Acrylamide microspheres as well as preparation method and application thereof

By introducing specific structural units and zwitterionic compounds into microspheres, the adsorption between microspheres and formations and the aggregation ability between microspheres are enhanced, solving the problem of low plugging efficiency of polymer microspheres, achieving a highly efficient plugging effect, and improving oilfield recovery.

CN120818095APending Publication Date: 2025-10-21CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410447746.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-04-15
Publication Date
2025-10-21

AI Technical Summary

Technical Problem

Existing polymer microspheres are easy to diffuse in the formation, have low plugging efficiency, and cannot effectively mechanically bridge, resulting in insufficient plugging strength and affecting oil field recovery.

Method used

Introducing a shell containing specific structural units into the microspheres enhances the adsorption between the microspheres and the formation, and forming electrostatic ion pairs on the surface of the microspheres through zwitterionic compounds improves the aggregation ability between the microspheres, thereby enhancing the sealing effect.

Benefits of technology

In highly mineralized brine, when the microsphere concentration is 2000ppm, the plugging rate is greater than 98%, which significantly improves the plugging efficiency and solves the problem of microsphere diffusion in the formation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120818095A_ABST
    Figure CN120818095A_ABST
Patent Text Reader

Abstract

The invention discloses an acrylamide microsphere and a preparation method and application thereof.The acrylamide microsphere comprises a polymer inner core and a polymer shell layer, the polymer shell layer comprises an acrylamide structural unit, a structural unit shown in the formula (1) and a crosslinking structural unit II, in the formula (1), R1 and R1'are independently selected from hydrogen atoms or alkyl groups; r2 is selected from an oxygen atom,-NH or an alkyl-substituted nitrogen atom; r3 and R4 are independently selected from alkyl groups; r5 is selected from anionic organic groups; and R6 and R7 are independently selected from alkyl groups. The acrylamide microspheres are applied to oil and gas field development, especially profile control agents or blocking agents. Compared with common polymer microspheres, the acrylamide microspheres provided by the invention have the advantage that the plugging efficiency is greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of oil and gas field development, and in particular relates to acrylamide microspheres that can be used for underground depth profile control, and a preparation method and application thereof. Background Art

[0002] The international situation is complex and volatile, and the stable and healthy development of the national economy faces multiple challenges, of which energy security is of paramount importance. Crude oil is currently one of the most important energy sources for the industrial sector. However, my country's crude oil reservoirs are complex, making sustained and stable supply difficult after long-term production. Most mature oil fields in China have developed extensive water flooding channels or high-permeability layers after long-term water flooding. This results in ineffective circulation of subsequently injected flooding fluids, making it difficult to further improve sweep and oil washing efficiency, and severely restricting the improvement of crude oil recovery rates.

[0003] Profile control and channel sealing are important measures to enhance oil recovery in high-water-cut oilfields. Commonly used materials include cross-linked gel particles, polymer jelly, and polymer microspheres. Microspheres have a small particle size, good injectability, and easy penetration into deep formations. They can effectively and long-term block advantageous channels deep in the formation and have been widely used in profile control and channel sealing.

[0004] However, polymer microspheres also suffer from low plugging efficiency and strength. This is primarily due to their small particle size, which makes them easily diffuse in the formation due to dilution by formation water, resulting in a concentration below the effective concentration. This prevents effective mechanical bridging and, consequently, prevents effective plugging. This is due to weak interactions between the microspheres and between them and the formation. Summary of the Invention

[0005] To overcome the problems existing in the prior art, the present invention provides acrylamide microspheres, a preparation method, and applications thereof. The present invention introduces a shell containing a structural unit represented by formula (1) into the microspheres, which can impart a strong adsorption effect between the microspheres and the formation. After injection into the formation, the acrylamide microspheres obtained by the present invention have a strong adsorption and retention capacity in the formation, which can produce a more efficient plugging effect. At the same time, the microspheres also have a stronger adsorption and aggregation capacity, which can effectively enhance the plugging effect. This is beneficial to improving the deep profile control process of oil fields and is of great value in improving the recovery rate of high-water-content oil fields.

[0006] One of the objects of the present invention is to provide an acrylamide microsphere comprising a polymer core and a polymer shell, wherein the polymer shell comprises an acrylamide structural unit, a structural unit represented by formula (1) and a cross-linked structural unit II:

[0007]

[0008] In formula (1), R1 and R1' are independently selected from hydrogen atoms or alkyl groups; R2 is selected from oxygen atoms, -NH or alkyl-substituted nitrogen atoms; R3 and R4 are independently selected from alkylene groups; R5 is selected from anionic organic groups; R6 and R7 are independently selected from alkyl groups.

[0009] In a preferred embodiment, in formula (1), R1 and R1' are independently selected from a hydrogen atom or a C1-C15 alkyl group; R2 is selected from an oxygen atom, -NH or an alkyl-substituted nitrogen atom; R3 and R4 are each independently selected from a C1-C15 alkylene group; R5 is selected from one of a carboxyl group, a sulfate group, a sulfonic acid group, and a phosphoric acid group; R6 and R7 are each independently selected from a C1-C15 alkyl group.

[0010] In a further preferred embodiment, in formula (1), R1 and R1' are independently selected from a hydrogen atom or a C1-C6 alkyl group; R2 is selected from an oxygen atom, -NH or an alkyl-substituted nitrogen atom; R3 and R4 are each independently selected from a C2-C8 alkylene group; R5 is selected from one of a carboxyl group, a sulfate group, a sulfonic acid group, and a phosphoric acid group; R6 and R7 are each independently selected from a C1-C6 alkyl group.

[0011] In a preferred embodiment, in the polymer shell layer, by weight:

[0012] 5 to 10 parts of acrylamide structural units, for example 5, 6, 7, 8, 9 or 10 parts;

[0013] 5 to 10 parts, for example 5, 6, 7, 8, 9 or 10 parts, of the structural unit represented by formula (1);

[0014] Cross-linking structural unit II 0.0005 to 0.2 parts, for example 0.0005, 0.005, 0.05, 0.1, 0.1, 0.15 or 0.2 parts.

[0015] In a further preferred embodiment, in the polymer shell layer, in parts by weight:

[0016] 5 to 7.5 parts of acrylamide structural units,

[0017] 5 to 7.5 parts of the structural unit represented by formula (1),

[0018] Cross-linking structural unit II 0.005 to 0.1 parts.

[0019] In a preferred embodiment, the polymer core comprises an acrylamide structural unit, an anionic structural unit, an optional nonionic structural unit, and a cross-linking structural unit I.

[0020] In a further preferred embodiment, in the polymer core, by weight:

[0021] 5 to 30 parts of acrylamide structural units, for example 5, 10, 15, 20, 25 or 30 parts;

[0022] 1 to 25 parts of anionic structural units, for example 1, 5, 10, 15, 20 or 25 parts;

[0023] 0-10 parts of nonionic structural units, for example 0, 2, 4, 6, 8 or 10 parts;

[0024] Cross-linked structural unit I 0.001 to 0.5 parts, for example 0.001, 0.005, 0.01, 0.05, 0.1, 0.3 or 0.5 parts.

[0025] In a further preferred embodiment, in the polymer core, by weight:

[0026] 20-25 parts of acrylamide structural units;

[0027] 5 to 10 parts of anionic structural units;

[0028] 0-7.5 parts of nonionic structural unit;

[0029] Cross-linked structural unit I 0.01 to 0.25 parts.

[0030] In a preferred embodiment, the anion structure is selected from at least one of a carboxylic acid structural unit and / or an alkali metal salt thereof, a sulfonic acid structural unit and / or an alkali metal salt thereof.

[0031] In a further preferred embodiment, the anionic structural unit is derived from at least one of acrylic acid, methacrylic acid, p-vinylbenzenesulfonic acid, maleic acid, fumaric acid, vinylbenzenesulfonic acid, allylsulfonic acid, allylbenzenesulfonic acid, 2-acrylamido-2-methylpropanesulfonic acid, and alkali metal salts thereof.

[0032] In a preferred embodiment, the nonionic structural unit is selected from at least one of a substituted acrylamide structural unit, a (substituted) hydroxyalkyl acrylate structural unit, a (substituted) acrylic acid (substituted) amino ester structural unit, and a pyrrolidone structural unit.

[0033] In a further preferred embodiment, the nonionic structural unit is derived from at least one of methacrylamide, dimethylacrylamide, diethylacrylamide, hydroxymethylacrylamide, hydroxyethylacrylamide, dimethylaminopropyl methacrylamide, hydroxymethyl methacrylate, hydroxyethyl methacrylate, dimethylaminoethyl methacrylate, vinyl pyrrolidone, and tert-butylacrylamide.

[0034] In a preferred embodiment, the cross-linked structural unit I and the cross-linked structural unit II are each independently derived from a compound containing at least two double bonds, preferably from a compound containing 2 to 5 double bonds.

[0035] In a further preferred embodiment, the cross-linked structural unit I and the cross-linked structural unit II are independently derived from at least one of ethylene glycol diallyl ether, glycerol diallyl ether, glycerol triallyl ether, pentaerythritol diallyl ether, pentaerythritol triallyl ether, and pentaerythritol tetraallyl ether.

[0036] In a preferred embodiment, the polymer core optionally contains a zwitterionic compound.

[0037] It is not desirable to immediately seal the formation near the wellbore; rather, it is desirable to allow the microspheres to migrate for a period of time before becoming effective. In the present invention, after the microspheres enter the aqueous solution, the zwitterionic compound slowly diffuses out. Thus, the zwitterionic compound can form electrostatic ion pairs with the structural unit represented by formula (1) on the surface of the microspheres, thereby providing more contact and aggregation points between the microspheres and further strengthening the interaction between the microspheres.

[0038] In a further preferred embodiment, the zwitterionic compound is selected from at least one of the compounds represented by formula (2):

[0039]

[0040] In formula (2), R8 is selected from C1 to C10 alkylene groups (preferably C1 to C5 alkylene groups), R9 is selected from anionic organic groups, and R 10 ~R 12 Each is independently selected from a C1 to C10 alkyl group (preferably a C1 to C5 alkyl group).

[0041] In a further preferred embodiment, the zwitterionic compound is at least one selected from (3-carboxypropyl)trimethylammonium chloride, (carboxymethyl)trimethylammonium chloride, and (2-carboxyethyl)trimethylammonium chloride.

[0042] In a preferred embodiment, in the polymer core, based on 5 to 30 parts, preferably 20 to 25 parts, of acrylamide structural units, the zwitterionic compound is 0 to 10 parts, preferably 2 to 5 parts, for example 0, 2, 4, 6, 8 or 10 parts.

[0043] A second object of the present invention is to provide a method for preparing acrylamide microspheres, preferably for preparing the acrylamide microspheres described in one of the first objects of the present invention, the preparation method comprising: (A) preparing a polymer core using a raw material I including acrylamide, an anionic monomer, an optional nonionic monomer, a crosslinker I, and an optional zwitterionic compound; and (B) preparing a polymer shell using a raw material including acrylamide, a monomer compound corresponding to the structural unit represented by formula (1), and a crosslinker II, to obtain the acrylamide microspheres.

[0044] In a preferred embodiment, the anionic monomer is selected from at least one of a carboxylic acid polymerizable monomer and / or an alkali metal salt thereof, a sulfonic acid polymerizable monomer and / or an alkali metal salt thereof.

[0045] In a further preferred embodiment, the anionic monomer is selected from at least one of acrylic acid, methacrylic acid, p-vinylbenzenesulfonic acid, maleic acid, fumaric acid, vinylbenzenesulfonic acid, allylsulfonic acid, allylbenzenesulfonic acid, 2-acrylamido-2-methylpropanesulfonic acid, and alkali metal salts thereof.

[0046] In a preferred embodiment, the nonionic monomer is selected from at least one of substituted acrylamide polymerizable monomers, (substituted) hydroxyalkyl acrylate polymerizable monomers, (substituted) acrylate (substituted) amino ester polymerizable monomers, and pyrrolidone polymerizable monomers.

[0047] In a further preferred embodiment, the nonionic monomer is selected from at least one of methacrylamide, dimethylacrylamide, diethylacrylamide, hydroxymethylacrylamide, hydroxyethylacrylamide, dimethylaminopropyl methacrylamide, hydroxymethyl methacrylate, hydroxyethyl methacrylate, dimethylaminoethyl methacrylate, vinyl pyrrolidone, and tert-butylacrylamide.

[0048] In a preferred embodiment, the cross-linking agent I and the cross-linking agent II are each independently selected from compounds containing at least two double bonds, preferably compounds containing 2 to 5 double bonds.

[0049] In a further preferred embodiment, the crosslinking agent I and the crosslinking agent II are each independently selected from at least one of ethylene glycol diallyl ether, glycerol diallyl ether, glycerol triallyl ether, pentaerythritol diallyl ether, pentaerythritol triallyl ether and pentaerythritol tetraallyl ether.

[0050] In a preferred embodiment, in step (A), in parts by weight:

[0051] 5 to 30 parts of acrylamide, preferably 20 to 25 parts;

[0052] 1 to 25 parts of anionic monomer, preferably 5 to 10 parts;

[0053] 0-10 parts of nonionic monomer, preferably 0-7.5 parts;

[0054] Cross-linking agent I 0.001 to 0.5 parts, preferably 0.01 to 0.25 parts;

[0055] The amount of the zwitterionic compound is 0 to 10 parts, preferably 2 to 5 parts.

[0056] For example, acrylamide is 5, 10, 15, 20, 25 or 30 parts, the nonionic monomer is 0, 2, 4, 6, 8 or 10 parts, the crosslinker I is 0.001, 0.005, 0.01, 0.03, 0.05, 0.1, 0.2, 0.4 or 0.5 parts, and the zwitterionic compound is 0, 2, 4, 6, 8 or 10 parts.

[0057] In a preferred embodiment, in step (B), by weight:

[0058] 5 to 10 parts of acrylamide; preferably 5 to 7.5 parts;

[0059] 5 to 10 parts of the monomer compound corresponding to the structural unit represented by formula (1); preferably 5 to 7.5 parts;

[0060] Cross-linking agent II 0.0005 to 0.2 parts; preferably 0.005 to 0.1 parts.

[0061] For example, in step (3), by weight: acrylamide is 5, 6, 7, 8, 9 or 10 parts; the monomer compound corresponding to the structural unit represented by formula (1) is 5, 6, 7, 8, 9 or 10 parts; and the cross-linking agent II is 0.0005, 0.005, 0.05, 0.1, 0.15 or 0.2 parts.

[0062] In a preferred embodiment, the preparation method comprises:

[0063] (1) mixing raw materials I including acrylamide, an anionic monomer, an optional nonionic monomer, a crosslinking agent I, and an optional zwitterionic compound, adjusting the pH, and adding an azo initiator to obtain an aqueous phase; mixing an emulsifier and an oil solvent to obtain an oil phase;

[0064] (2) mixing the oil phase and the water phase, stirring, introducing a protective gas, and adding an oxidizing agent aqueous solution and a reducing agent aqueous solution to obtain a reaction system I;

[0065] (3) acrylamide, a monomer compound corresponding to the structural unit represented by formula (1), a crosslinking agent II and water are mixed and added to the reaction system I, stirred and introduced with a protective gas, and then an oxidant aqueous solution and a reducing agent aqueous solution are added to carry out a reaction.

[0066] In a preferred embodiment, in step (1), the pH is adjusted to 5-10, for example, 5, 6, 7, 8, 9 or 10.

[0067] In a preferred embodiment, the monomer compound corresponding to the structural unit represented by formula (1) is selected from at least one of the compounds represented by the following formulae:

[0068]

[0069] In the above formula, R1, R1', R2, R3, R4, R5, R6, and R7 are defined the same as in formula (1).

[0070] In a preferred embodiment, in step (1), the azo initiator is selected from at least one of azobisisobutyronitrile, azobisisovaleronitrile, azobisisoheptanoonitrile, dimethyl azobisisobutyrate, azobisisobutylamidine hydrochloride, 2,2'-azo[2-(2-imidazolin-2-yl)propane]dihydrochloride, azobis(2,5-dimethyl-6-carboxy)hexanenitrile, and 4,4'-azobis(4-cyanovaleric acid).

[0071] In a preferred embodiment, in step (1), the emulsifier is selected from at least one of fatty alcohol polyoxypropylene polyoxyethylene ether, aromatic alcohol polyoxypropylene polyoxyethylene ether, fatty acid polyoxypropylene polyoxyethylene ester, fatty amine polyoxypropylene polyoxyethylene ether, sorbitan oleate, sorbitan stearate, sorbitan palmitate, and sorbitan laurate, and is most preferably used in combination to make the HLB value between 5.5 and 6.

[0072] In a preferred embodiment, in step (1), the oil solvent is selected from at least one of aliphatic hydrocarbons, aromatic hydrocarbons, and mineral oil.

[0073] In a further preferred embodiment, the aliphatic hydrocarbon is selected from at least one of cyclohexane, hexane, heptane, and octane, and / or the aromatic hydrocarbon is selected from at least one of benzene, toluene, ethylbenzene, and xylene, and / or the mineral oil is selected from at least one of liquid paraffin, white oil, gasoline, diesel, and kerosene.

[0074] In a preferred embodiment, in step (2) and step (3),

[0075] The oxidant is at least one selected from the group consisting of ammonium persulfate, potassium persulfate, sodium persulfate, hydrogen peroxide, benzoyl peroxide, potassium bromate, tert-butyl hydroperoxide, lauroyl peroxide, cumene hydroperoxide, di-tert-butyl peroxide, diisopropyl peroxide, tert-butyl perbenzoate, tert-butyl pervalerate, methyl ethyl ketone peroxide, cyclohexanone peroxide, diisopropyl peroxydicarbonate, and dicyclohexyl peroxydicarbonate; and / or

[0076] The reducing agent is selected from at least one of sodium bisulfite, sodium thiosulfate, sodium dithionite, sodium metabisulfite, tetramethylethylenediamine, ammonium ferrous sulfate, sodium formaldehyde sulfoxylate, N,N-dimethylaniline, tartaric acid, ferrous sulfate, N,N-diethylaniline, ferrous pyrophosphate, silver nitrate, mercaptan, ferrous chloride, tetraethyleneimine, glycerol, and pentaerythritol.

[0077] In a preferred embodiment, in step (1) and step (2), in parts by weight:

[0078] 0.0001 to 0.005 parts of oxidizing agent, preferably 0.0002 to 0.003 parts;

[0079] 0.0001 to 0.005 parts of reducing agent, preferably 0.0002 to 0.003 parts;

[0080] 0.001 to 0.05 parts of azo initiator, preferably 0.005 to 0.02 parts;

[0081] 10 to 100 parts of water, preferably 25 to 50 parts, for example 10, 35, 50, 80 or 100 parts;

[0082] 40 to 100 parts of oil solvent, preferably 50 to 75 parts, for example 40, 60, 80 or 100 parts;

[0083] 2 to 20 parts of emulsifier, preferably 2.5 to 15 parts, for example 2, 5, 10, 12, 15, 15 or 20 parts.

[0084] In a preferred embodiment, in step (3), in parts by weight:

[0085] 0.0001 to 0.005 parts of oxidizing agent, preferably 0.0002 to 0.003 parts;

[0086] 0.0001 to 0.005 parts of reducing agent, preferably 0.0002 to 0.003 parts;

[0087] 10 to 100 parts of water, preferably 10 to 30 parts, for example 10, 20, 40, 60, 80 or 100 parts.

[0088] In a preferred embodiment, in step (2) and step (3), the protective gas is selected from at least one of nitrogen and an inert gas.

[0089] In a preferred embodiment, in step (2), after stirring, protective gas is introduced for 0.1 to 10 hours, preferably 0.5 to 5 hours, and then an aqueous oxidant solution is added. After 0.1 to 20 minutes, preferably 0.5 to 10 minutes, an aqueous reducing agent solution is slowly added dropwise until the reaction system is heated up.

[0090] In a preferred embodiment, in step (3), stirring and introducing protective gas for 5 to 60 minutes (for example, 5, 10, 20, 30, 40, 50 or 60 minutes), adding an aqueous solution of an oxidant, and after 0.1 to 15 minutes (for example, 0.1, 0.5, 1, 2, 4, 6, 8, 10, 12, 14 or 15 minutes), slowly adding an aqueous solution of a reducing agent dropwise until the temperature of the reaction system is completely raised, and then keeping the temperature at 35 to 70°C (for example, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C or 70°C) for 0.2 to 5 hours (for example, 0.2, 0.5, 1, 2, 3, 4 or 5 hours).

[0091] In a preferred embodiment, the concentration of the aqueous oxidizing agent solution in steps (2) to (3) is independently 0.1 to 10 wt%, preferably 0.2 to 5 wt%, for example, 0.2 wt%, 0.5 wt%, 0.8 wt%, 1 wt%, 2 wt%, 3 wt%, 4 wt% or 5 wt%; and / or the concentration of the aqueous reducing agent solution in steps (2) to (3) is independently 0.1 to 10 wt%, preferably 0.2 to 5 wt%, for example, 0.2 wt%, 0.5 wt%, 0.8 wt%, 1 wt%, 2 wt%, 3 wt%, 4 wt% or 5 wt%.

[0092] A third object of the present invention is to provide the use of the acrylamide microspheres described in the first object of the present invention or the acrylamide microspheres obtained by the preparation method described in the second object of the present invention in oil and gas field development, especially as profile control agents or plugging agents.

[0093] The endpoints and any values ​​of the ranges disclosed in the present invention are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and a separate point value, and the separate point values ​​can be combined with each other to obtain one or more new numerical ranges, and these numerical ranges should be considered as specifically disclosed in this article. Hereinafter, in principle, each technical solution can be combined with each other to obtain a new technical solution, which should also be considered as specifically disclosed in this article.

[0094] Compared with existing technologies, the present invention has the following beneficial effects: In 180,000 mg / L highly mineralized brine (calcium and magnesium ion contents of 2500 ppm each), when the microsphere concentration is 2000 ppm, the microsphere concentration in the produced fluid after dynamic adsorption in a sand-filled pipe is less than 50 ppm, and the plugging efficiency is greater than 98%. Compared with conventional polymer microspheres, the plugging efficiency of the acrylamide microspheres of the present invention is significantly improved. DETAILED DESCRIPTION

[0095] The present invention will be described in detail below with reference to specific embodiments. It is necessary to point out that the following embodiments are only used to further illustrate the present invention and are not to be construed as limiting the scope of protection of the present invention. Non-essential improvements and adjustments made by those skilled in the art to the present invention based on the contents of the present invention still fall within the scope of protection of the present invention.

[0096] It should also be noted that the various specific technical features described in the following specific embodiments can be combined in any appropriate manner without contradiction. To avoid unnecessary repetition, the present invention will not further describe various possible combinations.

[0097] In addition, the various embodiments of the present invention may be arbitrarily combined as long as they do not violate the concept of the present invention. The technical solutions thus formed belong to part of the original disclosure of this specification and also fall within the scope of protection of the present invention.

[0098] Unless otherwise specified, the raw materials used in the examples and comparative examples are all disclosed in the prior art, for example, they can be directly purchased or prepared according to the preparation methods disclosed in the prior art.

[0099] [Example 1]

[0100] 22 parts of acrylamide, 5 parts of acrylic acid, 2 parts of vinyl pyrrolidone, 0.015 parts of ethylene glycol diallyl ether, and 3 parts of (3-carboxypropyl)trimethylammonium chloride (purchased from Shanghai Aladdin Biochemical Technology Co., Ltd., CAS No.: 6249-56-5) were dissolved in 25 parts of water to obtain a reaction solution. The pH value of the solution was adjusted to 7.0 with sodium hydroxide. 0.01 parts of azobisisobutylamidine hydrochloride was added and stirred uniformly to obtain a uniform aqueous phase. 10 parts of anhydrous sorbitan monooleate (Span 80) and 1.75 parts of isomeric tridecanol polyoxyethylene ether (5) were added to 55 parts of 3# white oil and stirred uniformly to obtain an oil phase. The oil phase and aqueous phase were added to a reactor separately and stirred at 700 rpm for 1 hour while continuously introducing nitrogen for deoxygenation.

[0101] 0.0004 parts of sodium persulfate and 0.0005 parts of sodium bisulfite were prepared into a 1 wt% uniform aqueous solution, and after adding the oxidant aqueous solution, stirring was continued for 10 minutes, and the reducing agent aqueous solution was slowly added dropwise until the temperature rose to 50°C, until the reaction system finished heating up.

[0102] 7.5 parts of acrylamide, 7.5 parts of 3-[(3-acrylamidopropyl)dimethylammonium]propionate (purchased from Shanghai Aladdin Biochemical Technology Co., Ltd., CAS No.: 79704-35-1), and 0.0075 parts of ethylene glycol diallyl ether were dissolved in 15 parts of deionized water to form a uniform solution, which was then added to the above reaction system. Stirring was continued while nitrogen was passed through for 30 minutes. A 1wt% aqueous solution of an oxidizing agent (containing 0.0002 parts of sodium persulfate) was added. After 5 minutes, a 1wt% aqueous solution of a reducing agent (containing 0.00025 parts of sodium bisulfite) was slowly added dropwise until the reaction system finished heating up. The temperature was then maintained at 50°C for 1 hour. The obtained product was the product.

[0103] [Example 2]

[0104] 20 parts of acrylamide, 5 parts of 2-acrylamido-2-methylpropanesulfonic acid, 4 parts of tert-butyl acrylamide, 0.02 parts of glycerol diallyl ether (purchased from Shanghai Aladdin Biochemical Technology Co., Ltd., CAS No.: 17018-07-4), and 3.5 parts of (carboxymethyl)trimethylammonium chloride (purchased from Shanghai Aladdin Biochemical Technology Co., Ltd., CAS No.: 590-46-5) were dissolved in 27 parts of water to obtain a reaction solution. The pH value of the solution was adjusted to 7.0 with sodium hydroxide. 0.0075 parts of azobisisobutylamidine hydrochloride was added and stirred evenly to obtain a uniform aqueous phase. 12 parts of anhydrous sorbitan stearate and 1.5 parts of isomeric tridecanol polyoxyethylene ether (8) were added to 50 parts of 5# white oil and stirred evenly to obtain an oil phase. The oil phase and the aqueous phase were added to a reactor respectively, stirred at 700 rpm for 1 hour, and nitrogen was continuously introduced for deoxygenation.

[0105] 0.001 parts of potassium bromate and 0.002 parts of sodium dithionite were prepared into a 1% uniform aqueous solution. After adding the oxidant aqueous solution, stirring was continued for 10 minutes. The reducing agent aqueous solution was slowly added dropwise until the temperature rose to 50°C, until the reaction system finished heating up.

[0106] 7 parts of acrylamide, 4-[(3-methacrylamidopropyl)dimethylammonium]butane-1-sulfonate (purchased from Shanghai Aladdin Biochemical Technology Co., Ltd., CAS number: 83623-32-9) 6.5 parts, and 0.008 parts of glycerol diallyl ether (purchased from Shanghai Aladdin Biochemical Technology Co., Ltd., CAS number: 17018-07-4) were dissolved in 12.5 parts of deionized water to form a uniform solution, which was added to the above reaction system. Continue stirring and purging with nitrogen for 30 minutes, add a 1wt% aqueous solution of an oxidant (containing 0.002 parts of potassium bromate), and after 5 minutes, slowly add a 1wt% aqueous solution of a reducing agent (containing 0.0025 parts of sodium dithionite) dropwise until the reaction system is heated to completion, and keep warm at 50°C for 1 hour. The obtained product is the product.

[0107] [Example 3]

[0108] 25 parts of acrylamide, 7.5 parts of acrylic acid, 5 parts of vinyl pyrrolidone, 0.015 parts of pentaerythritol triallyl ether, and 5 parts of (3-carboxypropyl)trimethylammonium chloride (purchased from Shanghai Aladdin Biochemical Technology Co., Ltd., CAS No.: 6249-56-5) were dissolved in 30 parts of water to obtain a reaction solution. The pH value of the solution was adjusted to 7.0 with sodium hydroxide. 0.015 parts of azobisisobutylamidine hydrochloride was added and stirred uniformly to obtain a uniform aqueous phase. 12 parts of anhydrous sorbitan monooleate and 2.25 parts of isomeric tridecanol polyoxyethylene ether (5) were added to 58 parts of diesel and stirred uniformly to obtain an oil phase. The oil phase and the aqueous phase were added to a reactor respectively, stirred at 700 rpm for 1 hour, and nitrogen was continuously introduced for deoxygenation.

[0109] 0.00075 parts of ammonium persulfate and 0.001 parts of sodium metabisulfite were prepared into a 1% uniform aqueous solution, and after adding the oxidant aqueous solution, stirring was continued for 10 minutes, and the reducing agent aqueous solution was slowly added dropwise until the temperature rose to 50°C, until the reaction system finished heating up.

[0110] 7.5 parts of acrylamide, 7 parts of 4-[[2-(methacryloyloxy)ethyl]dimethylammonio]butane-1-sulfonate (purchased from Shanghai Aladdin Biochemical Technology Co., Ltd., CAS No.: 6613-65-6), and 0.0075 parts of pentaerythritol triallyl ether were dissolved in 17.5 parts of deionized water to form a uniform solution, which was then added to the above reaction system. Stirring was continued while nitrogen was passed through for 30 minutes. A 1wt% aqueous solution of an oxidant (containing 0.00025 parts of ammonium persulfate) was added. After 5 minutes, a 1wt% aqueous solution of a reducing agent (containing 0.001 parts of sodium metabisulfite) was slowly added dropwise until the reaction system finished heating up. The temperature was then maintained at 50°C for 1 hour. The obtained product was the product.

[0111] [Example 4]

[0112] 22 parts of acrylamide, 7.5 parts of 2-acrylamido-2-methylpropanesulfonic acid, 7 parts of tert-butylacrylamide, 0.025 parts of ethylene glycol diallyl ether, and 4 parts of (3-carboxypropyl)trimethylammonium chloride were dissolved in 32.5 parts of water to obtain a reaction solution. The pH value of the solution was adjusted to 7.0 with sodium hydroxide. 0.02 parts of azobisisobutylamidine hydrochloride was added and stirred uniformly to obtain a uniform aqueous phase. 8.5 parts of anhydrous sorbitan stearate and 1.25 parts of isomeric tridecanol polyoxyethylene ether (8) were added to 60 parts of kerosene and stirred uniformly to obtain an oil phase. The oil phase and the aqueous phase were added to a reactor respectively, stirred at 700 rpm for 1 hour, and nitrogen was continuously introduced for deoxygenation.

[0113] 0.0025 parts of tert-butyl hydroperoxide and 0.003 parts of ferrous ammonium sulfate were prepared into a 1% uniform aqueous solution. After adding the oxidant aqueous solution, stirring was continued for 10 minutes. The reducing agent aqueous solution was slowly added dropwise until the temperature rose to 50°C, until the reaction system finished heating up.

[0114] 6.5 parts of acrylamide, 7 parts of 3-[(3-acrylamidopropyl)dimethylammonium]propionate (purchased from Shanghai Aladdin Biochemical Technology Co., Ltd., CAS No.: 79704-35-1), and 0.006 parts of ethylene glycol diallyl ether were dissolved in 25 parts of deionized water to form a uniform solution, which was then added to the above reaction system. Stirring was continued while nitrogen was passed through for 30 minutes. A 1wt% aqueous solution of an oxidizing agent (containing 0.002 parts of tert-butyl hydroperoxide) was added. After 5 minutes, a 1wt% aqueous solution of a reducing agent (containing 0.0025 parts of ferrous ammonium sulfate) was slowly added dropwise until the reaction system was heated to completion. The temperature was then maintained at 50°C for 1 hour. The obtained product was the product.

[0115] [Comparative Example 1]

[0116] Dissolve 22 parts of acrylamide, 5 parts of acrylic acid, 2 parts of vinyl pyrrolidone, and 0.015 parts of ethylene glycol diallyl ether in 25 parts of water to obtain a reaction solution. Adjust the solution to pH 7.0 with sodium hydroxide, add 0.01 parts of azobisisobutylamidine hydrochloride, and stir evenly to obtain a uniform aqueous phase. Add 10 parts of anhydrous sorbitan monooleate and 1.75 parts of isomeric tridecyl alcohol polyoxyethylene ether (5) to 55 parts of 3# white oil and stir evenly to obtain an oil phase. Add the oil phase and aqueous phase separately to a reactor, stir at 700 rpm for 1 hour, and continuously introduce nitrogen for deoxygenation.

[0117] 0.0004 parts of sodium persulfate and 0.0005 parts of sodium bisulfite were prepared into a 1 wt% uniform aqueous solution, and after adding the oxidant aqueous solution, stirring was continued for 10 minutes, and the reducing agent aqueous solution was slowly added dropwise until the temperature rose to 50°C, until the reaction system finished heating up.

[0118] 7.5 parts of acrylamide, 7.5 parts of 3-[(3-acrylamidopropyl)dimethylammonium]propionate (purchased from Shanghai Aladdin Biochemical Technology Co., Ltd., CAS No.: 79704-35-1), and 0.0075 parts of ethylene glycol diallyl ether were dissolved in 15 parts of deionized water to form a uniform solution, which was then added to the above reaction system. Stirring was continued while nitrogen was passed through for 30 minutes. A 1wt% aqueous solution of an oxidizing agent (containing 0.0002 parts of sodium persulfate) was added. After 5 minutes, a 1wt% aqueous solution of a reducing agent (containing 0.00025 parts of sodium bisulfite) was slowly added dropwise until the reaction system finished heating up. The temperature was then maintained at 50°C for 1 hour. The obtained product was the product.

[0119] [Comparative Example 2]

[0120] 20 parts of acrylamide, 5 parts of 2-acrylamido-2-methylpropanesulfonic acid, 4 parts of tert-butyl acrylamide, 0.02 parts of pentaerythritol triallyl ether (purchased from Shanghai Aladdin Biochemical Technology Co., Ltd., CAS No.: 1471-17-6), and 3.5 parts of (carboxymethyl)trimethylammonium chloride were dissolved in 27 parts of water to obtain a reaction solution. The pH value of the solution was adjusted to 7.0 with sodium hydroxide. 0.0075 parts of azobisisobutylamidine hydrochloride was added and stirred evenly to obtain a uniform aqueous phase. 12 parts of anhydrous sorbitan stearate and 1.5 parts of isomeric tridecanol polyoxyethylene ether (8) were added to 50 parts of 5# white oil and stirred evenly to obtain an oil phase. The oil phase and the aqueous phase were added to a reactor respectively, stirred at 700 rpm for 1 hour, and nitrogen was continuously introduced for deoxygenation.

[0121] 0.001 parts of potassium bromate and 0.002 parts of sodium dithionite were prepared into a 1% uniform aqueous solution. After adding the oxidant aqueous solution, stirring was continued for 10 minutes. The reducing agent aqueous solution was slowly added dropwise until the temperature rose to 50°C, until the reaction system finished heating up.

[0122] Dissolve 7 parts of acrylamide and 0.008 parts of pentaerythritol triallyl ether (purchased from Shanghai Aladdin Biochemical Technology Co., Ltd., CAS No.: 1471-17-6) in 12.5 parts of deionized water to form a uniform solution, which is then added to the above reaction system. Continue stirring while purging with nitrogen for 30 minutes. Add a 1wt% aqueous oxidizing agent solution (containing 0.002 parts of potassium bromate). After 5 minutes, slowly add a 1wt% aqueous reducing agent solution (containing 0.0025 parts of sodium dithionite) dropwise until the reaction system has heated up. Incubate at 50°C for 1 hour. The resulting product is the product.

[0123] [Comparative Example 3]

[0124] 25 parts of acrylamide, 7.5 parts of acrylic acid, 5 parts of vinyl pyrrolidone, and 0.015 parts of pentaerythritol triallyl ether were dissolved in 30 parts of water to obtain a reaction solution. The pH of the solution was adjusted to 7.0 with sodium hydroxide. 0.015 parts of azobisisobutylamidine hydrochloride was added and stirred uniformly to obtain a uniform aqueous phase. 12 parts of sorbitan oleate and 2.25 parts of isomeric tridecanol polyoxyethylene ether (5) were added to 58 parts of diesel and stirred uniformly to obtain an oil phase. The oil phase and the aqueous phase were added to a reactor separately and stirred at 700 rpm for 1 hour while continuously introducing nitrogen for deoxygenation.

[0125] Prepare a 1% uniform aqueous solution of 0.00075 parts of ammonium persulfate and 0.001 parts of sodium metabisulfite. Add the oxidizing agent aqueous solution and continue stirring for 10 minutes. Slowly add the reducing agent aqueous solution dropwise until the temperature rises to 50°C. The product is obtained after the reaction system is heated up.

[0126] [Comparative Example 4]

[0127] 22 parts of acrylamide, 5 parts of acrylic acid, 2 parts of vinyl pyrrolidone, 0.015 parts of ethylene glycol diallyl ether, 3 parts of (3-carboxypropyl)trimethylammonium chloride, and 7.5 parts of 3-[(3-acrylamidopropyl)dimethylammonium]propionate (purchased from Shanghai Aladdin Biochemical Technology Co., Ltd., CAS No.: 79704-35-1) were dissolved in 25 parts of water to obtain a reaction solution. The pH value of the solution was adjusted to 7.0 with sodium hydroxide. 0.01 parts of azobisisobutylamidine hydrochloride was added and stirred uniformly to obtain a uniform aqueous phase. 10 parts of anhydrous sorbitan monooleate and 1.75 parts of isomeric tridecanol polyoxyethylene ether (5) were added to 55 parts of 3# white oil and stirred uniformly to obtain an oil phase. The oil phase and the aqueous phase were added to a reactor respectively, stirred at 700 rpm for 1 hour, and nitrogen was continuously introduced for deoxygenation.

[0128] Prepare a 1 wt% uniform aqueous solution of 0.0004 parts of sodium persulfate and 0.0005 parts of sodium bisulfite. Add the oxidizing agent aqueous solution and continue stirring for 10 minutes. Slowly add the reducing agent aqueous solution dropwise until the temperature rises to 50°C or until the reaction system is heated up. The obtained product is the product.

[0129]

Evaluation experiment

[0130] The brine used for the evaluation had a total mineralization of 180,000 mg / L and was highly mineralized (calcium and magnesium ion contents were 2500 ppm each), and the microsphere concentration was 2000 ppm. A uniform solution with an effective microsphere concentration of 2000 ppm was prepared in the brine, and 200 mL of this solution was allowed to flow through a sand-filled pipe with a length of 10 cm, a diameter of 1.2 cm, and a permeability of 1000 mD (K1) under constant pressure conditions of 0.2 MPa. The produced fluid was collected and the flow rate of the produced fluid was recorded. The permeability of the sand-filled pipe at the end of the flow curve was calculated according to Darcy's formula and recorded as K2. The magnitude of the permeability reduction, (K1-K2) / K1*100%, was used as the plugging rate to evaluate the plugging effect of the microspheres. At the same time, the concentration of microspheres in the produced fluid was calculated by measuring the nitrogen content in the produced fluid to evaluate the adsorption capacity of the microspheres to sandstone. The results are shown in Table 1.

[0131] Table 1: Plugging rates of samples from the examples and comparative examples after aging at different temperatures

[0132] Microsphere concentration in produced fluid, ppm Plugging rate, % Example 1 27 98.2 Example 2 19 99.1 Example 3 31 98.7 Example 4 42 98.1 Comparative Example 1 77 92.6 Comparative Example 2 125 88.4 Comparative Example 3 153 84.3 Comparative Example 4 55 93

[0133] It can be clearly seen that the acrylamide microspheres obtained in Examples 1 to 4 of the present invention have a higher plugging rate and a lower microsphere concentration in the produced fluid compared with the acrylamide microspheres obtained in Comparative Examples 1 to 4. This proves that the acrylamide microspheres obtained in the present invention have stronger adsorption and retention during the migration of rock voids, resulting in more effective plugging, thereby effectively changing the heterogeneity of the formation, improving the sweep efficiency of the subsequent injection of displacement fluid, and improving the crude oil recovery rate. This also confirms the principle of synergistic enhancement of the components in the present invention.

[0134] The present invention has been described in detail above with reference to specific embodiments and exemplary examples. However, these descriptions should not be construed as limiting the present invention. Those skilled in the art will appreciate that various equivalent substitutions, modifications, or improvements may be made to the technical solutions and implementations of the present invention without departing from the spirit and scope of the present invention, all of which fall within the scope of the present invention. The scope of protection of the present invention shall be determined by the appended claims.

Claims

1. An acrylamide microsphere comprising a polymer core and a polymer shell, wherein: The polymer shell layer includes an acrylamide structural unit, a structural unit represented by formula (1) and a cross-linking structural unit II: In formula (1), R1 and R1' are independently selected from hydrogen atoms or alkyl groups; R2 is selected from oxygen atoms, -NH or alkyl-substituted nitrogen atoms; R3 and R4 are independently selected from alkylene groups; R5 is selected from anionic organic groups; R6 and R7 are independently selected from alkyl groups.

2. The acrylamide microspheres according to claim 1, characterized in that: In formula (1), R1 and R1' are independently selected from hydrogen atoms or C1-C15 alkyl groups; R2 is selected from oxygen atoms, -NH or alkyl-substituted nitrogen atoms; R3 and R4 are independently selected from C1-C15 alkylene groups; R5 is selected from one of carboxyl groups, sulfate groups, sulfonic acid groups and phosphoric acid groups; R6 and R7 are independently selected from C1-C15 alkyl groups; Preferably, in formula (1), R1 and R1' are independently selected from a hydrogen atom or a C1-C6 alkyl group; R2 is selected from an oxygen atom, -NH or an alkyl-substituted nitrogen atom; R3 and R4 are each independently selected from a C2-C8 alkylene group; R5 is selected from one of a carboxyl group, a sulfate group, a sulfonic acid group, and a phosphoric acid group; R6 and R7 are each independently selected from a C1-C6 alkyl group.

3. The acrylamide microspheres according to claim 1, characterized in that: In the polymer shell layer, by weight: 5 to 10 parts of acrylamide structural unit, 5 to 10 parts of structural unit represented by formula (1), and 0.0005 to 0.2 parts of cross-linking structural unit II; Preferably, in the polymer shell layer, by weight, the following amounts are present: 5 to 7.5 parts of acrylamide structural units, 5 to 7.5 parts of structural units represented by formula (1), and 0.005 to 0.1 parts of cross-linked structural units II.

4. The acrylamide microspheres according to any one of claims 1 to 3, characterized in that: The polymer core comprises an acrylamide structural unit, an anionic structural unit, an optional nonionic structural unit, and a cross-linking structural unit I; Preferably, in the polymer core, by weight: 5 to 30 parts of acrylamide structural units, 1 to 25 parts of anionic structural units, 0 to 10 parts of nonionic structural units, and 0.001 to 0.5 parts of cross-linking structural units I; More preferably, in the polymer core, by weight, the following components are present: 20 to 25 parts of acrylamide structural units, 5 to 10 parts of anionic structural units, 0 to 7.5 parts of nonionic structural units, and 10.01 to 0.25 parts of cross-linking structural units.

5. The acrylamide microspheres according to claim 4, characterized in that: The anion structure is selected from at least one of a carboxylic acid structural unit and / or an alkali metal salt thereof, a sulfonic acid structural unit and / or an alkali metal salt thereof; and / or, The nonionic structural unit is selected from at least one of a substituted acrylamide structural unit, a (substituted) hydroxyalkyl acrylate structural unit, a (substituted) acrylic acid (substituted) amino ester structural unit, and a pyrrolidone structural unit; and / or, The cross-linked structural unit I and the cross-linked structural unit II are each independently derived from a compound containing at least two double bonds, preferably from a compound containing 2 to 5 double bonds.

6. The acrylamide microspheres according to claim 5, characterized in that: The anionic structural unit is derived from at least one of acrylic acid, methacrylic acid, p-vinylbenzenesulfonic acid, maleic acid, fumaric acid, vinylbenzenesulfonic acid, allylsulfonic acid, allylbenzenesulfonic acid, 2-acrylamido-2-methylpropanesulfonic acid, and alkali metal salts thereof; and / or, The nonionic structural unit is derived from at least one of methacrylamide, dimethylacrylamide, diethylacrylamide, hydroxymethylacrylamide, hydroxyethylacrylamide, dimethylaminopropyl methacrylamide, hydroxymethyl methacrylate, hydroxyethyl methacrylate, dimethylaminoethyl methacrylate, vinyl pyrrolidone, and tert-butylacrylamide; and / or, The cross-linked structural unit I and the cross-linked structural unit II are independently derived from at least one of ethylene glycol diallyl ether, glycerol diallyl ether, glycerol triallyl ether, pentaerythritol diallyl ether, pentaerythritol triallyl ether and pentaerythritol tetraallyl ether.

7. The acrylamide microspheres according to any one of claims 1 to 6, characterized in that: The polymer core optionally contains a zwitterionic compound; preferably, the zwitterionic compound is selected from at least one of the compounds represented by formula (2): In formula (2), R8 is selected from C1 to C10 alkylene groups, R9 is selected from anionic organic groups, and R 10 ~R 12 Each independently selected from C1 to C10 alkyl groups; More preferably, in the polymer core, based on 5 to 30 parts of acrylamide structural units, the zwitterionic compound is 0 to 10 parts, preferably 2 to 5 parts.

8. A method for preparing acrylamide microspheres, preferably for preparing the acrylamide microspheres according to any one of claims 1 to 7, the method comprising: (A) preparing a polymer core using raw material I including acrylamide, an anionic monomer, an optional nonionic monomer, a crosslinker I, and an optional zwitterionic compound; (B) preparing a polymer shell using raw materials including acrylamide, a monomer compound corresponding to the structural unit represented by formula (1), and a crosslinker II to obtain the acrylamide microspheres.

9. The preparation method according to claim 8, characterized in that The anionic monomer is selected from at least one of a carboxylic acid polymerizable monomer and / or an alkali metal salt thereof, a sulfonic acid polymerizable monomer and / or an alkali metal salt thereof, preferably, the anionic monomer is selected from at least one of acrylic acid, methacrylic acid, p-vinylbenzenesulfonic acid, maleic acid, fumaric acid, vinylbenzenesulfonic acid, allylsulfonic acid, allylbenzenesulfonic acid, 2-acrylamido-2-methylpropanesulfonic acid, and alkali metal salts thereof; and / or, The nonionic monomer is selected from at least one of substituted acrylamide polymerizable monomers, (substituted) hydroxyalkyl acrylate polymerizable monomers, (substituted) acrylate (substituted) amino ester polymerizable monomers, and pyrrolidone polymerizable monomers. Preferably, the nonionic monomer is selected from at least one of methacrylamide, dimethylacrylamide, diethylacrylamide, hydroxymethylacrylamide, hydroxyethylacrylamide, dimethylaminopropyl methacrylamide, hydroxymethyl methacrylate, hydroxyethyl methacrylate, dimethylaminoethyl methacrylate, vinyl pyrrolidone, and tert-butylacrylamide. and / or, The crosslinking agent I and the crosslinking agent II are each independently selected from compounds containing at least two double bonds, preferably compounds containing 2 to 5 double bonds; preferably, the crosslinking agent I and the crosslinking agent II are each independently selected from at least one of ethylene glycol diallyl ether, glycerol diallyl ether, glycerol triallyl ether, pentaerythritol diallyl ether, pentaerythritol triallyl ether, and pentaerythritol tetraallyl ether.

10. The preparation method according to claim 8, characterized in that In step (A), by weight: 5 to 30 parts of acrylamide, preferably 20 to 25 parts; 1 to 25 parts of anionic monomer, preferably 5 to 10 parts; 0-10 parts of nonionic monomer, preferably 0-7.5 parts; Cross-linking agent I 0.001 to 0.5 parts, preferably 0.01 to 0.25 parts; The amount of the zwitterionic compound is 0 to 10 parts, preferably 2 to 5 parts.

11. The preparation method according to any one of claims 8 to 10, characterized in that: In step (B), by parts by weight: 5 to 10 parts of acrylamide; preferably 5 to 7.5 parts; 5 to 10 parts of the monomer compound corresponding to the structural unit represented by formula (1); preferably 5 to 7.5 parts; Cross-linking agent II 0.0005 to 0.2 parts; preferably 0.005 to 0.1 parts.

12. Use of the acrylamide microspheres according to any one of claims 1 to 7 or the acrylamide microspheres obtained by the preparation method according to any one of claims 8 to 11 in oil and gas field development, especially as profile control agents or plugging agents.