123826A

  • Washing aid

    JP2023045353A

  • (METH)acrylic copolymer, adhesive composition containing same, and adhesive sheet

    WO2015080244A1