Composite catalyst and method for preparing polyethylene furandicarboxylate by using same
The composite catalyst synthesized by hydrothermal synthesis of MgO and Zn3(C6H5O7)2 solves the biotoxicity problem of PEF catalysts, realizes the preparation of non-toxic, high-viscosity, low-melt-index PEF polyester, and broadens its application in the biological field.
Patent Information
- Application Number
- CN202511167178.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-08-20
- Publication Date
- 2025-10-31
AI Technical Summary
Existing catalysts used in PEF production are biotoxic, which limits their application in fields such as biomedical materials and food packaging bags. Furthermore, catalyst residues are difficult to completely remove, increasing production costs.
A composite catalyst was synthesized using MgO and Zn3(C6H5O7)2 via a hydrothermal process and used to prepare polyethylene furanate dicarboxylate, including esterification, pre-condensation, and final condensation steps, ensuring that the catalyst is non-toxic and easy to remove after the reaction.
A non-toxic, high-viscosity, low melt index, and low blood compatibility PEF polyester was prepared, which improved biocompatibility, simplified the production process for high-value applications, and has the potential for large-scale production.
Smart Images

Figure CN120865257A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of bio-based polyester synthesis technology, and in particular to a composite catalyst and a method for preparing polyethylene furanate using the catalyst. Background Technology
[0002] Polyethylene furanate (PEF), as an emerging bio-based polymer material, possesses superior thermal and mechanical properties and a higher glass transition temperature compared to petroleum-based polyethylene terephthalate (PET), and is considered an ideal alternative to PET. Currently, PEF is mainly synthesized through melt polycondensation, which features high production efficiency, low cost, and suitability for large-scale production, making it the most cost-effective large-scale production process for PEF.
[0003] Currently, catalysts used in PEF production mainly include metal catalysts such as tin, antimony, hafnium, germanium, or zirconium, organic non-metallic catalysts, and enzyme catalysts. However, due to their certain biotoxicity, PEF's application in fields with high biocompatibility requirements, such as biomedical materials and food packaging bags, is limited. High-value-added applications of PEF typically require catalyst removal before use, but the strong interaction between the catalyst and polar ester functional groups makes it difficult to completely remove trace residues, thus significantly increasing PEF production costs. Therefore, finding a catalyst that degrades into non-toxic products after fulfilling its function has become a key research direction for the high-value applications of PEF. Summary of the Invention
[0004] To address the shortcomings of the aforementioned technologies, this invention provides a composite catalyst and a method for preparing polyethylene furanate using the catalyst, which effectively solves the problem of catalyst residue affecting biocompatibility.
[0005] This invention discloses a composite catalyst synthesized from MgO and Zn3(C6H5O7)2 via a hydrothermal process, wherein the mass ratio of MgO to Zn3(C6H5O7)2 is 1:1-2.
[0006] Its preparation method is as follows:
[0007] First, add Zn3(C6H5O7)2 to deionized water according to the mass ratio, stir to dissolve, then add MgO and perform ultrasonic dispersion. The ultrasonic dispersion is performed at 100-200W for 20-40 minutes.
[0008] Then it is transferred to a high-temperature reactor and placed in an oven for hydrothermal processing, where the hydrothermal temperature is 100-200℃ and the time is 10-18h.
[0009] Finally, after the reaction is complete, the reaction products are collected, washed with anhydrous ethanol, and dried at a temperature of 40-100℃ to obtain the composite catalyst.
[0010] A method for preparing polyethylene furanate using the above-mentioned composite catalyst includes the following steps:
[0011] First, add EG, FDCA and composite catalyst to the reaction flask, wherein the molar ratio of EG to FDCA is 1.01-1.8:1 and the mass ratio of composite catalyst to FDCA is 0.01-2:100.
[0012] During the esterification reaction stage, the system is stirred at normal pressure under inert gas protection, and the temperature of the reaction system is raised to 180-220℃. The esterification reaction time is 2-6 hours.
[0013] During the pre-condensation reaction stage, the vacuum level of the reaction system is reduced from atmospheric pressure to 1000 Pa, the temperature is raised to 190-230℃, and the pre-condensation reaction time is greater than or equal to 1 hour.
[0014] In the final polycondensation stage, the temperature of the reaction system rises to 240-260℃, the pressure drops to less than 50Pa, and the final polycondensation reaction time is greater than or equal to 1 hour.
[0015] The final polycondensation reaction yields polyethylene furanate.
[0016] After the final polycondensation reaction is completed, N2 is introduced into the reaction system, and the temperature of the flask and the casting head is set to 200-240℃. The reactant melt is granulated by water cooling and pelletizing, and then dried to obtain PEF polyester.
[0017] The combined time for the pre-condensation reaction and the final condensation reaction is 2-6 hours.
[0018] The reaction flask is a three-necked round-bottom flask equipped with a polytetrafluoroethylene (PTFE) stirrer.
[0019] Before the esterification reaction, the air inside the reaction flask is evacuated by inert gas replacement and the interface is sealed with vacuum silicone ester to ensure the airtightness of the reaction.
[0020] The present invention provides a composite catalyst and a method for preparing polyethylene furanate (PEF) using this catalyst. Under the action of the composite catalyst, PEF polyester with high viscosity (0.8–1.5 g / dL), low melt index (3–10 g / 10 min), and low blood compatibility (less than 5%), without the need for removal and with no potential toxicity, can be rapidly produced in a short time, exhibiting excellent overall performance. This method can improve the biocompatibility of PEF products, simplify the production process for high-value applications of PEF, and has the potential for large-scale production. Attached Figure Description
[0021] Figure 1 This is a schematic diagram of the structure of the composite catalyst of the present invention;
[0022] Figure 2 This invention describes the reaction mechanism of the composite catalyst 0.2NC catalyzing the polycondensation of EG and FDCA to form PEF.
[0023] Figure 3 This is a transmission electron microscope image of the composite catalyst 0.2NC in this invention. Detailed Implementation
[0024] To further illustrate the technical means and effects of the present invention in achieving its intended purpose, the following detailed description of the specific implementation methods, structures, features, and effects of the present invention, in conjunction with the accompanying drawings and preferred embodiments, is provided below.
[0025] The intrinsic viscosity and melt flow index in the following examples were determined according to the following method:
[0026] Intrinsic viscosity: 0.2g of PEF polyester was dissolved in 20ml of a phenol-1,1,2,2-tetrachloroethane mixture (mass ratio 1:1). The intrinsic viscosity was measured using a single-point method in a 25℃ water bath. The formula for calculating intrinsic viscosity is:
[0027]
[0028] Where: η r Relative viscosity, η sp : Specific viscosity, t0: Solvent outflow time, t1: Polymer solution outflow time, c: Polymer solution concentration.
[0029] Melt flow index: Characterized by the melt flow index tester (FR-1811A) based on national standards GB / T 3682.1 and 3682.2.
[0030] Blood compatibility: Tested based on national standard GB / T 16886.4, and expressed as hemolysis rate.
[0031] Example 1:
[0032] This invention discloses a method for preparing a composite catalyst:
[0033] First, 0.1M (1.436g) Zn3(C6H5O7)2 was dissolved in 25mL of deionized water. After stirring and dissolving, 40mg MgO was added and ultrasonically dispersed at 120W for 30min. Then, it was transferred to a high-temperature reactor and placed in a hydrothermal reactor at 160℃ for 12h. Finally, after the reaction was completed, the reactants were collected, washed with anhydrous ethanol, and dried at 60℃. The resulting sample was recorded as 0.1NC.
[0034] Example 2:
[0035] This invention discloses a method for preparing a composite catalyst:
[0036] First, 0.2M (2.872g) Zn3(C6H5O7)2 was dissolved in 25mL of deionized water. After stirring and dissolving, 80mg MgO was added and ultrasonically dispersed at 150W for 20min. Then, the mixture was transferred to a high-temperature reactor and placed in an oven for hydrothermal reaction at 180℃ for 14h. Finally, after the reaction was completed, the reactants were collected, washed with anhydrous ethanol, and dried at 100℃. The resulting sample was recorded as 0.2NC.
[0037] like Figure 3 As shown, it is a transmission electron microscope image of sample 0.2NC.
[0038] Example 3:
[0039] This invention discloses a method for preparing a composite catalyst:
[0040] First, 0.4M (5.744g) Zn3(C6H5O7)2 was dissolved in 25mL of deionized water. After stirring and dissolving, 120mg MgO was added and ultrasonically dispersed at 120W for 30min. Then, the mixture was transferred to a high-temperature reactor and placed in an oven for hydrothermal reaction at 180℃ for 12h. Finally, after the reaction was completed, the reactants were collected, washed with anhydrous ethanol, and dried at 60℃. The resulting sample was recorded as 0.4NC.
[0041] Example 4:
[0042] This invention discloses a method for preparing a composite catalyst:
[0043] First, 0.05M (0.718g) Zn3(C6H5O7)2 was dissolved in 25mL of deionized water. After stirring and dissolving, 10mg MgO was added and ultrasonically dispersed at 120W for 30min. Then, the mixture was transferred to a high-temperature reactor and placed in an oven for hydrothermal reaction at 180℃ for 16h. Finally, after the reaction was completed, the reactants were collected, washed with anhydrous ethanol, and dried at 80℃. The resulting sample was recorded as 0.05NC.
[0044] Example 5:
[0045] This invention discloses a method for preparing a composite catalyst:
[0046] First, 0.25M (3.59g) Zn3(C6H5O7)2 was dissolved in 25mL of deionized water. After stirring and dissolving, 40mg MgO was added and ultrasonically dispersed at 180W for 20min. Then, the mixture was transferred to a high-temperature reactor and placed in an oven for hydrothermal reaction at 200℃ for 12h. Finally, after the reaction was completed, the reactants were collected, washed with anhydrous ethanol, and dried at 40℃. The resulting sample was recorded as 0.25NC.
[0047] The structural schematic diagrams of the composite catalysts obtained in Examples 1-5 above may be as follows: Figure 1 As shown.
[0048] Example 6:
[0049] This invention discloses a method for preparing polyethylene furanate (PEF-1):
[0050] All PEF synthesis operations were carried out in a three-necked round-bottom flask equipped with a polytetrafluoroethylene (PTFE) stirrer under continuous mechanical stirring. First, 1.8 mol EG, 1.0 mol FDCA, and 0.156 g of 0.2 NC were added to a 100 mL three-necked round-bottom flask. To ensure the reaction was airtight, a vacuum silicone sealant was used to seal the interface, and the flask was placed in an oil bath for heating. Next, after stirring at 110 °C for 0.5 h, the temperature was increased to 180 °C and reacted for 3 h. Subsequently, the vacuum was reduced from atmospheric pressure to 1000 Pa, and the temperature was maintained at 210 °C for 1 h. Finally, the temperature was maintained at 240 °C, the vacuum was reduced to below 50 Pa, and the reaction was continued for 3 h. Finally, N2 was introduced into the system to increase the internal pressure to 0.2 MPa, and the temperature of the flask and casting head was set to 240 °C. The polymer melt was then water-cooled, granulated using a pelletizer, dried, and sealed for storage, designated as PEF-1. Among them, the intrinsic viscosity of PEF-1 in the molten state extruded by inert gas is 1.22 dL / g, the melt index at 240℃ is 5.81 g / 10 min, and the blood compatibility is 0.37%.
[0051] Example 7:
[0052] This invention discloses a method for preparing polyethylene furanate (PEF-2):
[0053] All PEF synthesis operations were carried out in a three-necked round-bottom flask equipped with a polytetrafluoroethylene (PTFE) stirrer under continuous mechanical stirring. First, 1.105 mol EG, 1 mol FDCA, and 0.312 g of 0.2 NC were added to a 100 mL three-necked round-bottom flask. To ensure the reaction was airtight, a vacuum silicone sealant was used to seal the interface, and the flask was placed in an oil bath for heating. Next, after stirring at 110 °C for 0.5 h, the temperature was increased to 200 °C and reacted for 4 h. Subsequently, the vacuum was reduced from atmospheric pressure to 1000 Pa, and the temperature was maintained at 200 °C for 2 h. Finally, the temperature was maintained at 230 °C, the vacuum was reduced to below 50 Pa, and the reaction was continued for 3 h. Finally, N2 was introduced into the system to increase the internal pressure to 0.2 MPa, and the temperature of the flask and casting head was set to 240 °C. The polymer melt was then water-cooled and granulated using a pelletizer, dried, and sealed for storage, designated as PEF-2. Among them, the intrinsic viscosity of PEF-2 in the molten state extruded by inert gas is 1.20 dL / g, the melt index at 240℃ is 6.72 g / 10 min, and the blood compatibility is 0.34%.
[0054] Example 8:
[0055] This invention discloses a method for preparing polyethylene furanate (PEF-3):
[0056] All PEF synthesis operations were carried out in a three-necked round-bottom flask equipped with a polytetrafluoroethylene (PTFE) stirrer under continuous mechanical stirring. First, 1.5 mol EG, 1 mol FDCA, and 1.248 g of 0.2 NC were added to a 100 mL three-necked round-bottom flask. To ensure the reaction was airtight, a vacuum silicone sealant was used to seal the interface, and the flask was placed in an oil bath for heating. Next, after stirring at 110 °C for 0.5 h, the temperature was increased to 200 °C and reacted for 4 h. Subsequently, the vacuum was reduced from atmospheric pressure to 1000 Pa, and the temperature was maintained at 210 °C for 1 h. Finally, the temperature was maintained at 230 °C, the vacuum was reduced to below 50 Pa, and the reaction was continued for 5 h. Finally, N2 was introduced into the system to increase the internal pressure to 0.2 MPa, and the temperature of the flask and casting head was set to 240 °C. The polymer melt was then water-cooled, granulated using a pelletizer, dried, and sealed for storage, designated PEF-3. Among them, the intrinsic viscosity of PEF-3 in the molten state extruded by inert gas is 1.34 dL / g, the melt index at 240℃ is 3.74 g / 10 min, and the blood compatibility is 0.28%.
[0057] Example 9:
[0058] This invention discloses a method for preparing polyethylene furanate (PEF-4):
[0059] All PEF synthesis operations were carried out in a three-necked round-bottom flask equipped with a polytetrafluoroethylene (PTFE) stirrer under continuous mechanical stirring. First, 1.5 mol EG, 1.2 mol FDCA, and 3.12 g of 0.2 NC were added to a 100 mL three-necked round-bottom flask. To ensure the reaction was airtight, a vacuum silicone sealant was used to seal the interface, and the flask was placed in an oil bath for heating. Next, after stirring at 110 °C for 0.5 h, the temperature was increased to 210 °C and reacted for 3 h. Subsequently, the vacuum was reduced from atmospheric pressure to 1000 Pa, and the temperature was maintained at 230 °C for 1 h. Finally, the temperature was maintained at 210 °C, the vacuum was reduced to below 50 Pa, and the reaction was continued for 4 h. Finally, N2 was introduced into the system to increase the internal pressure to 0.2 MPa, and the temperature of the flask and casting head was set to 240 °C. The polymer melt was then water-cooled, granulated using a pelletizer, dried, and sealed for storage, designated PEF-4. Among them, the intrinsic viscosity of PEF-4 in the molten state extruded by inert gas is 1.26 dL / g, the melt index at 240℃ is 5.47 g / 10 min, and the blood compatibility is 0.19%.
[0060] Example 10:
[0061] This invention discloses a method for preparing polyethylene furanate (PEF-5):
[0062] All PEF synthesis operations were carried out in a three-necked round-bottom flask equipped with a polytetrafluoroethylene (PTFE) stirrer under continuous mechanical stirring. First, 1.5 mol EG, 1.4 mol FDCA, and 1.56 g of 0.2 NC were added to a 100 mL three-necked round-bottom flask. To ensure the reaction was airtight, a vacuum silicone sealant was used to seal the interface, and the flask was placed in an oil bath for heating. Next, after stirring at 110 °C for 0.5 h, the temperature was increased to 160 °C and reacted for 6 h. Subsequently, the vacuum was reduced from atmospheric pressure to 1000 Pa, and the temperature was maintained at 200 °C for 2.5 h. Finally, the temperature was maintained at 220 °C, the vacuum was reduced to below 50 Pa, and the reaction was continued for 4 h. Finally, N2 was introduced into the system to increase the internal pressure to 0.2 MPa, and the temperature of the flask and casting head was set to 230 °C. The polymer melt was then water-cooled, granulated using a pelletizer, dried, and sealed for storage, designated PEF-5. Among them, the intrinsic viscosity of PEF-5 in the molten state extruded by inert gas is 1.49 dL / g, the melt index at 240℃ is 1.43 g / 10 min, and the blood compatibility is 0.22%.
[0063] In Examples 6-10, the air inside the reactor was evacuated by inert gas replacement before the transesterification, and the interface was sealed with vacuum silicone ester to ensure the airtightness of the reaction.
[0064] In Examples 6-10 above, the specific reaction mechanism of 0.2NC catalyzing the polycondensation of EG and FDCA to form PEF is as follows: Figure 2 As shown.
[0065] Comparative Example 1:
[0066] The preparation of PEF using MgO as a catalyst is as follows:
[0067] PEF was prepared using the same method as in Example 8, with MgO as the reaction catalyst. The intrinsic viscosity was 0.94 dL / g, the melt index at 240°C was 9.1 g / 10 min, and the blood compatibility was 0.43%.
[0068] Comparative Example 2:
[0069] PEF was prepared using Zn3(C6H5O7)2 as a catalyst, as detailed below:
[0070] PEF was prepared using the same method as in Example 8, with Zn3(C6H5O7)2 as the reaction catalyst. The intrinsic viscosity was 1.37 dL / g, the melt index at 240°C was 3.11 g / 10 min, and the blood compatibility was 3.9%.
[0071] Comparative Example 3:
[0072] PEF was prepared using stannous octoate as a catalyst, as detailed below:
[0073] PEF was prepared using the same method as in Example 8, with stannous octoate as the reaction catalyst. The intrinsic viscosity was 1.41 dL / g, the melt index at 240°C was 1.13 g / 10 min, and the blood compatibility was 12.44%.
[0074] Comparative Example 4:
[0075] PEF was prepared using tetrabutyl titanate as a catalyst, as detailed below:
[0076] PEF was prepared using the same method as in Example 8, with tetrabutyl titanate as the reaction catalyst. The intrinsic viscosity was 1.44 dL / g, the melt index at 240°C was 0.99 g / 10 min, and the blood compatibility was 14.47%.
[0077] Table 1. Experimental results of PEF preparation:
[0078]
[0079]
[0080] Based on the experimental results and comparing the examples and comparative examples, the composite catalyst, based on the chelation of carboxyl groups and metallic Mg, the bridging coordination with Zn, and its non-toxic properties, not only improves the spinnability of PEF but is also non-toxic. The composite catalyst described in this invention can significantly reduce catalyst toxicity while maintaining product viscosity, thus broadening the application of PEF in the biological field.
[0081] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention in any way. Although the present invention has been disclosed above with reference to preferred embodiments, it is not intended to limit the present invention. Any person skilled in the art can make some modifications or alterations to the above-disclosed technical content to create equivalent embodiments without departing from the scope of the present invention. Any simplification, equivalent changes, and alterations made to the above embodiments based on the technical essence of the present invention without departing from the scope of the present invention shall still fall within the scope of the present invention.
Claims
1. A composite catalyst, characterized in that: it is composed of... MgO and Zn3(C6H5O7)2 are synthesized by a hydrothermal process, wherein the mass ratio of MgO to Zn3(C6H5O7)2 is 1:1-2.
2. The composite catalyst according to claim 1, characterized in that: Its preparation method is as follows: First, add Zn3(C6H5O7)2 to deionized water according to the mass ratio, stir to dissolve, then add MgO and perform ultrasonic dispersion. The ultrasonic dispersion is performed at 100-200W for 20-40 minutes. Then it is transferred to a high-temperature reactor and placed in an oven for hydrothermal processing, where the hydrothermal temperature is 100-200℃ and the time is 10-18h. Finally, after the reaction is complete, the reaction products are collected, washed with anhydrous ethanol, and dried at a temperature of 40-100℃ to obtain the composite catalyst.
3. A method for preparing polyethylene furanate using the composite catalyst as described in claim 1, characterized in that: Includes the following steps: First, add EG, FDCA and composite catalyst to the reaction flask, wherein the molar ratio of EG to FDCA is 1.01-1.8:1 and the mass ratio of composite catalyst to FDCA is 0.01-2:
100. During the esterification reaction stage, the system is stirred at normal pressure under inert gas protection, and the temperature of the reaction system is raised to 180-220℃. The esterification reaction time is 2-6 hours. During the pre-condensation reaction stage, the vacuum level of the reaction system is reduced from atmospheric pressure to 1000 Pa, the temperature is raised to 190-230℃, and the pre-condensation reaction time is greater than or equal to 1 hour. In the final polycondensation stage, the temperature of the reaction system rises to 240-260℃, the pressure drops to less than 50Pa, and the final polycondensation reaction time is greater than or equal to 1 hour. The final polycondensation reaction yields polyethylene furanate.
4. The method for preparing polyethylene furanate according to claim 3, characterized in that: After the final polycondensation reaction is completed, N2 is introduced into the reaction system, and the temperature of the reaction flask and the casting head is set to 200-240℃. The reactant melt is granulated by water cooling and pelletizing, and then dried to obtain PEF polyester.
5. The method for preparing polyethylene furanate according to claim 3, characterized in that: The reaction flask is a three-necked round-bottom flask equipped with a polytetrafluoroethylene (PTFE) stirrer.